Preparation method and application of metal covalent organic framework composite material

By growing COF-LZU1 layer in situ on UIO-66-NH2, UiO-66-NH2@COF-LZU1 composite material was prepared, combining the characteristics of MOFs and COFs, the stability and functionality of existing porous adsorbent materials were solved. In terms of limitations, higher adsorption performance and separation effect are achieved, especially excellent performance in carbon dioxide adsorption and CO2/CH4 separation.

CN118994625APending Publication Date: 2024-11-22GUANGDONG LABORATORY OF CHEMISTRY & FINE CHEMICAL IND JIEYANG CENTER JIEYANG
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411369426.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing porous adsorption materials such as MOFs and COFs have limitations in stability and functionality, especially in poor performance in carbon dioxide adsorption and separation applications.

Method used

By growing COF-LZU1 layer in situ on UIO-66-NH2, UiO-66-NH2@COF-LZU1 (MCOF-x) composite material was prepared, combining the characteristics of MOFs and COFs, and using a condensation reaction method to avoid harsh synthesis Conditions to achieve efficient batch preparation.

Benefits of technology

The obtained MCOF-x composite materials show higher stability, larger surface area and better adsorption properties, especially in carbon dioxide adsorption and CO2/CH4 separation, providing new solutions to environmental pollution and resource utilization. Ideas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994625A_ABST
    Figure CN118994625A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a metal covalent organic framework composite material, and belongs to the technical field of porous adsorption materials. The preparation method comprises the following steps: by taking UIO-66-NH2 as a core, firstly, reacting with an aldehyde group building block (BTCA) of COF-LZU1 to generate aldehyde functionalized UiO-66-NH2 (CHO); then, PDA is connected to the UiO-66-NH2 (CHO) through a condensation reaction, so that a COF-LZU1 layer is constructed, and the UiO-66-NH2 (at) COF-LZU1 composite material is formed. The composite material has octahedral structure characteristics, has a rough surface, and has excellent carbon dioxide adsorption performance and good carbon dioxide / methane separation performance. Meanwhile, by means of the preparation method of the composite material, the adsorption effect of pure COF-LZU1 powder on carbon dioxide (CO2) can be remarkably improved, the synergistic enhancement effect is achieved, and a new thought is provided for further optimizing and designing a novel composite material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of porous adsorption materials, and specifically relates to a preparation method and application of a metal covalent organic framework composite material. Background Art

[0002] With the continuous growth of the global population and the rapid development of industrialization, the demand for energy is becoming increasingly urgent. Energy, as an indispensable basic resource for the development of modern society, is directly related to the sustainable development of the economy and the improvement of the quality of human life. However, energy is currently mainly obtained by relying on fossil fuels, biomass combustion and animal metabolism, all of which will produce a large amount of carbon dioxide. CO2 is one of the main gases that cause the greenhouse effect. Excessive emissions of CO2 cause an imbalance in the carbon content in the regional ecological environment system, which in turn leads to global warming, glacier melting, ocean acidification, sea level rise, and frequent disasters such as droughts and hurricanes, posing a serious threat to the ecological environment and the sustainable development of the world economy. Therefore, reducing CO2 emissions has become a key problem that must be faced and solved for sustainable economic development.

[0003] Porous crystalline materials are composed of inorganic and organic materials, such as zeolites, metal-organic frameworks (MOFs), covalent organic frameworks (COFs) and porous organic cages. They have clear topological structures and inherent porosity, and show great potential in the fields of catalysis, gas adsorption and separation. Among them, metal-organic framework materials (MOFs) formed by the coordination of metal ions or metal clusters with organic ligands are a class of porous crystalline materials with high specific surface area, adjustable pore structure and multiple functions. The uniform distribution of metal ions expands the physicochemical properties of the material. However, the limited stability of the coordination bonds limits the application range of this material. Covalent organic framework materials (COFs) have also emerged as a new type of crystalline porous material. It is a porous crystalline polymer composed entirely of organic monomers through reversible covalent bonds (such as BO, C=N, CN, C=C, etc.), which makes COFs highly chemically and thermally stable and not easily corroded by chemical reagents or dissociated at high temperatures. However, since COFs are mainly composed of light elements such as C, O, and N, their functions are relatively simple and there are some challenges in molecular stacking and biocompatibility.

