Urine-wet color-changing thermoplastic film as well as preparation method and application thereof
By using wet urinary discolored thermoplastic film in disposable absorbent products, combined with surfactant and water-soluble toner, the problem of insolid adhesion of color indicators and incomplete discoloration is solved, and more accurate judgment of absorption conditions and higher adhesion stability.
Patent Information
- Application Number
- CN202411128900.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-22
AI Technical Summary
The color indicators of existing disposable absorbent products do not adhere firmly during use, resulting in inaccurate judgment of absorption, and poor coordination between hydrophilic ink and water-repellent base film, affecting the color discoloration effect.
Urinary wet color discoloration thermoplastic film is used to add surfactant and water-soluble toner of suitable particle size to the base film, combined with water-based acrylic resin of appropriate molecular weight to form a color-developing layer and a vanishing layer to improve the adhesion stability of the color-changing layer. and discoloration thoroughly, and the hydrophilicity and temperature stability of the base film are enhanced by a second surfactant.
The adhesion stability and color discoloration effect of the color change layer are significantly improved, the user's accuracy in judging the absorption situation, and at the same time, the production cost and the emergence of opaque areas during the stretching of the base film are reduced.
Smart Images

Figure CN118994686A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of waterproof thermoplastic films, in particular to a urine-discoloring thermoplastic film and a preparation method and application thereof. Background Art
[0002] It is difficult for users or caregivers of disposable absorbent products to judge the use of disposable absorbent products during use, and it is also difficult to confirm whether the absorbent core in the disposable absorbent products is in a state of absorption saturation in a timely manner. In order for users to use health care products more effectively, a means should be designed to convey the use, relative level or degree of disposable absorbent products to users or caregivers during the use of disposable absorbent products, such as a color indicator that causes the product to change color.
[0003] In the prior art, a color indicator is often coated on the surface of a base film to form a color-changing area to prepare disposable absorbent products; when in use, the color-changing layer on one side of the base film coated with the color indicator comes into contact with the liquid, thereby causing a color change, and the use of the disposable absorbent product is judged by the color change effect.
[0004] At present, the commonly used color indicators are generally combined with hydrophilic ink to form a hydrophilic slurry coated on the surface of the base film. However, the base film of disposable absorbent products has strong water repellency. In actual use, it will also cause the liquid to be unable to spread to the location of the color indicator in time after contacting the base film, so that the color indicator coating area is not completely discolored (or disappears), reducing the accuracy of users in judging the use of disposable absorbent products; in addition, the color indicator is generally combined with hydrophilic ink to form a hydrophilic slurry, which has poor spreading performance on the surface of the water-repellent base film, and the adhesion between the base film and the base film after molding is poor. The disposable absorbent products currently on the market cannot solve the above problems well. Summary of the invention
[0005] In order to improve the adhesion stability between the color-changing layer and the base film in disposable absorbent products and the thoroughness of the water absorption and color-changing process, the present application provides a urine-wetting color-changing thermoplastic film and a preparation method and application thereof.
[0006] In a first aspect, the present application provides a urine-discoloring thermoplastic film, which adopts the following technical solution:
[0007] A urine-wetting color-changing thermoplastic film, comprising a base film and a color-changing layer disposed on the base film, wherein the color-changing layer comprises a color-developing layer close to the base film and a disappearing layer away from the base film;
[0008] The base film includes a surfactant, and the mass proportion of the surfactant in the base film is 0.1%-5%; the surfactant includes a first surfactant and a second surfactant;
[0009] Wherein, the first surfactant comprises at least one of polyols, polyol fatty acids, alkanolamides, and polyethylene oxide additives; the second surfactant comprises at least one of polyethylene oxide-polypropylene oxide block copolymers, polyoxypropylene-polyoxyethylene block copolymers, and siloxane block polyethers;
[0010] The disappearing layer is formed by drying the aqueous slurry, and the aqueous slurry comprises the following raw materials by weight percentage: 10%-70% of aqueous acrylic resin and 1%-30% of water-soluble color powder;
[0011] The particle size of the water-soluble color powder is 0.02-2 μm; the molecular weight of the water-based acrylic resin is 200-5000 Da, and the water-based acrylic resin includes at least one of polyacrylic acid, polybutyl acrylate and modified products thereof.
[0012] Preferably, the aqueous slurry further comprises the following raw materials in terms of weight percentage: 20%-40% water, 0.1%-1% leveling agent, and 0.1%-1% auxiliary agent; the auxiliary agent includes an antibacterial agent and a bactericide.
