Preparation method and application of defect modified ZIF-7 material
By introducing zinc salt with anionic steric hindrance effect to change the structure of ZIF-7 material, the problem of poor compatibility between ZIF-7 and resin polymer is solved, significantly improving the mechanical and corrosion resistance of the coating, and controlling the material morphology through different anions is used to regulate the material morphology and particle size, optimize coating performance.
Patent Information
- Application Number
- CN202411307116.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-22
AI Technical Summary
The classic ZIF-7 material has poor compatibility with resin polymer due to structural saturation in the coating system, resulting in insufficient coating performance.
By introducing zinc salts with anionic steric hindrance effect, the framework structure of ZIF-7 material is changed, defects are formed, and the resin polymer molecular chains are promoted to enter the inside of the material, achieving molecular-level mutual penetration and interlocking, and improving compatibility.
The mechanical properties and corrosion resistance of the coating are significantly improved, and the material morphology and particle size are regulated by different anions to optimize the overall performance of the coating.
Smart Images

Figure CN118994623A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of modified nanomaterials, and in particular to a preparation method and application of a defect-modified ZIF-7 material. Background Art
[0002] Metal-organic framework materials (MOFs) are a class of porous materials with periodic crystalline structures formed by the coordination of metal ions and organic ligands. Zeolite imidazolate framework materials (ZIFs) are classic MOFs materials. ZIF-7 with benzimidazole as ligand and NH2-ZIF-7 with composite benzimidazole / 2-aminobenzimidazole have been widely used in the fields of anti-corrosion coatings, antibacterial coatings, self-healing coatings, etc. in recent years. However, the coordination of the internal structure of the classic ZIF-7 material tends to be saturated. In the coating system, only the surface layer of the particles can interact with the resin polymer at the interface, which leads to compatibility problems caused by heterogeneous doping. Summary of the invention
[0003] In order to solve the above technical problems, the present invention provides a method for preparing and applying defect-modified ZIF-7 materials, which uses the anion steric effect to construct "defects" in ZIF-7 materials, changes its original overall regular framework arrangement, and enables more resin polymer molecular chains to energy-savingly penetrate into the interior of the particles, thereby realizing the "interlocking" effect of mutual penetration between polymer and nanomaterial molecules, thereby improving the compatibility with the coating system at the molecular level, and further improving the comprehensive performance of the coating in all aspects.
[0004] A method for preparing a defect-modified ZIF-7 material of the present invention comprises the following steps:
[0005] Step 1: dissolving a zinc salt having an anion steric effect in a synthetic solvent of ZIF-7 for standby use;
[0006] Step 2: dissolving the imidazole ligand of the ZIF-7 material in a synthesis solvent, adding a zinc salt solution, and carrying out a stirring reaction at a set temperature for a set time to synthesize a defect-modified ZIF-7 solution;
[0007] Step 3, separating and drying the defect-modified ZIF-7 solution produced by the synthesis by suction filtration or centrifugation to obtain defect-modified ZIF-7 powder;
[0008] Step 4: The separated defect-modified ZIF-7 powder is mixed into the polymer coating system in proportion.
[0009] Preferably, the anion of the zinc salt having anion steric effect in step 1 is one of phosphate, gluconate and phytate.
[0010] Preferably, the synthesis solvent in step 1 is one or more of N,N-dimethylformamide, water, ethanol and methanol.
[0011] Preferably, the ligand-containing ZIF-7 in step 2 is a single ligand ZIF-7 (the ligand is only benzimidazole) or a composite ligand ZIF-7 (a mixed ligand of benzimidazole and 2-aminobenzimidazole).
[0012] Preferably, the set temperature in step 2 is 25-120° C., and the set time in step 2 is 2-72 hours.
[0013] Preferably, the polymer coating system in step 4 includes one or more of an acrylic resin system, an epoxy resin system, a polyurethane resin system, and an alkyd resin system.
[0014] Preferably, the doping ratio of the defect-modified ZIF-7 powder to the polymer resin in step 4 is 1:100-1:10.
[0015] The invention discloses an application of a defect-modified ZIF-7 material, wherein the defect-modified ZIF-7 material has an application field of coating.