[0004] In recent years, new MOFs-based hybrid materials have been successfully prepared by hybridizing MOFs with other functional materials (such as metal nanoparticles (NPs), polymers, and other MOFs, etc.), so that the obtained materials have the structural characteristics of a single component and show new properties. In particular, core-shell MOFs@MOFs hybrids are prepared by wrapping one MOFs on the surface of another MOFs, which show better performance than single-type MOFs in the presence of synergistic effects. The successful preparation of core-shell MOFs@MOFs composites provides researchers with inspiration for exploring the synthesis of core-shell MOFs@COFs composites (MCOFs). This type of material introduces metal elements during the synthesis of a highly stable COFs skeleton, which is similar to building a bridge between MOFs and COFs to give full play to their respective advantages and make up for their defects. Despite this, there are relatively few systematic studies on MCOFs composites, and there are still many unknowns.

[0005] In general, UiO-66-NH2 is an amino-modified zirconium-based porous material with advantages such as good water stability, good chemical stability, strong heat resistance and simple preparation. The presence of amino (-NH2) groups allows the in-situ growth of COF layers directly on the surface of MOFs without additional functionalization steps. COF-LZU1 is a two-dimensional layered porous material with abundant benzene rings and nitrogen-containing groups, which has high stability in water and most organic solvents. This material has low density, rich functional groups, good crystallinity and excellent thermal stability, and shows good application prospects in the field of gas adsorption. Summary of the invention

[0006] The present invention aims to solve at least one of the technical problems in the related art to a certain extent. To this end, the main purpose of the present invention is to provide a method for preparing a metal covalent organic framework composite material, which overcomes the inherent limitations of MOFs and COFs materials; the preparation method successfully obtains a UiO-66-NH2@COF-LZU1 (MCOF-x) composite material by in-situ growing a COF-LZU1 layer on UIO-66-NH2.

[0007] The present invention also aims to provide the use of the metal covalent organic framework composite material in carbon dioxide adsorption and / or carbon dioxide / methane separation.

[0008] The objective of the present invention is achieved through the following technical solutions:

[0009] The basic concept of the present invention is: This study takes UIO-66-NH2 as the core, and first reacts with the aldehyde building block of COF-LZU1 to generate aldehyde-functionalized UiO-66-NH2 (CHO); then, PDA is connected to UiO-66-NH2 (CHO) through a condensation reaction at room temperature to successfully prepare MCOF-x composite materials. The resulting composite material has the characteristics of both COFs and MOFs, showing higher stability, larger surface area and better adsorption performance. Compared with the traditional COFs synthesis method, this method not only avoids harsh synthesis conditions, but also can efficiently prepare MCOFs composite materials in batches. This discovery provides a new idea for solving problems such as environmental pollution and resource utilization.

[0010] A method for preparing a metal covalent organic framework composite material, wherein UIO-66-NH2 is used as a core, and first reacts with the aldehyde building block of COF-LZU1 to generate aldehyde-functionalized UiO-66-NH2 (CHO). Then, PDA is connected to UiO-66-NH2 (CHO) through a condensation reaction to construct a COF-LZU1 layer, forming a UiO-66-NH2@COF-LZU1 composite material, i.e., a metal covalent organic framework composite material.

[0011] In some specific implementations, the steps include:

[0012] 1) Preparation of UIO-66-NH2: Zirconium chloride (ZrCl4) and 2-aminoterephthalic acid (BDC-NH2) are fully dissolved in a first solvent, mixed evenly, and then a catalyst is added, heated to react, washed, dried, and purified to obtain UiO-66-NH2 nanoparticles.

[0013] 2) Preparation of UiO-66-NH2@COF-LZU1 (MCOF-x) composite material: The activated UiO-66-NH2 nanoparticles and trimesic acid (BTCA) are fully dissolved in the second solvent, a catalyst is added, mixed, p-phenylenediamine (PDA) solution is added, allowed to react, washed, and dried to obtain a UiO-66-NH2@COF-LZU1 composite material, i.e., a metal covalent organic framework composite material.