[0013] The disappearing layer is in contact with the color-developing layer on the surface of the base film of the present invention. Since the color-developing layer is water-repellent, when the disappearing layer contacts water, the speed at which the disappearing layer dissolves and changes color when it comes into contact with water will be affected. In addition, since the base film itself is water-repellent, when water acts on the base film, the water cannot be quickly transferred from the surface of the base film to the disappearing layer, which is not conducive to the complete disappearance of the disappearing layer when it comes into contact with water, and will affect the color-changing effect of the thermoplastic film when it comes into contact with water.
[0014] First, the present invention selects a water-soluble color powder with a suitable particle size and a water-based acrylic resin with a suitable molecular weight. The water-based acrylic resin with the above molecular weight has a molecular chain segment of a suitable length. The water-based acrylic resin can act on the surface of the single water-soluble color powder particles to avoid agglomeration of the water-soluble color powder, and greatly improve the dispersion uniformity of the water-soluble color powder in the vanishing layer, thereby increasing the color change speed of the vanishing layer after contacting water and improving the significance of the color change effect of the thermoplastic film.
[0015] Second, in the present invention, a surfactant is added to the base film. The introduction of the surfactant can improve the hydrophilicity of the base film, and help water to quickly spread from the surface of the base film to the vanishing layer, thereby further improving the thoroughness of the discoloration of the vanishing layer when it comes into contact with water; and the first surfactant is combined with the second surfactant. The combined use of the two can also reduce the proportion of the surfactant used in the base film and reduce the production cost of the base film.
[0016] Third, since the first surfactant will become turbid at a certain temperature, as the temperature rises during the preparation of the base film, dot-shaped opaque areas will appear on the surface of the base film, which will reduce the user's observation clarity of the color change layer on the base film; and in the present invention, by selecting a second surfactant to match it, on the one hand, the second surfactant can form micelles in the system and increase the intermolecular forces in the surfactant system; on the other hand, the hydroxyl groups in the second surfactant can react with the ether groups in the first surfactant to form hydrogen bonds, further increasing the intermolecular forces in the surfactant system, thereby improving the temperature stability of the surfactant system, so that the base film always maintains a relatively uniform transparent state during the preparation process.
[0017] Fourth, the present invention uses a surfactant to cooperate. Although the hydrophilicity of the base film surface is improved at this time, it does not affect the spreading performance of the color developing layer ink (hydrophobic) on the base film surface. This is because the hydrophobic segments in the second surfactant, such as propylene oxide segments, polyoxypropylene segments, and silicone segments, can adjust the hydrophilic-lipophilic balance value of the surfactant, and have a certain adsorption capacity for the hydrophobic ink that forms the color developing layer, which helps to improve the spreading performance of the ink that forms the color developing layer on the base film surface, and helps to improve the adhesion strength between the disappearing layer and the base film surface.
[0018] Fifth, by using the above second surfactant in the present invention, a cross-linked three-dimensional network structure can be generated in the base film, which helps to improve the flexibility of the base film and improve the comfort level when the base film contacts the user without reducing the firmness of the base film.
[0019] In summary, the present invention uses the above-mentioned surfactant in combination with a water-soluble color powder of suitable particle size, an aqueous acrylic resin of suitable molecular weight and a surfactant, which improves the thoroughness of dissolution of the disappearing layer, improves the adhesion stability between the color developing layer and the base film, and helps to obtain a base film with uniform transparency.
[0020] Preferably, in the first surfactant, the polyol includes at least one of polyvinyl alcohol and its modified products, polypropylene glycol and its modified products, polytetramethylene glycol and its modified products, and polyether polyols; the polyol fatty acid includes at least one of glyceryl stearate, polyethylene glycol stearate, and polyglycerol stearate; the alkanolamides include at least one of alkyl alcohol amides and polyoxyethylene alkanolamides; the polyethylene oxide additive includes at least one of polyoxyethylene ether and its modified products, and fatty alcohol polyoxyethylene ether.
[0021] By selecting the above-mentioned first surfactant and second surfactant in combination, not only the hydrophilicity of the base film can be improved, but also the spreading performance of the oily color-developing layer on the surface of the base film will not be affected, which helps to improve the adhesion between the color-changing layer and the base film, and can also form a stable three-dimensional network structure in the base film to improve the flexibility of the base film.
[0022] Preferably, the mass ratio of the first surfactant to the second surfactant is 5:0.5-2.
[0023] By controlling the dosage ratio of the first surfactant to the second surfactant, the hydrophilicity of the base film is improved while maintaining a high degree of transparency and uniformity, and the improvement in the hydrophilicity of the base film does not affect the spreading performance of the color-developing layer ink on the surface of the base film and the adhesion strength between the color-developing layer and the base film, thereby obtaining a thermoplastic film with excellent comprehensive performance.
