Preparation method of antibacterial and anti-adhesion coating based on silicone rubber surface
By preparing the antibacterial coating SR-PDA-Ag-HFPT on the surface of silicone rubber, the antibacterial and anti-adhesion coating is formed by using nucleophilic substitution reaction, which solves the problem of easy adsorption of bacteria on the surface of silicone rubber, and achieves broad-spectrum antibacterial and anti-adhesion The significant improvement in performance significantly improves the safety of biomedical devices.
Patent Information
- Application Number
- CN202310545950.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-16
- Publication Date
- 2024-11-22
AI Technical Summary
The surface of silicone rubber is prone to adsorbing bacteria and proteins, leading to biofilm formation and related inflammation, damaging the therapeutic effect and even leading to morbidity and death. It is necessary to develop an antibacterial and anti-adhesion coating to inhibit the formation of biofilm.
The coating SR-PDA-Ag with antibacterial properties is prepared on the surface of silicon rubber, and the amino group or hydroxyl group on the PDA is used for nucleophilic substitution reaction with hexafluoropropylene trimer (HFPT) to graft to form an antibacterial and anti-adhesion coating. Layer SR-PDA-Ag-HFPT.
The coating has broad-spectrum antibacterial and hydrophobic properties, which significantly inhibit bacterial adhesion and growth, and significantly improves the antibacterial and anti-adhesion capabilities of biomedical devices of silicone rubber materials.
Smart Images

Figure CN118994683A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for preparing an antibacterial and anti-adhesion coating based on a silicone rubber surface, and in particular to the preparation and application of a coating with strong antibacterial ability and significant anti-adhesion ability. Background Art
[0002] Silicone rubber (SR) is widely used in biomedical devices and implants due to its excellent biological inertness, chemical stability and non-irritation to human tissue. However, the SR surface is very susceptible to adsorption of bacteria and proteins, leading to the formation of biofilms and related inflammation, which greatly impairs the therapeutic effect and even causes morbidity and mortality. Therefore, it is crucial to develop antibacterial and anti-adhesion coatings on the SR surface to inhibit the formation of biofilms.
[0003] In an alkaline environment with a pH value of 8.5, dopamine (DA) can form polydopamine (PDA) by self-polymerization. PDA can adhere to various solid substrates to form coatings, and its adhesion mechanism is regulated by various interactions, including hydrogen bonding, chelation, electrostatic and hydrophobic interactions. The surface of the PDA coating has a large number of amino and catechol groups, which can be used to functionally modify the PDA coating. At the same time, the catechol groups can reduce heavy metal salts to metal nanoparticles, such as silver ions to silver nanoparticles, and firmly fix them on the PDA coating. Silver nanoparticles can cause bacterial cell death by reacting with sulfur-containing proteins or sulfhydryl groups in the bacterial cell membrane. Since silver nanoparticles have broad-spectrum antibacterial activity against Gram-positive and Gram-negative bacteria and do not cause drug resistance, the PDA coating has good antibacterial properties after silver nanoparticles are generated.
[0004] Hexafluoropropylene trimer (HFPT) has a hydrophobic perfluoroalkyl group and has three isomers, including T-1, T-2, and T-3 structures, among which T-2 has a stronger reactivity with various nucleophilic reagents. In the presence of triethylamine, the other two structures can be isomerized to T-2 type, which enhances the reactivity with nucleophilic reagents. Hexafluoropropylene trimer can be used to prepare polymers and polymer monomers, and is also widely used as a surfactant in various resins, metals, and coatings.
[0005] A method for preparing an antibacterial and anti-adhesion coating based on a silicone rubber surface is provided herein, wherein HFPT is grafted onto a silicone rubber surface having a silver nano-coating by a nucleophilic substitution reaction, thereby obtaining an antibacterial and anti-adhesion coating. Summary of the invention
[0006] The present invention includes the following steps: firstly, preparing a coating SR-PDA-Ag with antibacterial properties, and further depositing PDA on the surface of the coating. Then, the amino group or hydroxyl group on the PDA is subjected to a nucleophilic substitution reaction with hexafluoropropylene trimer (HFPT) to graft the PDA on the surface of the coating to obtain a coating SR-PDA-Ag-HFPT with antibacterial and anti-adhesion properties.