[0016] Compared with the prior art, the beneficial effects of the present invention are as follows: in order to solve the "heterogeneous phase" problem existing in the application of classic ZIF-7 nanomaterials in the field of coatings, the ZIF-7 material is used to change the original regular framework structure of ZIF-7 by the anion steric effect, and defects are constructed to prepare defect-modified ZIF-7-based coatings with better comprehensive performance; at the same time, the anions such as phosphate, gluconate and phytate used to construct defects transform the ZIF-7 material into a variety of morphological sizes such as two-dimensional sheets and three-dimensional spherical porous materials, and form a strong hydrogen bond effect with the resin skeleton, thereby further improving the mechanical properties of the coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 TEM morphology (a) and corresponding XRD spectrum (b) of phosphate-defect modified ZIF-7 (Phosphate-ZIF-7) in Example 1;
[0018] Figure 2 TEM morphology (a) and corresponding XRD spectrum (b) of gluconate-ZIF-7 modified with gluconate in Example 2;
[0019] Figure 3 TEM morphology (a) and corresponding XRD spectrum (b) of phytate-ZIF-7 modified with phytate in Example 3;
[0020] Figure 4 TEM morphology (a) and corresponding XRD spectrum (b) of ZIF-7 (NH2-gluconate-ZIF-7) with amino-complex ligand modified by gluconate defect in Example 4;
[0021] Figure 5 It is a schematic flow chart of the preparation method of the defect-modified ZIF-7 material of the present invention. DETAILED DESCRIPTION
[0022] In order to facilitate understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thorough and comprehensive.
[0023] Example 1
[0024] The preparation method and application of a defect-modified ZIF-7 material of the present invention selects phosphate as anion, zinc phosphate as a zinc source for synthesizing ZIF-7, and the ligand is a classic single benzimidazole of ZIF-7. The experimental steps are as follows:
[0025] Step 1: Dissolve 0.4214 g of zinc phosphate tetrahydrate in 50 mL of water for later use;
[0026] Step 2: Dissolve 0.5018 g of benzimidazole in 150 mL of water by ultrasonication, add the prepared zinc phosphate tetrahydrate solution, and stir at 30° C. for 24 hours, which is recorded as Phosphate-ZIF-7;
[0027] Step 3, centrifugally drying the reacted Phosphate-ZIF-7;
[0028] Step 4: Phosphate-ZIF-7 and water-based silicone-modified acrylic resin were mixed at a mass ratio of 1:50 to prepare defect-modified ZIF-7-based coating, which was applied on a carbon steel substrate and cured at 50°C, and a control sample of blank resin was prepared. A dumbbell-shaped mold was used to prepare tensile mechanical properties.
[0029] In this example, the TEM morphology of defect-modified Phosphate-ZIF-7 is as follows: Figure 1 As shown in a, it is a three-dimensional spherical porous material with a particle size of 60-150nm. The corresponding XRD spectrum is shown in Figure 1 As shown in b, compared with the spectrum of the classic ZIF-7, the crystal structure has undergone a major transformation, which confirms that the regular framework structure of ZIF-7 has undergone a major transformation, namely, defect formation.
[0030] The tensile test was carried out on the tensile specimens prepared by dumbbell-shaped molds. The results showed that the maximum tensile stress of the blank water-based silicone-modified acrylic resin was 6.3±0.2Mpa, which was increased to 17.5±0.5MPa after adding Phosphate-ZIF-7, and the mechanical properties of the coating were significantly improved.
[0031] The electrochemical impedance spectroscopy test of the sample coated on the carbon steel substrate showed that the impedance modulus of the blank coating on the carbon steel substrate at 0.01 Hz was 43651 Ω·cm 2 , and then doped with Phosphate-ZIF-7 to 245610Ω·cm 2 , it has been improved by an order of magnitude, and the corrosion resistance of the coating has been significantly improved.
[0032] Example 2
[0033] The preparation method and application of a defect-modified ZIF-7 material of the present invention selects gluconate as anion, zinc gluconate as a zinc source for synthesizing ZIF-7, and the ligand is a classic single benzimidazole of ZIF-7. The experimental steps are as follows:
[0034] Step 1: Dissolve 0.4192 g of zinc gluconate in 50 mL of water for later use;
[0035] Step 2: Dissolve 0.5018 g of benzimidazole in 150 mL of water by ultrasonication, add the prepared zinc gluconate solution, and stir at 30° C. for 24 hours, which is recorded as Gluconate-ZIF-7;
[0036] Step 3, centrifugally drying the reacted Gluconate-ZIF-7;
[0037] Step 4: Mix Gluconate-ZIF-7 and waterborne epoxy resin at a mass ratio of 1:60 to prepare defect-modified ZIF-7-based coating. Apply it on a T2 copper substrate and cure it at 30°C. Prepare a control sample of blank resin and prepare a tensile mechanical property sample using a dumbbell-shaped mold.