[0024] Preferably, the ratio of the thickness of the color-changing layer to the thickness of the base film is 0.01-1:8-25.
[0025] In the actual use of thermoplastic film, the color-changing layer is in direct contact with water, and the user needs to observe the color change process of the color layer before and after it comes into contact with water through the base film; and the base film needs to be stretched during the molding process, which will cause disconnected microporous structures to appear in the base film, and the presence of micropores will affect the propagation of light, making the base film appear whitish, which will affect the user's observation of the color change effect of the color-changing layer before and after it comes into contact with water to a certain extent. When the appropriate thickness of the color-changing layer and the appropriate thickness of the base film are set, the influence of the base film whiteness on the observation effect of the color change is weakened, and the significance of the color change measurement is improved.
[0026] Preferably, the ratio of the thickness of the color development layer to the thickness of the disappearing layer is 1:20-20:1.
[0027] Preferably, the ratio of the thickness of the color development layer to the thickness of the disappearing layer is 1:8-12:1.
[0028] The present invention controls the thickness of the disappearing layer and the thickness of the display layer to be within a reasonable range, which helps to observe with the naked eye the change in the superimposed color effect of the disappearing layer and the display layer before and after the disappearing layer meets water; and when the thickness of the disappearing layer is kept within the above range, it can be dissolved relatively quickly to produce a color change, and work together with the color development layer to completely change the color of the color change layer, thereby improving the user's intuitiveness in observing the color change of the color change layer before and after it meets water.
[0029] Preferably, the base film comprises inorganic powder, and the mass proportion of the inorganic powder in the base film is 3%-65%.
[0030] Preferably, the base film comprises inorganic powder, and the mass proportion of the inorganic powder in the base film is 15%-35%.
[0031] Preferably, the base film further comprises polyolefin.
[0032] Preferably, the particle size of the inorganic powder is 0.3-5 μm; the inorganic powder includes at least one of silicon dioxide, glass microspheres, wollastonite powder and modified products thereof.
[0033] The present invention adds inorganic powders of the above-mentioned particle size range to the base film, and the inorganic powders can fill the tiny gaps generated in the base film during the stretching process, thereby changing the reflection path of light, improving the transparency of the base film, and allowing the observer to more intuitively and clearly observe the color change effect of the color change layer before and after it meets water. In addition, the inorganic powder used in the present invention has little effect on the surfactant, and can avoid adsorption of the surfactant to a great extent, so that the surfactant can be evenly dispersed in the base film, so that the base film around the color change layer at different positions of the base film has good hydrophilicity (generally in specific applications, such as diapers, there is not only one color change layer, but multiple color change layers are dispersed on the surface of the base film), improving the consistency of the color change effect of the color change layer at different positions before and after it meets water.
[0034] Preferably, the color development layer includes a waxy substance.
[0035] In a second aspect, the present application provides a method for preparing a urine-discoloring thermoplastic film, which adopts the following technical solution:
[0036] A method for preparing a urine-discoloring thermoplastic film comprises the following steps:
[0037] S1, blending raw materials constituting the base film to obtain plastic particles;
[0038] S2, extruding the plastic particles and subjecting them to steps including preheating, stretching, shaping, and cooling to obtain the base film;
[0039] S3, printing the slurry for forming the color development layer on the surface of the base film, and forming the color development layer after drying; continuing to print the aqueous slurry on the color development layer, and forming the disappearing layer after drying, so as to obtain the urine color-changing thermoplastic film.
[0040] Preferably, in the slurry forming the color development layer, the content of the waxy substance is ≥5%.
[0041] Preferably, in S2, the temperature during preheating is 50-100°C; the temperature during stretching is 60-100°C, and the stretching ratio is 1-10 times; the temperature during shaping is 60-120°C; and the temperature during cooling is 10-80°C.
[0042] In a third aspect, the present application provides an application of a urine-discoloring thermoplastic film in a disposable absorbent product, using the following technical solution:
[0043] The invention discloses an application of a thermoplastic film that changes color when urine is wet in disposable absorbent products.
[0044] Preferably, the disposable absorbent products include diapers, diapers, diaper pads and the like. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 It is a schematic structural diagram of the urine-wetting color-changing thermoplastic film of the present invention.
[0046] Explanation of the reference numerals: 1. urine-discoloring thermoplastic film; 2. base film; 3. color-changing layer; 31. color-developing layer; 32. disappearing layer. DETAILED DESCRIPTION
[0047] For better understanding and implementation, the technical solution of the present invention will be clearly and completely described below in conjunction with embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments.
