Zirconium-based porous metal organic framework catalyst, preparation method and application
Through the hydrothermal synthesis and application of zirconium-based porous metal organic framework catalyst, the problem of reduced catalytic activity of acrylic condensation catalysts in the reaction is solved, and the efficient and selective amide preparation is achieved, which complies with green chemical specifications.
Patent Information
- Application Number
- CN202411158384.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-22
AI Technical Summary
The existing acine condensation catalysts have reduced catalytic activity due to the formation of water during the reaction, and cannot be reused. The homogeneous catalysts are priced, have low atomic utilization, and produce toxic and harmful by-products, which do not comply with green chemical specifications.
The zirconium-based porous metal organic framework catalyst is prepared by hydrothermal synthesis method, and is used to prepare amide reactions for acyl acid condensation, and a highly efficient and gentle benzoic acid and benzylamine condensation catalytic system is constructed to solve the problem of reuse of catalysts and reduced water decomposition activity.
It realizes efficient and selective amide preparation, the catalyst can be reused, the reaction conditions are mild, and it complies with green chemical specifications, which improves the conversion efficiency and product selectivity of the amide process.
Smart Images

Figure CN118994619A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of chemical industry for preparing high-value chemicals by efficient catalytic conversion of biomass platform compounds, and in particular to a zirconium-based porous metal organic skeleton catalyst, a preparation method and application thereof in a process for preparing amides by condensation of amino acids. Background Art
[0002] Amide is a very important biomass platform compound, which is widely used in the fields of medicine, pesticide, materials and food additives. According to the in-depth analysis of the Comprehensive Medicinal Chemistry Database, more than 25% of known drugs contain amide structural units. Many common drugs such as loperamide acetaminophen (analgesic), lidocaine (Xylocaine, local anesthetic), atorvastatin (cholesterol lowering) contain amide structures. In addition, amides are also widely present in the structure of potential drug compounds. Amide compounds are also widely used in papermaking, plastics, rubber and agriculture, and serve as important intermediates in the synthesis of therapeutic agents.
[0003] At present, there are two types of amine acid condensation catalysts: homogeneous and heterogeneous. Most heterogeneous catalysts are composed of commercially available inorganic oxides such as Nb2O5, Al2O3, ZrO2, SiO2, TiO2, etc. Although they are easy to separate and recycle, the generation of water during the reaction will reduce the catalytic activity and cannot be effectively used multiple times. Homogeneous catalysts are generally complex organic substances. Although they have high reaction efficiency, they are expensive, have low atomic utilization, and produce more toxic and harmful by-products, which do not meet the green chemistry standards. Summary of the invention
[0004] The purpose of the present invention is to address the problems existing in the background technology, propose a zirconium-based porous metal organic framework catalyst, a preparation method and its application in the process of preparing amides by condensation of amine acids, construct an efficient and mild catalytic system for the condensation reaction of benzoic acid and benzylamine to prepare amides, and effectively solve the problems that heterogeneous catalysts cannot be reused and free water deactivates the catalyst.
[0005] To achieve the above object, the present invention adopts the following technical solution:
[0006] In a first aspect, the present invention provides a method for preparing a zirconium-based porous metal organic framework catalyst, comprising:
[0007] Mixing Zr salt and 1,3,5-benzenetricarboxylic acid in a solvent and stirring at room temperature to form a uniform colloid; the molar ratio of Zr salt to 1,3,5-benzenetricarboxylic acid is 1:1;
[0008] The uniform colloid is subjected to a hydrothermal reaction to obtain a white granular solid;
[0009] The white granular solid is freeze-dried, ground and sieved to obtain a zirconium-based porous metal organic framework catalyst.
[0010] Furthermore, the Zr salt is any one of zirconium chloride and zirconium oxide chloride.
[0011] Furthermore, the solvent is a mixed solution of N,N-dimethylformamide and formic acid solution in a molar ratio of 1:1.
[0012] In a second aspect, the present invention provides a zirconium-based porous metal-organic framework catalyst prepared by the preparation method of the zirconium-based porous metal-organic framework catalyst described in any one of the first aspects.
[0013] In a third aspect, the present invention provides the use of the aforementioned zirconium-based porous metal organic framework catalyst in the process of preparing amides by condensation of amine acids.