[0014] In certain specific embodiments, the molar ratio of zirconium chloride to 2-aminoterephthalic acid in step 1) is 1:(1-3); the first solvent is N,N-dimethylformamide (DMF); and the catalyst in step 1) is acetic acid (HAc).

[0015] In certain specific embodiments, the amount ratio of DMF and HAc in step 1) is (5-20):1; the uniform mixing method is ultrasonic dispersion, and the ultrasonic dispersion time is 10-30 minutes; the heating reaction condition is heating at 60-180°C for 12-36 hours.

[0016] In some specific embodiments, the washing reagent in step 1) is one or more of acetone, methanol, THF, and DMF; the purification reagent is one or more of acetone, methanol, THF, and DMF; and the drying condition is vacuum drying at 60-180°C for 12-36h.

[0017] In certain specific embodiments, in step 2), the mass ratio of trimesaldehyde to UiO-66-NH2 nanoparticles is 3:(1-6); the second solvent is 1,4-dioxane; and the catalyst is acetic acid (HAc).

[0018] In certain specific embodiments, the molar ratio of trimesaldehyde to p-phenylenediamine in step 2) is 1-3:2-4; the dispersion solvent of PDA is 1,4-dioxane; the mixing method is ultrasonic dispersion; and the ultrasonic dispersion time is 10-30 min.

[0019] In some specific embodiments, the static reaction in step 2) is carried out at room temperature of 25-30°C for 1-3 days; the washing reagent is one or more of acetone, methanol, THF, and DMF; and the drying condition is vacuum drying at 60-180°C for 12-36h.

[0020] A metal covalent organic framework composite material prepared by the above-mentioned preparation method.

[0021] An application of the aforementioned metal covalent organic framework composite material in carbon dioxide adsorption and / or carbon dioxide / methane separation.

[0022] Compared with the prior art, the present invention has at least the following advantages:

[0023] 1) The preparation method of the metal covalent organic framework composite material provided by the present invention takes UIO-66-NH2 as the core. The presence of -NH2 enables COF-LZU1 to directly grow a COF layer in situ on its surface without an additional functionalization step. The obtained UiO-66-NH2@COF-LZU1 composite material has the characteristics of both COFs and MOFs, and has higher stability, larger surface area and better adsorption performance;

[0024] 2) The UiO-66-NH2@COF-LZU1 composite material obtained by the present invention has a more stable multilayer pore structure and abundant active functional groups;

[0025] 3) The UiO-66-NH2@COF-LZU1 composite material obtained in the present invention also exhibits good adsorption capacity (CO2) and separation effect (CO2 / CH4). BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the specific embodiments of the present invention, the drawings required for use in the specific embodiments or the description of the prior art will be briefly introduced below.

[0027] Figure 1 is a preparation flow chart of the MCOF-X composite material prepared in the present invention;

[0028] Figure 2 This is the XRD pattern of the MCOF-200 composite material prepared in Example 3 of the present invention;

[0029] Figure 3 FT-IR image of the MCOF-200 composite material prepared in Example 3 of the present invention;

[0030] Figure 4 TGA graph of the MCOF-X composite material prepared in Examples 1-4 of the present invention;

[0031] Figure 5 This is a SEM image of the MCOF-200 composite material prepared in Example 3 of the present invention;

[0032] Figure 6 TEM image of the MCOF-200 composite material prepared in Example 3 of the present invention and the corresponding element distribution map;

[0033] Figure 7 This is the CO2 adsorption curve of the MCOF-200 composite material prepared in Example 3 of the present invention at 273 / 298K and 1 bar;

[0034] Figure 8 CO2 adsorption capacity of the MCOF-X composite material prepared in Examples 1-4 of the present invention at 273 / 298K and 1 bar;

[0035] Fig. 9 CO2 and CH4 adsorption curves of the MCOF-200 composite material prepared in Example 3 of the present invention at 273K (relative pressure (P / P0) = 0-1);

[0036] Fig.10 This is the CO2 and CH4 adsorption curve of the MCOF-200 composite material prepared in Example 3 of the present invention at 273K. (Relative pressure (P / P0) = 0-0.12). DETAILED DESCRIPTION

[0037] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. The following embodiments are only illustrative and not restrictive, and the protection scope of the present invention cannot be limited thereto.