[0048] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0049] Unless otherwise indicated, all numerical values expressing quantities of ingredients, reaction conditions, and so forth used in the specification and claims are to be understood as modified by the term “about.” Accordingly, unless indicated to the contrary, the numerical parameters set forth herein are approximations that can vary depending upon the desired properties desired to be obtained.
[0050] As used herein, "and / or" means one or all of the mentioned elements.
[0051] As used herein, “including” and “comprising” encompasses the case where only the stated elements are present as well as the case where there are other elements other than the stated elements.
[0052] All percentages in the present invention are by weight, unless otherwise specified.
[0053] Unless otherwise indicated, "a", "an", "an" and "the" used in this specification are intended to include "at least one" or "one or more". For example, "a component" means one or more components, so more than one component may be considered and may be employed or used in the implementation of the embodiment.
[0054] Example 1
[0055] A urine-discoloring thermoplastic film comprises a base film and a color-changing layer arranged on the base film, wherein the color-changing layer comprises a color-developing layer close to the base film and a disappearing layer far from the base film; the thickness ratio of the color-changing layer to the base film is 0.01:20, and the thickness ratio of the color-developing layer to the disappearing layer is 1:10.
[0056] The base film comprises the following raw materials by weight percentage: 94% of polyolefin, 3% of surfactant (polyol and polyethylene oxide-polypropylene oxide block copolymer in a mass ratio of 5:0.5), 0.3% of antioxidant, and 2.7% of desiccant;
[0057] The color developing layer is obtained by drying the color developing slurry, and the color developing slurry is a solvent-based ink;
[0058] The disappearing layer is obtained by drying the aqueous slurry, and the aqueous slurry includes the following raw materials by weight: 60% of water polyacrylic acid (molecular weight of 500Da), 9% of water-soluble color powder (particle size of 0.05μm), 30% of water, 0.5% of leveling agent, and 0.5% of antibacterial agent;
[0059] A urine-discoloring thermoplastic film is prepared by the following steps:
[0060] S1, blending raw materials constituting the base film to obtain plastic particles;
[0061] S2, extruding the plastic particles, preheating and stretching at 100° C. (stretching ratio is 2 times), shaping at 120° C., and cooling at 30° C. to obtain a base film;
[0062] S3, printing the slurry for forming the color developing layer on the surface of the above-mentioned base film, and forming the color developing layer after drying; continuing to print the water-based slurry on the color developing layer, and forming the disappearing layer after drying, so as to obtain the urine-wetting color-changing thermoplastic film.
[0063] Specifically, the urine-displaying color-changing process of the urine-displaying color-changing thermoplastic film of this embodiment is as follows: before urine-displaying, the disappearing layer is yellow, the color-developing layer is blue, and the visual pattern effect presented by the superposition of yellow and blue of the disappearing layer and the color-developing layer is green; after urine-displaying, the water-soluble color powder in the disappearing layer comes into contact with urine and is dissolved by the water in urine, and the yellow element gradually disappears as the urine diffuses, leaving only the blue color of the color-developing layer, that is, the color change before and after urine-displaying is from green to blue, which visually produces a color-changing effect and serves as a reminder for replacement.
[0064] Example 2
[0065] A urine-discoloring thermoplastic film comprises a base film and a color-changing layer arranged on the base film, wherein the color-changing layer comprises a color-developing layer close to the base film and a disappearing layer far from the base film; the thickness ratio of the color-changing layer to the base film is 0.5:25, and the thickness ratio of the color-developing layer to the disappearing layer is 1:20.
[0066] The base film comprises the following raw materials by weight percentage: 95% of polyolefin, 4% of surfactant (polyol fatty acid and polyoxypropylene-polyoxyethylene block copolymer in a mass ratio of 5:2), 0.5% of antioxidant, and 0.5% of desiccant;
[0067] The color developing layer is obtained by drying the color developing slurry, and the color developing slurry is a solvent-based ink;
[0068] The disappearing layer is obtained by drying the aqueous slurry, and the aqueous slurry includes the following raw materials by weight: 40% of polybutyl acrylate (molecular weight of 1000Da), 28% of water-soluble color powder (particle size of 0.08μm), 30% of water, 1% of leveling agent, and 1% of antibacterial agent;
[0069] A urine-discoloring thermoplastic film is prepared by the following steps:
[0070] S1, blending raw materials constituting the base film to obtain plastic particles;
[0071] S2, after extruding the plastic particles, preheating and stretching at 50° C. (stretching ratio is 3 times), shaping at 60° C., and cooling at 10° C. to obtain a base film;
[0072] S3, printing the slurry for forming the color developing layer on the surface of the above-mentioned base film, and forming the color developing layer after drying; continuing to print the water-based slurry on the color developing layer, and forming the disappearing layer after drying, so as to obtain the urine-wetting color-changing thermoplastic film.