[0014] Furthermore, the use of the zirconium-based porous metal organic framework catalyst in the process of preparing amides by amine acid condensation includes: placing the zirconium-based porous metal organic framework catalyst, benzoic acid, benzylamine and a reaction solvent in a reaction container, and conducting an amine acid condensation reaction under nitrogen protection conditions to obtain N-benzylbenzamide.
[0015] Furthermore, the reaction temperature of the amine acid condensation reaction is 40-120° C., and the reaction time is 2-24 h.
[0016] Preferably, the reaction temperature of the amine acid condensation reaction is 70-90° C., and the reaction time is 8-12 h.
[0017] Furthermore, the reaction solvent of the amine acid condensation reaction is any one of tetrahydrofuran, 1,4-dioxane and toluene, or a mixture of two or more of tetrahydrofuran, ethyl acetate, 1,4-dioxane, ethanol, N,N-dimethylformamide and toluene.
[0018] Preferably, the reaction solvent for the amine acid condensation reaction is any one of tetrahydrofuran and toluene.
[0019] Reaction mechanism: MOF808 interacts with the carbonyl group of carboxylic acid to form an intermediate, followed by an equal amount of amine nucleophilic addition to the intermediate. After that, excess free amine continues to add to the intermediate to form a cyclic compound. Finally, the unstable cyclic compound removes water molecules to form the target product amide.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] (1) The present invention prepares the MOF808 catalyst by a simple hydrothermal synthesis method, the preparation process is simple, and the synthetic process route is short; by regulating the active components of the catalyst, the process conditions for preparing amides by condensation of amine acids with benzoic acid and benzylamine are optimized, and a reaction catalytic system for preparing amides by condensation of amine acids is constructed, which effectively solves the problem that the catalyst cannot be reused in the process of preparing amides;
[0022] (2) The catalyst of the present invention can efficiently and selectively condense benzoic acid and benzylamine to prepare N-benzylbenzamide under the conditions of a reaction temperature of 90°C and a reaction solvent of tetrahydrofuran (THF), and has the advantages of high conversion efficiency, good product selectivity, mild reaction conditions, and easy recycling. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The chemical reaction formula for preparing amide by the amino acid condensation of benzoic acid and benzylamine in the present invention. DETAILED DESCRIPTION
[0024] The present invention will be further described below in conjunction with specific examples. The following examples are only used to more clearly illustrate the technical solutions of the present invention, and are not intended to limit the scope of protection of the present invention.
[0025] It should be noted that, unless otherwise specified, the technical terms or scientific terms used in this application should have the common meanings understood by those skilled in the art to which the present invention belongs.
[0026] Unless otherwise specified, the raw materials in the examples of the present invention were purchased from commercial sources.
[0027] Example 1
[0028] A method for preparing a zirconium-based porous metal organic framework catalyst comprises the following steps:
[0029] S1. Mix 4 mmol of zirconium chloride, 4 mmol of 1,3,5-benzenetricarboxylic acid, 16 mL of N,N-dimethylformamide solution, and 16 mL of formic acid solution in a solvent, and then stir at room temperature of 20-30°C for 1-2 hours to form a uniform colloid;
[0030] S2, placing the uniform colloid obtained in S1 in a polytetrafluoroethylene-lined hydrothermal synthesis reactor, and heating at a constant temperature of 120° C. for 48 h. After the reaction is completed, the hydrothermal reactor is cooled to room temperature, and the white granular solid is collected by filtration and washed with N,N-dimethylformamide solution for multiple times to remove unreacted ligand molecules;
[0031] S3. Freeze-dry, grind and sieve the white granular solid obtained in S2 to obtain the zirconium-based porous metal organic framework catalyst MOF808.
[0032] Example 2
[0033] The catalyst MOF808 prepared in Example 1 was applied to the amine acid condensation reaction of benzoic acid and benzylamine, comprising the following steps: 10 mg of catalyst, 1 mmol of benzoic acid, 2 mmol of benzylamine, 0.5 g of 4A molecular sieve and 2.5 mL of reaction solvent tetrahydrofuran (THF) were placed in a 15 mL reaction tube and sealed, a double-row tube was used to evacuate and nitrogen gas of a certain pressure was introduced, the reaction temperature was set to 90°C and maintained at 90°C for 48 hours, the stirring rate was 300 rpm, and after the set reaction time was over, the reaction tube was naturally cooled and the mixture of the reaction liquid and the catalyst was poured out. The catalyst in the above reaction liquid was fixed by filtering through a funnel, and the clarified reaction liquid was poured out to obtain the reacted catalyst.