[0007] The purpose of the present invention is to provide a method for preparing an antibacterial and anti-adhesion coating based on the surface of silicone rubber. The coating has good antibacterial and anti-adhesion capabilities, can be effectively applied to biomedical devices made of silicone rubber materials, and provides a new approach for developing new antibacterial and anti-adhesion coatings.
[0008] The technical solution of the present invention is:
[0009] The preparation method of the SR-PDA-Ag comprises the following steps:
[0010] (1) Preparation of SR-PDA: Silicone rubber (SR) was immersed in the prepared alkaline dopamine solution and reacted at room temperature for 72 hours to obtain the coating SR-PDA.
[0011] (2) Preparation of SR-PDA-Ag: SR-PDA was immersed in the prepared 40-60 mM AgNO3 and reacted at room temperature in the dark for 24 h to obtain SR-PDA-Ag.
[0012] The preparation method of the SR-PDA-Ag-HFPT comprises the following steps:
[0013] (1) The SR-PDA-Ag was re-immersed in the prepared alkaline dopamine solution, reacted at room temperature for 4 to 8 hours, and after drying, was placed in 5 to 10 mL of HFPT and 5 to 10 μL of triethylamine was added. The reaction was carried out at 50 to 70°C for 6 to 8 hours to obtain the antibacterial and anti-adhesion coating SR-PDA-Ag-HFPT.
[0014] Technical analysis of the present invention:
[0015] PDA can adhere to various solid substrates to form coatings. It can adhere to the SR surface through various interactions to obtain SR-PDA coatings, and the catechol groups on PDA can reduce silver ions to silver nanoparticles. At the same time, silver nanoparticles can cause bacterial cell death by reacting with sulfur-containing proteins or sulfhydryl groups in bacterial cell membranes, and have good antibacterial activity against both Gram-positive and Gram-negative bacteria. Therefore, SR-PDA-Ag has good antibacterial activity.
[0016] HFPT has perfluoroalkyl groups and is easy to react with nucleophilic reagents. At the same time, HFPT is cheap and easy to obtain. HFPT can be directly grafted on the surface of SR-PDA-Ag through nucleophilic substitution reaction with amino or hydroxyl groups on PDA, so that a large amount of perfluoroalkyl groups are obtained on the surface, which has hydrophobic properties. At the same time, there are silver nanoparticles in the SR-PDA-Ag-HFPT coating, so the coating has dual properties of antibacterial and anti-adhesion.
[0017] In summary, the present invention provides a novel method for preparing an antibacterial and anti-adhesion coating based on a silicone rubber surface. The coating has a broad-spectrum antibacterial property and strong hydrophobicity, and can effectively resist bacterial adhesion. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 XPS graphs of the SR-PDA-Ag-HFPT coating of Example 1 and other coatings;
[0019] Figure 2 The water contact angle diagram of the SR-PDA-Ag-HFPT coating of Example 1 and other coatings;
[0020] Figure 3 This is a graph showing the antibacterial rate of the SR-PDA-Ag-HFPT coating of Example 2 against different concentrations of Escherichia coli;
[0021] Figure 4 This is a graph showing the antibacterial rate of the SR-PDA-Ag-HFPT coating of Example 2 against Staphylococcus aureus at different concentrations;
[0022] Figure 5 This is a statistical diagram of the number of bacteria adhering to the SR-PDA-Ag-HFPT coating and the SR surface in Example 2;
[0023] Figure 6 This is a colony image of bacteria adhering to the SR-PDA-Ag-HFPT coating of Example 2 and the SR surface. DETAILED DESCRIPTION
[0024] Example 1
[0025] Preparation of SR-PDA-Ag-HFPT:
[0026] The preparation method of SR-PDA-Ag-HFPT includes three steps:
[0027] (1) Preparation of SR-PDA: The silicone rubber sheet was cut into 1 cm × 1 cm pieces, and then thoroughly cleaned in acetone and ethanol by ultrasonic for 5 min, and then vacuum dried for use. The dried SR was immersed in 10 mL of the prepared dopamine solution (4 mg / mL, in 10 mM Tris buffer, pH = 8.5) for 72 h, then the SR was taken out, rinsed with a large amount of deionized water to remove the free dopamine on the surface, and dried in a vacuum drying oven at 50 ° C for 12 h to obtain the coated SR-PDA.