[0073] The urine-displaying color-changing process of the urine-displaying color-changing thermoplastic film of this embodiment is as follows: before urine-displaying, the vanishing layer is red, the color-developing layer is blue, and the visual pattern effect presented by the superposition of red and blue of the vanishing layer and the color-developing layer is purple; after urine-displaying, the water-soluble color powder in the vanishing layer comes into contact with urine and is dissolved by the water in urine, and the red element gradually disappears as the urine diffuses, leaving only the blue color of the color-developing layer, that is, the color change before and after urine-displaying is from purple to blue, which visually produces a color-changing effect and serves as a reminder for replacement.
[0074] Example 3
[0075] A urine-discoloring thermoplastic film comprises a base film and a color-changing layer arranged on the base film, wherein the color-changing layer comprises a color-developing layer close to the base film and a disappearing layer far from the base film; the thickness ratio of the color-changing layer to the base film is 1:15, and the thickness ratio of the color-developing layer to the disappearing layer is 1:12.
[0076] The base film comprises the following raw materials by weight percentage: 94% of polyolefin, 1% of surfactant (alkanolamide and siloxane block polyether in a mass ratio of 5:1), 0.1% of antioxidant, and 4.9% of desiccant;
[0077] The color developing layer is obtained by drying the color developing slurry, and the color developing slurry is a solvent-based ink;
[0078] The disappearing layer is obtained by drying the aqueous slurry, and the aqueous slurry includes the following raw materials by weight: 54% polyacrylic acid (molecular weight 3000Da), 15.5% water-soluble color powder (particle size 1 μm), 30.3% water, 0.1% leveling agent, and 0.1% antibacterial agent;
[0079] A urine-discoloring thermoplastic film is prepared by the following steps:
[0080] S1, blending raw materials constituting the base film to obtain plastic particles;
[0081] S2, after extruding the plastic particles, preheating and stretching at 90° C. (stretching ratio is 8 times), shaping at 60° C., and cooling at 30° C. to obtain a base film;
[0082] S3, printing the slurry for forming the color developing layer on the surface of the above-mentioned base film, and forming the color developing layer after drying; continuing to print the water-based slurry on the color developing layer, and forming the disappearing layer after drying, so as to obtain the urine-wetting color-changing thermoplastic film.
[0083] The urine discoloration process of the urine-discoloring thermoplastic film of this embodiment is as follows: before urine, the vanishing layer is yellow and the color-developing layer is red, and the visual pattern effect presented by the superposition of yellow and red of the vanishing layer and the color-developing layer is orange; after urine, the water-soluble color powder in the vanishing layer comes into contact with urine and is dissolved by the water in urine, and the yellow element gradually disappears as the urine diffuses, leaving only the red color of the color-developing layer, that is, the color change before and after urine is from orange to red, which visually produces a color change effect and serves as a reminder for replacement.
[0084] Example 4
[0085] A urine-wetting color-changing thermoplastic film comprises a base film and a color-changing layer arranged on the base film, wherein the color-changing layer comprises a color-developing layer close to the base film and a disappearing layer far from the base film; the thickness ratio of the color-changing layer to the base film is 1:20, and the thickness ratio of the color-developing layer to the disappearing layer is 8:1.
[0086] The base film comprises the following raw materials by weight percentage: 92% of polyolefin, 5% of surfactant (polyethylene oxide additive and polyethylene oxide-polypropylene oxide block copolymer in a mass ratio of 5:1.5), 0.5% of antioxidant, and 2.5% of desiccant;
[0087] The color developing layer is obtained by drying the color developing slurry, and the color developing slurry is a solvent-based ink;
[0088] The disappearing layer is obtained by drying the aqueous slurry, and the aqueous slurry includes the following raw materials by weight: 50% of water-soluble butyl acrylate (molecular weight of 5000a), 15% of water-soluble color powder (particle size of 2 μm), 34% of water, 0.3% of leveling agent, and 0.7% of antibacterial agent;
[0089] A urine-discoloring thermoplastic film is prepared by the following steps:
[0090] S1, blending raw materials constituting the base film to obtain plastic particles;
[0091] S2, after extruding the plastic particles, preheating and stretching at 80° C. (stretching ratio is 7 times), shaping at 90° C., and cooling at 20° C. to obtain a base film;
[0092] S3, printing the slurry for forming the color developing layer on the surface of the above-mentioned base film, and forming the color developing layer after drying; continuing to print the water-based slurry on the color developing layer, and forming the disappearing layer after drying, so as to obtain the urine-wetting color-changing thermoplastic film.