[0034] Comparative Example 1-2
[0035] The commercially available ZrO2 and ZrCl4 catalysts are respectively applied to the amine acid condensation reaction of benzoic acid and benzylamine, comprising the following steps: 10 mg of catalyst, 1 mmol of benzoic acid, 2 mmol of benzylamine, 0.5 g of 4A molecular sieve and 2.5 mL of reaction solvent THF are placed in a 15 mL reaction tube and sealed, a double-row tube is used to evacuate and introduce nitrogen gas of a certain pressure, the reaction temperature is set to 90°C and maintained at 90°C for 48 hours, the stirring rate is 300 rpm, after the set reaction time is over, the reaction tube is naturally cooled, and the mixture of the reaction liquid and the catalyst is poured out. The catalyst in the above reaction liquid is fixed by filtering through a funnel, and the clarified reaction liquid is poured out to obtain the reacted catalyst.
[0036] The reaction products in the reaction solutions of Example 2, Comparative Examples 1 and 2 were qualitatively and quantitatively analyzed by GC and column chromatography to obtain the yield of the target product amide. The results are shown in Table 1:
[0037] Table 1 Selectivity comparison table of amide products corresponding to amine acid condensation
[0038] Case catalyst Reaction conditions Amide yield (%) Comparative Example 1 <![CDATA[ZrO2]]> 90℃, 48h 27.2 Comparative Example 2 <![CDATA[ZrCl4]]> 90℃, 48h 82 Example 2 MOF808 90℃, 48h 67.9
[0039] The purpose of Example 2, Comparative Examples 1 and 2 is to explore the effects of Zr-based catalysts and the MOF808 catalyst prepared by the present invention on the amine acid condensation reaction performance of benzoic acid and benzylamine. It can be found from Table 1 that different catalysts have a greater influence on the amine acid condensation reaction performance. ZrO2, ZrCl4, and MOF808 catalysts are all reactive, among which ZrCl4 has the best effect, but ZrCl4 is easily deliquescent when exposed to water and cannot be reused, and ZrO2 has the worst effect. Although the MOF808 catalyst of the present invention has a lower reaction activity than ZrCl4, it can be reused many times, and its reaction activity is only slightly lower than that of ZrCl4.
[0040] Embodiment 3-10
[0041] The catalyst prepared in Example 1 is respectively applied to the amine acid condensation reaction of benzoic acid and benzylamine, comprising the following steps: 10 mg of catalyst, 1 mmol of benzoic acid, 2 mmol of benzylamine, 0.5 g of 4A molecular sieve and 2.5 mL of different reaction solvents are placed in a 15 mL reaction tube and sealed, a double-row tube is used to evacuate and a certain pressure of nitrogen is introduced, the reaction temperature is set to 90 ° C and maintained at 90 ° C for 8 hours, the stirring rate is 300 rpm, and after the set reaction time is over, the reaction tube is naturally cooled and the mixture of the reaction solution and the catalyst is poured out. The catalyst in the above reaction solution is fixed by funnel filtration, and the clarified reaction solution is poured out to obtain the reacted catalyst.