[0028] (2) Preparation of SR-PDA-Ag: The SR-PDA prepared in the previous step was immersed in 10 mL of 40-60 mM AgNO3 at room temperature and in the dark. After standing for 24 h, the sample was washed with a large amount of ethanol and deionized water to remove the residual AgNO3 solution on the surface. After vacuum drying for 4 h, the silver nanoparticle coating SR-PDA-Ag was obtained.
[0029] (3) Preparation of SR-PDA-Ag-HFPT: Immerse SR-PDA-Ag in a prepared 10 mL dopamine solution (4 mg / mL, in 10 mM Tris buffer, pH = 8.5) and let it stand for 4 to 8 hours, and continue to deposit PDA on the surface. After the reaction is completed, rinse the surface with a large amount of deionized water and vacuum dry. Place the dried sample in a 25 mL round-bottom flask, add 5 to 10 mL HFPT and 5 to 10 μL triethylamine, and react at 50 to 70 ° C for 6 to 8 hours. After the reaction is completed, rinse with HFPT and deionized water three times respectively, and cure at 110 ° C for 1 hour to obtain the antibacterial and anti-adhesion coating SR-PDA-Ag-HFPT.
[0030] Characterization of individual coatings:
[0031] The coatings SR, SR-PDA, SR-PDA-Ag, and SR-PDA-Ag-HFPT were characterized by XPS. Figure 1 In the figure, SR-PDA-Ag-HFPT shows characteristic peaks of N 1s, Ag 3d and F 1s elements compared with other coatings, indicating that HFPT is successfully grafted on the surface. At the same time, the water contact angle of each coating is characterized. Figure 2 The contact angles of SR, SR-PDA, and SR-PDA-Ag are 109°, 63°, and 79°, respectively. HFPT is grafted onto the surface of SR-PDA-Ag-HFPT to obtain a fluorine-containing hydrophobic coating with a water contact angle of 125°.
[0032] Example 2
[0033] Antimicrobial Testing:
[0034] The frozen Escherichia coli (E. coli) and Staphylococcus aureus (S. aureus) were incubated with fresh culture medium (TSB) in a 37°C incubator for 24 h. After centrifugation at 3000 r / min for 10 min, the supernatant was replaced with sterile PBS and the bacterial suspension was diluted to 1×10 6 CFU / mL, 1×10 7 CFU / mL, 1×10 8 CFU / mL (the density of the bacterial suspension was determined by an ultraviolet spectrophotometer). The prepared SR, SR-PDA, and SR-PDA-Ag-HFPT were subjected to antibacterial tests, and all samples were sterilized under ultraviolet light for 1 hour. A 1cm×1cm SR sample was placed in a culture dish, 20μL of bacterial solution was dropped on the SR sample, and then a sterile 0.8×0.8cm PE sheet was covered on the surface. At the same time, a bottle cap filled with sterile saline was placed in the culture dish to maintain the humidity of the culture environment. After the culture dish was cultured in a constant temperature (37°C) incubator for 1 hour, each SR sample was placed in a PE tube filled with 2mL of saline, and ultrasonicated for 3 minutes to separate the attached bacteria, and 50μL of bacterial solution was taken for coating. The inhibition rate was calculated by the agar plate counting method, that is, the attached bacteria. Figure 3 , 4 .