[0093] Specifically, the urine-displaying color-changing process of the urine-displaying color-changing thermoplastic film of this embodiment is as follows: before urine-displaying, the disappearing layer is yellow, the color-developing layer is blue, and the visual pattern effect presented by the superposition of yellow and blue of the disappearing layer and the color-developing layer is green; after urine-displaying, the water-soluble color powder in the disappearing layer comes into contact with urine and is dissolved by the water in urine, and the yellow element gradually disappears as the urine diffuses, leaving only the blue color of the color-developing layer, that is, the color change before and after urine-displaying is from green to blue, which visually produces a color-changing effect and serves as a reminder for replacement.
[0094] Example 5
[0095] The difference between this embodiment and embodiment 1 is that the mass ratio of the first surfactant to the second surfactant is 10:2; the other steps and condition settings are consistent with those in embodiment 1.
[0096] Example 6
[0097] The difference between this embodiment and embodiment 1 is that the mass ratio of the first surfactant to the second surfactant is 5:0.1; the other steps and condition settings are consistent with those in embodiment 1.
[0098] Example 7
[0099] The difference between this embodiment and embodiment 1 is that, when the thickness of the color-changing layer is consistent with the thickness of the color-changing layer in embodiment 1, the ratio of the thickness of the color-changing layer to the base film in this embodiment is 0.5:30;
[0100] The other steps and conditions are the same as those in Example 1.
[0101] Example 8
[0102] The difference between this embodiment and embodiment 1 is that, when the thickness of the color developing layer is consistent with the thickness of the color developing layer in embodiment 1, the ratio of the thickness of the color developing layer to the thickness of the disappearing layer in this embodiment is 30:1;
[0103] The other steps and conditions are the same as those in Example 1.
[0104] Example 9
[0105] The difference between this embodiment and embodiment 1 is that, when the thickness of the color developing layer is consistent with the thickness of the color developing layer in embodiment 1, the ratio of the thickness of the color developing layer to the thickness of the disappearing layer in this embodiment is 1:30;
[0106] The other steps and conditions are the same as those in Example 1.
[0107] Example 10
[0108] The difference between this embodiment and embodiment 1 is that the base film includes the following raw materials by weight percentage: 34% of inorganic powder (glass beads with a particle size of 0.3-5 μm), 60% of polyolefin, 4% of surfactant, 0.3% of antioxidant, and 2.7% of desiccant; the content of wax in the color slurry forming the color development layer is 5%;
[0109] The other steps and conditions are the same as those in Example 1.
[0110] Embodiment 11
[0111] The difference between this embodiment and embodiment 1 is that the base film includes the following raw materials by weight percentage: 5% of inorganic powder (silicon dioxide with a particle size of 0.3-5 μm), 91.5% of polyolefin, 0.5% of surfactant, 0.3% of antioxidant, and 2.7% of desiccant; the content of wax in the color slurry forming the color development layer is 10%;
[0112] The other steps and conditions are the same as those in Example 1.
[0113] Example 12
[0114] The difference between this embodiment and embodiment 8 is that the base film includes the following raw materials by weight percentage: 34% of inorganic powder (glass beads with a particle size of 5-7 μm), 60% of polyolefin, 4% of surfactant, 0.3% of antioxidant, and 2.7% of desiccant; the content of wax in the color slurry forming the color development layer is 8%;
[0115] The other steps and conditions are the same as those in Example 1.
[0116] Embodiment 13
[0117] The difference between this embodiment and embodiment 1 is that the urine-discoloring thermoplastic film is prepared by the following steps:
[0118] A urine-discoloring thermoplastic film is prepared by the following steps:
[0119] S1, blending raw materials constituting the base film to obtain plastic particles;
[0120] S2, extruding the plastic particles, preheating and stretching at 150° C. (stretching ratio is 15 times), shaping at 100° C., and cooling at 5° C. to obtain a base film;
[0121] S3, printing the slurry for forming the color developing layer on the surface of the above-mentioned base film, and forming the color developing layer after drying; continuing to print the water-based slurry on the color developing layer, and forming the disappearing layer after drying, so as to obtain the urine-wetting color-changing thermoplastic film.
[0122] The other steps and conditions are the same as those in Example 1.