[0038] When a certain amount, concentration or other value or parameter is expressed in the form of a range, a preferred range, or a preferred upper and lower numerical limit, it should be understood that it is equivalent to specifically revealing any range by combining any pair of upper range limits or preferred numerical values ​​with any lower range limit or preferred numerical value, regardless of whether the range is specifically disclosed. Unless otherwise indicated, the numerical range values ​​listed herein include the endpoints of the range, and all integers and fractions within the range.

[0039] Unless otherwise indicated, all percentages, parts, ratios, etc. herein are by weight.

[0040] The materials, methods, and examples herein are illustrative and are not to be construed as limiting unless specifically stated.

[0041] In the following examples, all samples were analytically pure and used directly in the experiment without further purification. Zirconium chloride was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. with a purity of 98%; 2-aminoterephthalic acid was purchased from Shanghai Bid Pharmaceutical Technology Co., Ltd. with a purity of 95%; trimesic acid was purchased from Shanghai Bid Pharmaceutical Technology Co., Ltd. with a purity of 96%; p-phenylenediamine was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. with a purity of 97%; acetic acid was purchased from Guangzhou Xinhong Trading Co., Ltd.; DMF, 1,4-dioxane, THF, acetone, methanol, etc. were all purchased from Guangzhou Baijun Technology Co., Ltd.

[0042] The test methods used in the following embodiments include:

[0043] By testing the main properties of each test sample separately, its structural properties and adsorption performance under different conditions are reflected; the main properties tested in this application include multiple aspects, including but not limited to the following:

[0044] 1) Crystallinity test;

[0045] The X-ray diffraction patterns of the samples were obtained using a powder X-ray diffractometer (XRD). According to the method reported in the literature, the X-ray intensity reflected or scattered from the sample surface was measured at different angles and converted into specific parameter values. The data obtained and the spectrum data obtained by software simulation were processed and analyzed using origin software to obtain detailed results on the crystallization properties of the composite material. Model used: Japan Rigaku MiniFlex600.

[0046] 2) Surface functional group test

[0047] The surface functional groups of the composite material were tested using a Fourier transform infrared spectrometer (FT-IR). This method mainly involves mixing and grinding the fully dried sample with potassium bromide powder, pressing the mixed powder into thin slices using a tablet press, and then placing the thin slices into a special infrared spectrum test instrument for analysis. By recording the intensity changes of the light signal obtained by passing through the sample within a specific wavelength range, and analyzing and processing these signals, the corresponding infrared spectrum can be obtained; the model used is Japan Rigaku MiniFlex600.

[0048] 3) Thermal stability test

[0049] The thermal stability of the samples was tested using a thermogravimetric analyzer (TGA). During the test, nitrogen with a flow rate of 20 mL / min was used as the gas flow medium, and the temperature was gradually increased from room temperature to 100°C at a heating rate of 10°C / min, and maintained for 30 minutes to remove excess moisture. The temperature was then increased to 800°C at the same rate to evaluate the mass loss and thermal stability of the samples; the model used was the American TA Discovery TGA 550.

[0050] 4) Morphology test

[0051] The morphology of different samples was observed by cold field emission scanning electron microscopy (SEM) and transmission electron microscopy (TEM). SEM sample preparation method: aluminum foil was used as a carrier, the conductive glue was glued to the sample stage, the liquid sample dissolved in anhydrous ethanol by ultrasound was dripped onto the aluminum foil through a capillary, and after the solvent evaporated, gold spraying (current 10mA, time 50s) and SEM testing (acceleration voltage 10kV, acceleration current 10μA) were performed; the model used: cold field Hitachi S4800 of Hitachi, Japan;

[0052] TEM sample preparation method: The fully ground sample is dispersed in anhydrous ethanol, ultrasonically dissolved to obtain a uniform dispersion, and then dripped onto a copper grid to observe its TEM image (observation voltage 120kV). An EDS spectrometer is used to record the elemental composition and content distribution of the selected area. Model used: Japan JEOL JEM-F200.

[0053] 5) Adsorption test

[0054] The carbon dioxide / methane adsorption isotherms of the samples under different conditions were tested using a fully automatic specific surface and porosity analyzer (BET). The samples were degassed and dried at 120°C for 8 hours before the adsorption test. The test temperature was 273K and 298K, and the test pressure was 0-750mmHg. The model used was the American Micromeritecs ASAP2020.