[0038] In this example, the TEM morphology of defect-modified Gluconate-ZIF-7 is as follows: Figure 2 As shown in a, it is a square layer structure with a diagonal length of about 500nm-1μm. The corresponding XRD spectrum is as follows Figure 2 As shown in b, compared with the spectrum of the classic ZIF-7, the crystal structure has undergone a major transformation, which confirms that the regular framework structure of ZIF-7 has undergone a major transformation, namely, defect formation.
[0039] The tensile test was carried out on the tensile specimens prepared by dumbbell-shaped molds. The results showed that the maximum tensile stress of the blank water-based epoxy resin was 7.1±0.3Mpa, which was increased to 27.5±0.4MPa after adding Gluconate-ZIF-7, and the mechanical properties of the coating were significantly improved.
[0040] The electrochemical impedance spectroscopy test of the sample coated on the T2 copper substrate showed that the impedance modulus of the blank coating on the copper substrate at 0.01 Hz was 681241 Ω·cm 2 , after being doped with Gluconate-ZIF-7, it increased to 9467512Ω·cm 2 , the corrosion resistance of the coating is significantly improved.
[0041] Example 3
[0042] The preparation method and application of a defect-modified ZIF-7 material of the present invention selects phytate as anion, uses zinc phytate as a zinc source for synthesizing ZIF-7, and the ligand is a classic single benzimidazole of ZIF-7. The experimental steps are as follows:
[0043] Step 1: Dissolve 0.957 g of zinc gluconate in 100 mL of water for later use;
[0044] Step 2: Dissolve 0.5018 g of benzimidazole in 100 mL of water by ultrasonication, add the prepared zinc phytate solution, and stir at 30° C. for 24 hours, which is recorded as Phytate-ZIF-7;
[0045] Step 3, centrifugally drying the reacted Phytate-ZIF-7;
[0046] Step 4: Phytate-ZIF-7 and waterborne polyurethane resin were mixed at a mass ratio of 1:40 to prepare defect-modified ZIF-7-based coating, which was applied on an aluminum alloy substrate and cured at 100°C, and a control sample of blank resin was prepared. A dumbbell-shaped mold was used to prepare tensile mechanical properties.
[0047] In this example, the TEM morphology of defect-modified Phytate-ZIF-7 is as follows: Figure 3 As shown in a, it is an amorphous porous spherical cluster block structure, and the corresponding XRD spectrum is shown in Figure 3 As shown in (b), compared with the spectrum of the classic ZIF-7, the crystal structure has undergone a major transformation and is almost in an amorphous state, with only a crystalline peak near 2θ of 8°, which confirms that the regular framework structure of ZIF-7 has undergone a major transformation, that is, the framework structure has been disassembled and defects have been formed.
[0048] The tensile test was carried out on the tensile specimens prepared by dumbbell-shaped molds. The results showed that the maximum tensile stress of the blank waterborne polyurethane resin was 10.4±0.6Mpa, which increased to 34.2±0.2MPa after adding Phytate-ZIF-7, and the mechanical properties of the coating were significantly improved.
[0049] The electrochemical impedance spectroscopy test of the sample coated on the aluminum alloy substrate showed that the impedance modulus of the blank coating on the copper substrate at 0.01 Hz was 681241 Ω·cm 2 , after being doped with Gluconate-ZIF-7, it increased to 9467512Ω·cm 2 , the corrosion resistance of the coating is significantly improved.
[0050] Example 4
[0051] The preparation method and application of a defect-modified ZIF-7 material of the present invention selects gluconate as anion, zinc gluconate as a zinc source for synthesizing ZIF-7, and the ligand is a composite ligand, and benzimidazole and 2-aminobenzimidazole are used as ligands. The experimental steps are as follows:
[0052] Step 1: Dissolve 0.4192 g of zinc gluconate in 50 mL of water for later use;
[0053] Step 2: 0.3 g of benzimidazole and 0.6 g of 2-aminobenzimidazole were ultrasonically dissolved in a mixed solvent of 50 mL of DMF and 50 mL of ethanol, and the prepared zinc gluconate solution was added, and the mixture was reacted in a hydrothermal reactor at 120° C. for 2 hours, which was recorded as NH2-gluconate-ZIF-7.