[0123] Comparative Example 1
[0124] The difference between this comparative example and Example 1 is that an equal weight of polyolefin is used to replace the surfactant in Example 1;
[0125] The other steps and conditions are the same as those in Example 1.
[0126] Comparative Example 2
[0127] The difference between this comparative example and Example 1 is that an equal weight of polyol is used to replace the polyethylene oxide-polypropylene oxide block copolymer in Example 1;
[0128] The other steps and conditions are the same as those in Example 1.
[0129] Comparative Example 3
[0130] The difference between this comparative example and Example 1 is that an equal weight of water-soluble polyurethane with a molecular weight of 10000 Da is used to replace the water-based acrylic resin in Example 1;
[0131] The other steps and conditions are the same as those in Example 1.
[0132] Comparative Example 4
[0133] The difference between this comparative example and Example 1 is that the water-soluble toner in Example 1 is replaced by an equal weight of a particle size of 5-7 μm;
[0134] The other steps and conditions are the same as those in Example 1.
[0135] Test Method
[0136] 1. Test method for the disappearance time of the vanishing layer
[0137] The disappearance time of the disappearing layer on the thermoplastic film in the above-mentioned embodiment and comparative example was tested, and the specific test steps were as follows:
[0138] (1) Using the thermoplastic film in diapers;
[0139] (2) Add 250 ml of saline to the diaper core;
[0140] (3) Immediately after adding the saline solution, a 3.5 kg weight was placed on the diaper core and the sample was placed on a transparent glass table. The color change of the urine display pattern of the diaper could be observed from under the table.
[0141] (4) While placing the weight, press the stopwatch to start recording the time;
[0142] (5) Observe the process of the vanishing layer diffusing from the pattern and being absorbed by the core, and record the time when the vanishing layer completely separates from the pattern to reveal the color of the non-vanishing layer, which is the vanishing time of the vanishing layer. The test results are recorded in Table 1.
[0143] 2. Opacity Test
[0144] The opacity of the thermoplastic films in the above examples and comparative examples was tested using a Hunter ColorFlex EZ spectrophotometer. The test results are recorded in Table 1.
[0145] 3. Adhesion Test
[0146] The adhesion test between the color change layer and the base film is carried out using the following steps:
[0147] (1) Pull open the test tape (3M#600) and stick it on the surface of the base film of the printed color-changing layer of the above-mentioned embodiment and comparative example to be tested, and press back and forth on the sticking place ten times to remove bubbles;
[0148] (2) Tear up one end of the test tape a little to make it enough to grip one end of the test tape, and then quickly pull off the tape at an angle of about 90° relative to the base film (the time from applying to tearing off the test tape must be less than one minute);
[0149] (3) Visually inspect whether the adhesive surface of the test tape is clean and transparent, and confirm the area where the color-changing layer has fallen off;
[0150] (4) Calculate the residual rate of the color-changing layer on the surface of the base film and record the calculation results in Table 1.
[0151] Table 1
[0152]
[0153]
[0154] In combination with Examples 1-6, Comparative Examples 1-4 and Table 1, it can be seen that the present invention, by selecting water-soluble color powder with suitable particle size and water-based acrylic resin with suitable molecular weight, helps to improve the uniformity of dispersion of water-soluble color powder in the vanishing layer and improve the thoroughness of dissolution of the vanishing layer in water; further, by selecting suitable types of surfactants, on the one hand, it is possible to improve the hydrophilicity of the base film, increase the speed at which water diffuses from the base film surface to the vanishing layer, and enable water to quickly spread to the position of the vanishing layer, significantly improving the thoroughness of disappearance of the vanishing layer; on the other hand, the addition of the surfactant in the present application forms a three-dimensional network structure in the base film, which not only improves the flexibility of the base film, but also helps to improve the spreading performance of the slurry forming the vanishing layer on the base film surface and the adhesion ability between the vanishing layer and the base film, thereby significantly improving the bonding stability between the base film and the color-changing layer while improving the hydrophilicity of the base film.
[0155] Combining Example 1, Examples 7-9 and Table 1, it can be seen that by setting a suitable thickness of the color-changing layer and adjusting the ratio of the thickness of the disappearing layer to the color-developing layer in the color-changing layer, the observer can intuitively and clearly observe the color change of the color-changing layer before and after absorbing water.
[0156] In combination with Example 1, Examples 10-12 and Table 1, it can be seen that by adding an appropriate proportion of inorganic powder to the base film and controlling the type and particle size of the inorganic powder, on the one hand, the inorganic powder can be overfilled in the tiny gaps formed during the stretching process of the base film, thereby improving the transparency of the base film. On the other hand, the inorganic powder in the present invention has a small adsorption capacity for surfactants and will not adsorb the surfactant around it to affect the function of the surfactant in the base film.