[0055] Example 1

[0056] This embodiment provides a method for preparing a metal covalent organic framework composite material (such as Figure 1 As shown), it comprises the following steps:

[0057] (1) Preparation of UIO-66-NH2: 5.29 mg ZrCl4 (0.045 mmol) and 8.15 mg 2-aminoterephthalic acid (BDC-NH2, 0.045 mmol) were dissolved in 10 mL N,N-dimethylformamide (DMF), and then 1 mL acetic acid (HAc) was added. After the solution was mixed by ultrasonication until uniform, it was transferred into a stainless steel reactor and heated in a forced air drying oven at 120°C for 24 h. After the reaction, UiO-66-NH2 nanoparticles were obtained by washing, drying and purification.

[0058] (2) Preparation of UiO-66-NH2@COF-LZU1 (MCOF-50) composite material: 150 mg of pyridine trimesaldehyde (BTCA) was dissolved in 40 mL of 1,4-dioxane, 1 mL of acetic acid was added as a catalyst, and after mixing evenly, 50 mg of activated UiO-66-NH2 nanoparticles were added and stirred at room temperature until the mixture became more uniform. Subsequently, 150 mg of p-phenylenediamine (PDA) was dissolved in 20 mL of 1,4-dioxane and added to the above mixed solution. The mixture was allowed to stand at room temperature for 3 days. After the reaction was completed, the obtained solid was washed several times with tetrahydrofuran (THF) and methanol, and dried to obtain the MCOF-50 composite material.

[0059] The present application conducts performance tests on the prepared MCOF-50 composite material, specifically:

[0060] The CO2 adsorption performance of the MCOF-50 composite material of this embodiment at 1 bar and 273 / 298 K was studied by a fully automatic specific surface and porosity analyzer. The results showed that the material was degassed at 120 ° C for 8 h before the adsorption experiment, and the CO2 adsorption capacity of the composite material at 273 / 298 K was 20.06 / 11.37 cm 3 / g.

[0061] Example 2

[0062] This embodiment provides a method for preparing a metal covalent organic framework composite material, which comprises the following steps:

[0063] Preparation of UIO-66-NH2: 5.29 mg ZrCl4 (0.045 mmol) and 8.15 mg 2-aminoterephthalic acid (BDC-NH2, 0.045 mmol) were dissolved in 10 mL N, N-dimethylformamide (DMF), and then 1 mL of acetic acid (HAc) was added. After the solution was mixed evenly by ultrasound, it was transferred into a stainless steel reactor and heated in a blast drying oven at 120 ° C for 24 h. After the reaction, UiO-66-NH2 nanoparticles were obtained by washing, drying and purification;

[0064] (2) Preparation of UiO-66-NH2@COF-LZU1 (MCOF-100) composite material: 150 mg of 2-benzene trimethylene glycol (BTCA) was dissolved in 40 mL of 1,4-dioxane, 1 mL of acetic acid was added as a catalyst, and after mixing evenly, 100 mg of activated UiO-66-NH2 nanoparticles was added. The mixture was stirred at room temperature until the mixture became more uniform to obtain a mixed solution. Subsequently, 150 mg of p-phenylenediamine (PDA) was dissolved in 20 mL of 1,4-dioxane and added to the mixed solution. The mixture was allowed to react at room temperature for 3 days. After the reaction was completed, the obtained solid was washed several times with tetrahydrofuran (THF) and methanol, and dried to obtain the MCOF-100 composite material.

[0065] The present application conducts performance tests on the prepared MCOF-100 composite material, specifically:

[0066] The CO2 adsorption performance of the MCOF-100 composite material in this embodiment at 1 bar and 273 / 298 K was studied by a fully automatic specific surface area and porosity analyzer. The material was degassed at 120 ° C for 8 h before the adsorption experiment. The CO2 adsorption capacity of the composite material at 273 / 298 K was 25.89 / 14.45 cm 3 / g.