[0035] The concentration of SR-PDA-Ag-HFPT on E.coli was 1×10 6 CFU / mL, 1×10 7 CFU / mL, 1×10 8 The inhibition rates of SR-PDA-Ag-HFPT against 1×10 6 CFU / mL of E. coli had a good antibacterial effect, with an inhibition rate of 99.9%, while for 1×10 6 CFU / mL of S. aureus was slightly less effective, with an inhibition rate of 90%. For high-concentration bacterial solutions, the antibacterial effects of SR-PDA-Ag-HFPT on E. coli and S. aureus were not ideal. However, SR-PDA-Ag-HFPT still had an antibacterial effect on 1×10 6 The bacteria with CFU / mL have a good antibacterial rate, indicating that the coating prepared by the present invention still has a good antibacterial effect.
[0036] Anti-adhesion test:
[0037] Sterilize SR and SR-PDA-Ag-HFPT under UV light for 1 h and place them in a sterilized 24-well plate. Add 900 μL of fresh TSB to the 24-well plate and 100 μL of diluted bacterial solution (1×10 6 CFU / mL), and the samples were taken out after culturing in a constant temperature (37°C) incubator for 24 hours. Each sample surface was rinsed three times with sterile PBS and carefully placed in a PE tube filled with 2mL of saline. The PE tube was ultrasonicated for 3 minutes to separate the adhered bacteria from the sample surface. After diluting the bacterial suspension 10 times, 50μL of the bacterial solution was taken for coating, and the culture dish was cultured in a constant temperature (37°C) incubator. After the culture was completed, the colonies were counted and the anti-adhesion ability was evaluated, that is, the adhesion Figure 5 , 6 .
[0038] The surface bacterial density of SR-PDA-Ag-HFPT after 24 hours of interaction with E. coli and S. aureus was 7.2×10 4 CFU / cm 2 , 2.1×10 5 CFU / cm 2 However, the density of bacteria adhered to it was significantly lower than that of SR by 1-2 orders of magnitude, and it still had a certain degree of anti-adhesion. At the same time, the colony images of SR-PDA-Ag-HFPT and E. coli and S. aureus bacterial solutions also showed that there were only a few bacteria on the surface of SR-PDA-Ag-HFPT coating.
[0039] The above results show that the SR-PDA-Ag-HFPT coating prepared in the present invention has the dual properties of antibacterial and anti-adhesion through the synergistic effect of silver nanoparticles and HFPT, and can effectively inhibit bacterial adhesion within 24 hours of action with bacterial solution.
Claims
1. A method for preparing an antibacterial and anti-adhesion coating based on a silicone rubber surface, characterized in that The prepared coating has antibacterial and anti-adhesion capabilities, wherein the antibacterial capability is due to the silver nanoparticles generated in situ by the catechol groups on the PDA coating, and the anti-adhesion capability is due to the HFPT grafted on the surface of the silicone rubber by a nucleophilic substitution reaction.
2. The method for preparing the antibacterial and anti-adhesion coating on the surface of silicone rubber according to claim 1, characterized in that Follow these steps: (1) Depositing PDA on the surface of silicone rubber to obtain a coating SR-PDA; (2) reacting the SR-PDA coating prepared in step (1) with a certain concentration of silver nitrate to in situ generate silver nanoparticles to obtain a coating SR-PDA-Ag; (3) PDA is further deposited on the SR-PDA-Ag coating prepared in step (2), and then heated and reacted with HFPT in the presence of a trace amount of triethylamine to obtain a coating SR-PDA-Ag-HFPT.
3. The method for preparing the antibacterial and anti-adhesion coating on the surface of silicone rubber according to claim 2, characterized in that: The concentration of silver nitrate in step (2) is 40-60 mM.
4. The method for preparing the antibacterial and anti-adhesion coating on the surface of silicone rubber according to claim 2, characterized in that: In step (3), the volume ratio of triethylamine to HFPT is 1:1000, and the reaction heating temperature is 50-70°C.
5. Use of the antibacterial and anti-adhesion coating on the surface of silicone rubber according to claim 2 in antibacterial and anti-adhesion experiments.