[0157] In combination with Example 1, Example 13 and Table 1, it can be seen that in the thermoplastic film prepared by the method of the present invention, the hydrophilicity of the base film is improved, the water has good spreading performance on the surface of the base film, and the thoroughness of the dissolution of the disappearing layer when it comes into contact with water can be improved. In addition, the adhesion between the base film and the color-changing layer is strong, and the observer can clearly observe the color change of the color-changing layer before and after absorbing water.
[0158] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the protection scope of the present invention. Although the present invention is described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the technical solutions of the present invention can be modified or equivalently replaced, but these modifications or replacements are all within the protection scope of the present invention.
Claims
1. A thermoplastic film that changes color when wet, characterized in that: It includes a base film and a color change layer arranged on the base film, wherein the color change layer includes a color development layer close to the base film and a disappearing layer far from the base film; The base film includes a surfactant, and the mass proportion of the surfactant in the base film is 0.1%-5%; The surfactant comprises a first surfactant and a second surfactant; Wherein, the first surfactant comprises at least one of polyols, polyol fatty acids, alkanolamides, and polyethylene oxide additives; the second surfactant comprises at least one of polyethylene oxide-polypropylene oxide block copolymers, polyoxypropylene-polyoxyethylene block copolymers, and siloxane block polyethers; The disappearing layer is formed by drying the aqueous slurry, and the aqueous slurry comprises the following raw materials by weight percentage: 10%-70% of aqueous acrylic resin and 1%-30% of water-soluble color powder; The particle size of the water-soluble color powder is 0.02-2 μm; the molecular weight of the water-based acrylic resin is 200-5000 Da, and the water-based acrylic resin includes at least one of polyacrylic acid, polybutyl acrylate and polyacrylic acid modification.
2. The urine-discoloring thermoplastic film according to claim 1, characterized in that: In the first surfactant, the polyol includes at least one of polyvinyl alcohol and its modified products, polypropylene glycol and its modified products, polytetramethylene glycol and its modified products, and polyether polyols; the polyol fatty acid includes at least one of glyceryl stearate, polyethylene glycol stearate, and polyglycerol stearate; the alkanolamides include at least one of alkyl alcohol amides and polyoxyethylene alkanolamides; the polyethylene oxide additive includes at least one of polyoxyethylene ether and its modified products, and fatty alcohol polyoxyethylene ether.
3. The urine-discoloring thermoplastic film according to claim 1, characterized in that: The mass ratio of the first surfactant to the second surfactant is 5:0.5-2.
4. The urine-discoloring thermoplastic film according to claim 1, characterized in that: The ratio of the thickness of the color-changing layer to the thickness of the base film is 0.01-1:8-25.
5. The urine-discoloring thermoplastic film according to claim 1, characterized in that: The ratio of the thickness of the color developing layer to the thickness of the disappearing layer is 1:20-20:
1.
6. The urine-discoloring thermoplastic film according to claim 1, characterized in that: The base film includes inorganic powder, and the mass proportion of the inorganic powder in the base film is 3%-65%.
7. The urine-discoloring thermoplastic film according to claim 6, characterized in that: The particle size of the inorganic powder is 0.3-5 μm; the inorganic powder includes at least one of silicon dioxide, glass microspheres, wollastonite powder and modified products thereof.
8. The urine color-changing thermoplastic film according to any one of claims 6 to 7, characterized in that: The color developing layer includes a waxy substance.
9. The method for preparing the urine-discoloring thermoplastic film according to any one of claims 1 to 8, characterized in that: The steps include: S1, blending raw materials constituting the base film to obtain plastic particles; S2, extruding the plastic particles and subjecting them to steps including preheating, stretching, shaping, and cooling to obtain the base film; S3, printing the slurry for forming the color development layer on the surface of the base film, and forming the color development layer after drying; continuing to print the aqueous slurry on the color development layer, and forming the disappearing layer after drying, so as to obtain the urine color-changing thermoplastic film.
10. The method for preparing the urine-discoloring thermoplastic film according to claim 9, characterized in that: In S2, the temperature during the preheating process is 50-100°C; the temperature during the stretching process is 60-100°C, and the stretching ratio is 1-10 times; the temperature during the shaping process is 60-120°C; and the temperature during the cooling process is 10-80°C.
11. Use of the urine-color-changing thermoplastic film according to any one of claims 1 to 8 in disposable absorbent products.