[0067] Example 3

[0068] This embodiment provides a method for preparing a metal covalent organic framework composite material, which comprises the following steps:

[0069] (1) Preparation of UIO-66-NH2: 5.29 mg ZrCl4 (0.045 mmol) and 8.15 mg 2-aminoterephthalic acid (BDC-NH2, 0.045 mmol) were dissolved in 10 mL N,N-dimethylformamide (DMF), and then 1 mL acetic acid (HAc) was added. After the solution was mixed by ultrasound, it was transferred into a stainless steel reactor and heated in a blast drying oven at 120°C for 24 h. After the reaction, UiO-66-NH2 nanoparticles were obtained by washing, drying and purification.

[0070] (2) Preparation of UiO-66-NH2@COF-LZU1 (MCOF-200) composite material: 150 mg of 2-benzene trimethylene glycol (BTCA) was dissolved in 40 mL of 1,4-dioxane, 1 mL of acetic acid was added as a catalyst, and after mixing evenly, 200 mg of activated UiO-66-NH2 nanoparticles were added. The mixture was stirred at room temperature until the mixture became more uniform to obtain a mixed solution. Subsequently, 150 mg of p-phenylenediamine (PDA) was dissolved in 20 mL of 1,4-dioxane and added to the mixed solution. The mixture was allowed to react at room temperature for 3 days. After the reaction was completed, the solid was washed several times with tetrahydrofuran (THF) and methanol, and dried to obtain the MCOF-200 composite material.

[0071] The present application conducts performance tests on the prepared MCOF-200 composite material, specifically:

[0072] The CO2 adsorption performance of the MCOF-200 composite material in this embodiment at 1 bar and 273 / 298 K was studied by a fully automatic specific surface area and porosity analyzer. The material was degassed at 120 ° C for 8 h before the adsorption experiment. The CO2 adsorption capacity of the composite material at 273 / 298 K was 38.35 / 21.23 cm 3 / g.

[0073] Example 4

[0074] This embodiment provides a method for preparing a metal covalent organic framework composite material, which comprises the following steps:

[0075] (1) Preparation of UIO-66-NH2: 5.29 mg ZrCl4 (0.045 mmol) and 8.15 mg 2-aminoterephthalic acid (BDC-NH2, 0.045 mmol) were dissolved in 10 mL N,N-dimethylformamide (DMF), and then 1 mL acetic acid (HAc) was added. After the solution was mixed by ultrasound, it was transferred into a stainless steel reactor and heated in a forced air drying oven at 120°C for 24 h. After the reaction, UiO-66-NH2 nanoparticles were obtained by washing, drying and purification.

[0076] (2) Preparation of UiO-66-NH2@COF-LZU1 (MCOF-200) composite material: 150 mg of 2-benzene trimethylene glycol (BTCA) was dissolved in 40 mL of 1,4-dioxane, 1 mL of acetic acid was added as a catalyst, and after mixing evenly, 300 mg of activated UiO-66-NH2 nanoparticles were added. The mixture was stirred at room temperature until the mixture became more uniform to obtain a mixed solution. Subsequently, 150 mg of p-phenylenediamine (PDA) was dissolved in 20 mL of 1,4-dioxane and added to the mixed solution. The mixture was allowed to stand at room temperature for 3 days. After the reaction, the solid was washed several times with tetrahydrofuran (THF) and methanol, and dried to obtain the MCOF-300 composite material.

[0077] The present application conducts performance tests on the prepared MCOF-300 composite material, specifically:

[0078] The CO2 adsorption performance of the MCOF-300 composite material in this embodiment at 1 bar and 273 / 298 K was studied by a fully automatic specific surface area and porosity analyzer. The material was degassed at 120 ° C for 8 h before the adsorption experiment. The CO2 adsorption capacity of the composite material at 273 / 298 K was 43.95 / 25.41 cm 3 / g.

[0079] Performance test case

[0080] The present invention takes Example 3 as an example to perform physical characterization and adsorption / separation performance tests on the prepared MCOF-200 composite material, specifically:

[0081] 1. Physical characterization

[0082] 1) Powder X-ray Diffractometer (XRD)

[0083] Figure 2 XRD spectra of the composite materials of UiO-66-NH2, COF-LZU1 and MCOF-200 prepared in Example 3 of the present invention. It can be observed from the figure that the MCOF-200 composite material simultaneously exhibits signal peaks of COF-LZU1 and UiO-66-NH2, which indicates that the composite material is successfully prepared and maintains its structural integrity.