[0042] The reaction products in the reaction solution of Example 3-10 were qualitatively and quantitatively analyzed by GC and column chromatography to obtain the yield of the target product amide. The results are shown in Table 2:
[0043] Table 2 Selectivity comparison table of amide products corresponding to amine acid condensation
[0044] Example Solvents Reaction conditions Amide yield (%) 3 Tetrahydrofuran 90℃, 8h 57.0 4 Toluene 90℃, 8h 53.4 5 N,N-Dimethylformamide 90℃, 8h 26.1 6 Tetrahydrofuran:water (1:1) 90℃, 8h 24.3 7 Tetrahydrofuran:ethanol (1:1) 90℃, 8h 43.6 8 Ethyl acetate 90℃, 8h 16.4 9 Ethanol 90℃, 8h 3.4 10 1,4-Dioxane 90℃, 8h 33.7
[0045] The purpose of Examples 3-10 is to study the effect of different solvents on the performance of the MOF808 catalyst in catalyzing the amine acid condensation reaction of benzoic acid and benzylamine. As can be seen from Table 2, the solvent has a great influence on the performance of the MOF808 catalyst in catalyzing the amine acid condensation reaction of benzoic acid and benzylamine. In single solvents such as tetrahydrofuran, toluene, N,N-dimethylformamide, ethanol, and mixed solvents such as tetrahydrofuran: water (1:1), tetrahydrofuran: ethanol (1:1), the yield of the target product N-benzylbenzamide is quite different. Among them, tetrahydrofuran is used as a solvent, and under milder reaction conditions (90°C, 8h), the corresponding target product amide yield reaches 57.0%, indicating that this non-protonic non-polar solvent promotes the amine acid condensation reaction. However, when water is introduced into tetrahydrofuran, the yield of the target product amide drops to 24.3%, indicating that the introduction of water is not conducive to the amine acid condensation reaction. When ethanol is used as the reaction solvent, the yield of the target product amide is low, only 3.4%, but when it is mixed with tetrahydrofuran as the solvent, the amide yield can reach 43.6%.
[0046] Examples 11-16
[0047] The catalyst prepared in Example 1 is respectively applied to the amine acid condensation reaction of benzoic acid and benzylamine, comprising the following steps: 10 mg of catalyst, 1 mmol of benzoic acid, 2 mmol of benzylamine, 0.5 g of 4A molecular sieve and 2.5 mL of tetrahydrofuran solvent are placed in a 15 mL reaction tube and sealed, a double-row tube is used to evacuate and nitrogen of a certain pressure is introduced, different reaction temperatures are set and different reaction times are maintained at the temperature, the stirring rate is 300 rpm, after the set reaction time ends, the reaction tube is naturally cooled, and the mixture of the reaction solution and the catalyst is poured out. The catalyst in the above reaction solution is fixed by funnel filtration, and the clarified reaction solution is poured out to obtain the reacted catalyst.
[0048] The reaction products in the reaction solutions of Examples 11-16 were qualitatively and quantitatively analyzed by GC and column chromatography to obtain the yield of the target product amide. The results are shown in Table 3:
[0049] Table 3 Selectivity comparison table of amide products corresponding to amine acid condensation
[0050] Example Solvents Reaction conditions Amide yield (%) 11 Tetrahydrofuran 50℃, 12h 35.1 12 Tetrahydrofuran 70℃, 12h 52.3 13 Tetrahydrofuran 90℃, 12h 64.0 14 Tetrahydrofuran 110℃, 12h 67.2 15 Tetrahydrofuran 90℃, 4h 10.9 16 Tetrahydrofuran 90℃, 8h 57.0
[0051] The purpose of Examples 11-16 is to study the effects of reaction conditions such as temperature and reaction time on the performance of the MOF808 catalyst in catalyzing the amine acid condensation reaction of benzoic acid and benzylamine. As can be seen from Table 3, the reaction conditions have a great influence on the performance of the MOF808 catalyst in catalyzing the amine acid condensation reaction of benzoic acid and benzylamine. Under milder reaction conditions (90°C, 12h), the yield of the corresponding target product amide reaches 67.2%. Compared with the high temperature environment of 110°C in Example 14, Example 13 is more energy-saving and environmentally friendly, and meets the green chemistry specifications.
[0052] Examples 17-21
[0053] The catalyst prepared in Example 1 is respectively applied to the amine acid condensation reaction of benzoic acid and benzylamine, comprising the following steps: 10 mg of catalyst, 1 mmol of benzoic acid, 2 mmol of benzylamine, 0.5 g of 4A molecular sieve and 2.5 mL of tetrahydrofuran solvent are placed in a 15 mL reaction tube and sealed, a double-row tube is used to evacuate and a certain pressure of nitrogen is introduced, the reaction temperature is set to 90 ° C and maintained at 90 ° C for 12 hours, the stirring rate is 300 rpm, and after the reaction time is set, the reaction tube is naturally cooled and the mixture of the reaction solution and the catalyst is poured out. The catalyst in the above reaction solution is fixed by funnel filtration, and the clarified reaction solution is poured out to obtain the reacted catalyst. The catalyst is repeatedly used for multiple times, and subsequent examples 18-21 are implemented.
