Halloysite / chitosan / polypyrrole composite material and preparation method thereof
The preparation of eloite/chitosan/polypyrrole composite materials by ice template method and vacuum adsorption method was solved, and the problems of low conductivity and poor mechanical properties of existing electromagnetic interference shielding materials were achieved, and high conductivity and excellent electromagnetic shielding were achieved. Performance, suitable for industrial production.
Patent Information
- Application Number
- CN202411209439.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-22
AI Technical Summary
The existing electromagnetic interference shielding materials have problems such as low conductivity, poor mechanical properties, poor corrosion resistance and poor processing, which limits their wide application in the field of electromagnetic shielding.
The elolite/chitosan/polypyrrole composite material was prepared by ice template method and vacuum adsorption method. By adsorbing iron chloride on the surface of the sheet layer of the aerogel through vacuum adsorption, and forming a polypyrrole coating on the surface, forming a surface. Porous skeletons to improve conductivity and electromagnetic shielding performance.
It has achieved lightweight, high conductivity and excellent mechanical properties, good electromagnetic shielding characteristics and corrosion resistance, and is suitable for large-scale industrial production, showing high potential application value in the field of electromagnetic shielding.
Smart Images

Figure CN118994719A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of electromagnetic shielding materials, and in particular relates to the electromagnetic shielding performance and functionalization of a composite aerogel prepared with natural silicate minerals as raw materials. Background Art
[0002] Electromagnetic interference shielding materials play an important role in modern electronic devices. They can effectively reduce the propagation of electromagnetic waves and reduce mutual interference between devices. Although traditional shielding materials, such as conductive metals and ferromagnetic materials, have excellent shielding efficiency, they also have some obvious disadvantages, such as high density, poor processability and easy corrosion. Composite shielding materials with metal coating on the surface generally have problems such as poor wear resistance and scratch resistance.
[0003] In recent years, porous materials such as foams and aerogels have attracted attention due to their unique structural properties. These materials, due to their high specific surface area and low density, can produce strong multiple reflection effects and microwave absorption effects in three-dimensional porous structures, thus showing excellent electromagnetic interference shielding efficiency. However, the common problems of low conductivity and poor mechanical properties of porous materials have seriously restricted their widespread application in the field of electromagnetic shielding materials.
[0004] Therefore, it is urgent to develop a lightweight electromagnetic interference shielding material with high conductivity, excellent mechanical properties, corrosion resistance, good processability and wide absorption bandwidth performance. Summary of the invention
[0005] In view of the common problems in the prior art, the purpose of the present invention is to provide a method for preparing a lightweight electromagnetic interference shielding material that takes into account both electrical conductivity and mechanical strength. The method used in the present invention has a mild reaction, is easy to operate, and has low requirements for equipment and energy consumption; the prepared composite material has a light weight, a low density, and excellent compression strength; and the content of polypyrrole attached to the aerogel is controllable, which has both good electrical conductivity and excellent electromagnetic shielding properties, and the anisotropy shown has high potential application value in the field of electromagnetic shielding.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0007] The invention discloses a method for preparing a halloysite / chitosan / polypyrrole composite material based on an ice template method and a vacuum adsorption method. The method comprises the following steps: dissolving chitosan in acetic acid and mixing the chitosan with halloysite to prepare a halloysite / chitosan mixed solution; injecting the mixed solution into a mold, and obtaining a halloysite / chitosan composite aerogel through bidirectional freezing and freeze drying; vacuum adsorbing the obtained composite aerogel in a glutaraldehyde / ethanol solution, a ferric chloride solution and a pyrrole monomer in sequence, and finally soaking the composite aerogel in a pyrrole monomer, and obtaining the halloysite / chitosan / polypyrrole composite material after drying.
[0008] Specifically, the preparation method comprises:
[0009] 1) preparing a mixed solution of halloysite / chitosan: adding chitosan powder to an acetic acid solution and dispersing until completely dissolved, and adding halloysite powder and dispersing until uniform;
[0010] 2) preparing halloysite / chitosan composite aerogel: injecting the mixed solution obtained in step 1) into a mold, and after bidirectional freezing, placing it in a freeze dryer for freeze drying;
[0011] 3) placing the halloysite / chitosan composite aerogel obtained in step 2) into a suction filtration container, adding a 4% glutaraldehyde / ethanol solution for vacuum adsorption for 2 to 4 hours, and after the adsorption is completed, soaking the sample in the 4% glutaraldehyde / ethanol solution for 6 to 10 hours, pouring out the solution, and drying naturally;
[0012] 4) placing the composite aerogel obtained in step 3) into a suction filtration container, adding ferric chloride solution for vacuum adsorption for 2 to 4 hours, and after the adsorption is completed, soaking the sample in the ferric chloride solution for 6 to 10 hours, pouring out the solution, freezing it in a refrigerator for 18 to 30 hours, and then drying it in a freeze dryer for 18 to 30 hours;
[0013] 5) The composite aerogel obtained in step 4) is placed in a suction filtration container, and is immersed in ice water at 0°C, and pyrrole monomer is added for vacuum adsorption for 2 to 4 hours. After the adsorption is completed, the sample is immersed in pyrrole monomer at 0°C for reaction. After the reaction is completed, the sample is immersed in ethanol / water solution for washing and drying to obtain a chitosan / halloysite / polypyrrole composite material.