[0084] 2) Fourier transform infrared spectrometer (FT-IR)

[0085] Figure 3FT-IR spectra of the composite materials of UiO-66-NH2, COF-LZU1 and MCOF-200 prepared in Example 3 of the present invention. It can be observed from the figure that the MCOF-200 composite material contains the absorption peaks of the C=N functional group in COF-LZU1 and the Zr-O, C=O and CO functional groups in UiO-66-NH2, indicating that the MCOF-200 composite material with diversified functional groups has been successfully prepared.

[0086] 3) Thermogravimetric Analyzer (TGA)

[0087] Figure 4 The TGA diagrams of the UiO-66-NH2, COF-LZU1 and MCOF-x composite materials prepared in Examples 1-4 of the present invention show that the prepared composite materials exhibit excellent thermal stability, which provides strong support for their further application.

[0088] 4) Cold field emission scanning electron microscopy (SEM)

[0089] Figure 5 These are the SEM images of the UiO-66-NH2, COF-LZU1 and MCOF-200 composite materials prepared in Example 3 of the present invention. It can be observed from the figure that the skeleton of the prepared MCOF-200 composite material almost inherits the structural characteristics of the uniform octahedron of UiO-66-NH2, but its surface becomes rough due to the formation of the COF-LZU1 layer.

[0090] 5) Transmission electron microscopy (TEM)

[0091] Figure 6 This is a TEM image of the MCOF-200 composite material prepared in Example 3 of the present invention. It can be clearly observed from the figure that the MCOF-200 composite material is a typical core-shell structure. Correspondingly, the EDS surface scanning image shows that the C, N, O and Zr elements are evenly distributed, providing strong evidence for the successful preparation of the UiO-66-NH2@COF-LZU1 composite material.

[0092] 2. Adsorption / separation performance test

[0093] The CO2 adsorption curve (273 / 298K) and methane adsorption curve (273K) of the composite material (MCOF-x) with different UiO-66-NH2 addition conditions were studied using a fully automatic specific surface area and porosity analyzer.

[0094] Figure 7The CO2 adsorption curves of UIO-66-NH2, COF-LZU1 and MCOF-200 composites at different temperatures. It can be clearly seen from the figure that under 273 / 298K conditions, the CO2 adsorption capacity of the composite material MCOF-200 is significantly higher than that of pure COF-LZU1 powder; this result shows that the introduction of MOF (UIO-66-NH2) structure plays an important role in improving the adsorption performance of the material.

[0095] Figure 8 The CO2 adsorption capacity of the composite material (MCOF-x) at different UIO-66-NH2 contents at 1 bar and 273 / 298 K. From the figure, when the UIO-66-NH2 content reaches 200 mg, the obtained composite material (i.e., MCOF-200) shows an adsorption capacity significantly higher than the theoretical calculated value (results are shown in Table 1). This means that the introduction of MOF in the preparation process of the composite material can significantly improve the adsorption effect of pure COF-LZU1 powder on CO2, achieving a synergistic enhancement effect.

[0096] Table 1 Adsorption properties of MCOF-x composites

[0097]

[0098] Fig. 9 and Fig.10 is the adsorption isotherm of CO2 and CH4 at 273K and 1.0 bar for the MCOF-200 composite material in Example 3. As can be seen from the figure, the composite material has a high CO2 / CH4 selectivity, which means that the synthesized MCOF-200 composite material can more effectively separate CO2 from CH4.

[0099] In summary, the preparation method of the metal covalent organic framework composite material provided by the present invention is to prepare the MCOF-x composite material by introducing different amounts of UIO-66-NH2. After a large number of experimental screenings, it is confirmed that increasing the amount of UIO-66-NH2 within an appropriate range can significantly improve the mechanical strength, thermal stability and chemical stability of the composite material. However, adding too much or too little UIO-66-NH2 will cause the performance of the composite material to deteriorate or fail to achieve the expected effect. In addition, under certain conditions, as the amount of UIO-66-NH2 added increases, the composite material exhibits better adsorption and separation effects. It is worth noting that when the content of UIO-66-NH2 reaches 200 mg, the resulting composite material (i.e., MCOF-200) shows an adsorption capacity significantly higher than the theoretical calculated value. This means that the introduction of MOF in the preparation process of the composite material can significantly improve the adsorption effect of pure COF-LZU1 powder on CO2 and achieve a synergistic enhancement effect. This discovery provides new ideas for further optimizing and designing new composite materials, and the prepared MCOF-200 composite material can more effectively separate CO2 from CH4.