[0054] Step 3, centrifugally drying the reacted NH2-gluconate-ZIF-7;
[0055] Step 4: Mix NH2-gluconate-ZIF-7 and alkyd resin in a mass ratio of 1:45 to prepare defect-modified ZIF-7-based coating. Apply on galvanized steel substrate, cure at 60°C, and prepare a control sample of blank resin. Use a dumbbell-shaped mold to prepare tensile mechanical properties.
[0056] In this example, the TEM morphology of defect-modified NH2-gluconate-ZIF-7 is as follows: Figure 4 As shown in a, it is a three-dimensional porous spherical structure with a small particle size. The corresponding XRD spectrum is shown in Figure 4 As shown in (b), compared with the spectrum of the classic ZIF-7, the crystal structure has undergone a major transformation and is almost in an amorphous state. There is a strong crystallization peak near 2θ of 12°, which confirms that the regular framework structure of ZIF-7 has undergone a major transformation, namely, the framework structure is reconstructed and defects are formed.
[0057] The tensile test was carried out on the tensile specimens prepared by dumbbell-shaped molds. The results showed that the maximum tensile stress of the blank alkyd resin was 8.6±0.2Mpa, which was increased to 24.9±0.5MPa after adding NH2-gluconate-ZIF-7, and the mechanical properties of the coating were significantly improved.
[0058] The electrochemical impedance spectroscopy test of the samples coated on the aluminum alloy substrate showed that the impedance modulus of the blank coating on the galvanized steel substrate at 0.01 Hz was 9861 Ω·cm 2 , and then doped with NH2-gluconate-ZIF-7 to 57923Ω·cm 2 , the corrosion resistance of the coating is significantly improved.
[0059] The main functions achieved by the present invention are:
[0060] 1. Defect-modified ZIF-7 material improves compatibility with the coating at the molecular level and improves the comprehensive mechanical properties of the coating;
[0061] 2. Defect-modified ZIF-7 material improves the corrosion resistance of the coating;
[0062] 3. Defect-modified ZIF-7 materials can be modified to have two-dimensional sheets, three-dimensional porous, amorphous porous and other morphologies by using anions of different steric hindrance sizes. The synthesis conditions can also be adjusted to achieve particle size control.
[0063] The preparation method and application of the defect-modified ZIF-7 material of the present invention, the installation method, connection method or setting method thereof are all common mechanical methods, and any method that can achieve its beneficial effects can be implemented.
[0064] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a defect-modified ZIF-7 material, characterized in that: The following steps are involved: Step 1: dissolving a zinc salt having an anion steric effect in a synthetic solvent of ZIF-7 for standby use; Step 2: dissolving the imidazole ligand of the ZIF-7 material in a synthesis solvent, adding a zinc salt solution, and carrying out a stirring reaction at a set temperature for a set time to synthesize a defect-modified ZIF-7 solution; Step 3, separating and drying the defect-modified ZIF-7 solution produced by the synthesis by suction filtration or centrifugation to obtain defect-modified ZIF-7 powder; Step 4: The separated defect-modified ZIF-7 powder is mixed into the polymer coating system in proportion.
2. A method for preparing a defect-modified ZIF-7 material as claimed in claim 1, characterized in that, In the step 1, the anion of the zinc salt having anion steric hindrance effect is one of phosphate, gluconate and phytate.
3. A method for preparing a defect-modified ZIF-7 material as claimed in claim 1, characterized in that, The synthesis solvent in step 1 is one or more of N,N-dimethylformamide, water, ethanol and methanol.
4. A method for preparing a defect-modified ZIF-7 material as claimed in claim 1, characterized in that, The ligand-containing ZIF-7 in step 2 is single-ligand ZIF-7 or composite-ligand ZIF-7.
5. A method for preparing a defect-modified ZIF-7 material as claimed in claim 1, characterized in that, The set temperature in step 2 is 25-120° C., and the set time in step 2 is 2-72 hours.
6. A method for preparing a defect-modified ZIF-7 material as claimed in claim 1, characterized in that, The polymer coating system in step 4 includes one or more of an acrylic resin system, an epoxy resin system, a polyurethane resin system, and an alkyd resin system.
7. A method for preparing a defect-modified ZIF-7 material as claimed in claim 1, characterized in that, The doping ratio of the defect-modified ZIF-7 powder to the polymer resin in the step 4 is 1:100-1:
10.
8. An application of defect-modified ZIF-7 material, characterized in that: The defect-modified ZIF-7 material as claimed in claim 1 is applied in the coating field.