[0054] The reaction products in the reaction solutions of Examples 17-21 were qualitatively and quantitatively analyzed by GC and column chromatography to obtain the yield of the target product amide. The results are shown in Table 4:
[0055] Table 4 Selectivity comparison table of acid condensation corresponding to amide products
[0056] Example Catalyst reaction time Reaction conditions Amide yield (%) 17 12h 90℃, 12h 64.0 18 24h 90℃, 12h 62.1 19 48h 90℃, 12h 59.8 20 60h 90℃, 12h 54.2 21 72h 90℃, 12h 50.6
[0057] The purpose of Examples 17-21 is to study the reusability of the amine acid condensation reaction of benzoic acid and benzylamine catalyzed by MOF808 catalyst. As can be seen from Table 4, with the long-term use of MOF808 catalyst, the yield of the corresponding target product amide gradually decreases, but the overall yield is still higher than 50%. MOF808 catalyst can be used at least five times, and the recycling effect is good.
[0058] The present invention has been disclosed above with preferred embodiments, but they are not intended to limit the present invention. Any technical solutions obtained by adopting equivalent replacement or equivalent transformation solutions fall within the protection scope of the present invention.
Claims
1. A method for preparing a zirconium-based porous metal organic framework catalyst, characterized in that: include: Mixing Zr salt and 1,3,5-benzenetricarboxylic acid in a solvent and stirring at room temperature to form a uniform colloid; the molar ratio of Zr salt to 1,3,5-benzenetricarboxylic acid is 1:1; The uniform colloid is subjected to a hydrothermal reaction to obtain a white granular solid; The white granular solid is freeze-dried, ground and sieved to obtain a zirconium-based porous metal organic framework catalyst.
2. The method for preparing a zirconium-based porous metal organic framework catalyst according to claim 1, characterized in that: The Zr salt is any one of zirconium chloride and zirconium oxide chloride.
3. The zirconium-based porous metal-organic framework catalyst prepared according to the preparation method of the zirconium-based porous metal-organic framework catalyst according to claim 1 or 2.
4. Use of the zirconium-based porous metal organic framework catalyst according to claim 3 in the process of preparing amides by condensation of amine acids.
5. The use of the zirconium-based porous metal organic framework catalyst according to claim 4 in the process of preparing amides by condensation of amine acids, characterized in that: A zirconium-based porous metal organic framework catalyst, benzoic acid, benzylamine and a reaction solvent are placed in a reaction container, and an amine acid condensation reaction is carried out under nitrogen protection conditions to obtain N-benzylbenzamide.
6. The use of the zirconium-based porous metal organic framework catalyst according to claim 5 in the process of preparing amides by condensation of amine acids, characterized in that: The reaction temperature of the amino acid condensation reaction is 40~120°C, and the reaction time is 2~24h.
7. Use of the zirconium-based porous metal organic framework catalyst according to claim 6 in the process of preparing amides by condensation of amine acids, characterized in that: The reaction temperature of the amino acid condensation reaction is 70~90°C and the reaction time is 8~12h.
8. The use of the zirconium-based porous metal organic framework catalyst according to claim 5 in the process of preparing amides by condensation of amine acids, characterized in that: The reaction solvent of the amine acid condensation reaction is any one of tetrahydrofuran, 1,4-dioxane and toluene, or a mixture of two or more of tetrahydrofuran, ethyl acetate, 1,4-dioxane, ethanol, N,N-dimethylformamide and toluene.
9. The use of the zirconium-based porous metal organic framework catalyst according to claim 8 in the process of preparing amides by condensation of amine acids, characterized in that: The reaction solvent for the amine acid condensation reaction is any one of tetrahydrofuran and toluene.
Citation Information
Patent Citations
Method for preparing amide compound through catalysis of ligand-assisted zirconium oxychloride
CN103274958A
Preparation method for MOF material used for catalysis of amidation reaction
CN107903399A
Method for rapidly synthesizing MOF-808 material with low energy consumption
CN113265058A
Zirconium-based MOF based on amino acid functionalization and preparation method and application thereof
CN117586517A