[0100] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be included in the scope of the claims and specification of the present invention.

Claims

1. A method for preparing a metal covalent organic framework composite material, characterized in that: It takes UIO-66-NH2 as the core, which first reacts with the aldehyde building block of COF-LZU1 to generate aldehyde-functionalized UiO-66-NH2(CHO); then PDA is connected to UiO-66-NH2(CHO) through condensation reaction to construct the COF-LZU1 layer, forming the UiO-66-NH2@COF-LZU1 composite material, that is, a metal covalent organic framework composite material.

2. The method for preparing the metal covalent organic framework composite material according to claim 1, characterized in that: The specific steps include: 1) Preparation of UIO-66-NH2: Zirconium chloride and 2-aminoterephthalic acid are fully dissolved in a first solvent, mixed evenly, and then a catalyst is added, heated for reaction, washed, dried, and purified to obtain UiO-66-NH2 nanoparticles. 2) Preparation of UiO-66-NH2@COF-LZU1 composite material: The activated UiO-66-NH2 nanoparticles and trimesaldehyde are fully dissolved in the second solvent, a catalyst is added, mixed, p-phenylenediamine solution is added, allowed to react, washed, and dried to obtain the UiO-66-NH2@COF-LZU1 composite material, i.e., a metal covalent organic framework composite material.

3. The method for preparing the metal covalent organic framework composite material according to claim 1, characterized in that: The molar ratio of zirconium chloride to 2-aminoterephthalic acid in step 1) is 1:(1-3); the first solvent is N,N-dimethylformamide; the catalyst in step 1) is acetic acid.

4. The method for preparing the metal covalent organic framework composite material according to claim 3, characterized in that: Step 1) The amount ratio of N,N-dimethylformamide to acetic acid is (5-20):1; the uniform mixing method is ultrasonic dispersion, and the ultrasonic dispersion time is 10-30 minutes; the heating reaction condition is heating at 60-180°C for 12-36 hours.

5. The method for preparing the metal covalent organic framework composite material according to claim 4, characterized in that: Step 1) The washing reagent is one or more of acetone, methanol, THF, and DMF; the purification reagent is one or more of acetone, methanol, THF, and DMF; the drying condition is vacuum drying at 60-180°C for 12-36h.

6. The method for preparing the metal covalent organic framework composite material according to claim 1, characterized in that: In step 2), the mass ratio of trimesaldehyde to UiO-66-NH2 nanoparticles is 3:(1-6); the second solvent is 1,4-dioxane; and the catalyst is acetic acid.

7. The method for preparing the metal covalent organic framework composite material according to claim 2, characterized in that: Step 2) The molar ratio of trimesaldehyde to p-phenylenediamine is 1-3:2-4; the dispersing solvent of p-phenylenediamine is 1,4-dioxane; the mixing method is ultrasonic dispersion; and the ultrasonic dispersion time is 10-30 min.

8. The method for preparing the metal covalent organic framework composite material according to claim 2, characterized in that: Step 2) The static reaction is carried out at room temperature of 25-30°C for 1-3 days; the washing reagent is one or more of acetone, methanol, THF, and DMF; and the drying condition is vacuum drying at 60-180°C for 12-36h.

9. A metal covalent organic framework composite material prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the metal covalent organic framework composite material according to claim 9 in carbon dioxide adsorption and / or carbon dioxide / methane separation.

Citation Information

Cited By

  • Wear-resistant, high-toughness, flame-retardant and heat-resistant BC-coated COF-WEP anticorrosive paint as well as preparation method and coating thereof

    CN119752278A

  • MOF-based gas adsorbent with core-shell-shell structure as well as preparation method and application of MOF-based gas adsorbent

    CN121155535A

  • A ruthenium nanoparticle loaded and amine functionalized zirconium-based metal organic framework catalyst, a preparation method and application thereof

    CN122850272A