[0014] In a preferred embodiment, in step 1), the weight percentage concentration of the acetic acid solution is 4%; preferably, the purity of the halloysite powder is above 90%.
[0015] In a preferred embodiment, in step 1), in step 1), the mass volume ratio of the chitosan powder, the acetic acid solution and the halloysite powder is: (0.18-2.0) g:15 ml:(0.01-1.0) g.
[0016] In a preferred embodiment, in step 1), in order to improve the dispersion effect of chitosan powder and / or halloysite powder, ultrasonic stirring and / or cell crushing can be used for stirring and powdering. For example, chitosan powder is added to acetic acid solution and ultrasonic stirring is performed until it is completely dissolved; after adding halloysite powder, stirring is performed evenly, and then cell crushing is performed for 1 to 3 times. Preferably, the single treatment time is 5 to 10 minutes.
[0017] In a preferred embodiment, in step 2), the volume of the mixed solution in each mold is 6-10 mL, preferably, the volume of the mixed solution in each mold is 8 mL.
[0018] In a preferred embodiment, in step 2), the bidirectional freezing method is an operation method well known in the art, which can be performed in a mold. In a low temperature field, the solvent forms ice crystals as the temperature decreases, and the solute particles are squeezed between the ice crystal columns to form a certain oriented structure. In an embodiment of the present invention, the temperature of the oriented freezing is -200 to -20°C, preferably -180 to -20°C; the cooling rate can be 0.1 to 200°C / min, and further 1 to 100°C / min.
[0019] In a preferred embodiment, in step 2), the freeze-drying is an operation method well known in the art, and the freeze-drying time is 3 to 5 days, preferably, the freeze-drying time is 4 days.
[0020] In a preferred embodiment, in step 3), the mass volume ratio of the composite aerogel used to the 4% glutaraldehyde / ethanol solution is: (0.8-1.5) g: (20-80) ml.
[0021] In a preferred embodiment, in step 3), the vacuum adsorption time in the 4% glutaraldehyde / ethanol solution is 3 hours, and after the adsorption is completed, the sample is immersed in the 4% glutaraldehyde / ethanol solution for 8 hours.
[0022] In the present invention, the halloysite / chitosan composite aerogel is first cross-linked with a glutaraldehyde / ethanol solution to obtain a water-insoluble stable aerogel skeleton.
[0023] In a preferred embodiment, in step 4), the molar concentration of the ferric chloride solution is 0.01 to 3 mol / L; preferably, the molar concentration of the ferric chloride solution is 0.1 mol / L, 0.3 mol / L, 0.5 mol / L, 0.8 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, or 3 mol / L.
[0024] In a preferred embodiment, in step 4), the mass volume ratio of the composite aerogel to the ferric chloride solution is: (0.8-1.5) g: (20-80) ml.
[0025] In a preferred embodiment, in step 4), the vacuum adsorption time in the ferric chloride solution is 3 hours, and after the adsorption is completed, the sample is immersed in the ferric chloride solution for 8 hours.
[0026] In a preferred embodiment, in step 4), the freezing time in the refrigerator is 24 hours, and then the drying time in the freeze dryer is 24 hours.
[0027] In a preferred embodiment, in step 5), the mass volume ratio of the composite aerogel to the pyrrole monomer is: (0.8-1.5) g: (20-80) ml.
[0028] In a preferred embodiment, in step 5), the vacuum adsorption time in the pyrrole monomer is 3 hours.
[0029] In a preferred embodiment, in step 5), the soaking reaction time in the 0°C pyrrole monomer is 6 to 8 days, preferably, the reaction time is 7 days.
[0030] In a preferred embodiment, in step 5), the ethanol / water solution is prepared from ethanol and water in a volume ratio of 1:1, and the ethanol / water solution is rinsed 2 to 4 times.
[0031] In a preferred embodiment, in step 5), after the sample is washed in the ethanol / water solution, the step further includes placing the sample in a fume hood to stand for removing the ethanol. Preferably, the standing time is 24 hours.
[0032] In a preferred embodiment, in step 5), the drying time can be determined by conventional methods known to those skilled in the art, as long as the moisture of the sample can be removed, such as drying in a vacuum oven at 40° C. for 24 hours.
[0033] In the present invention, polypyrrole is deposited on the surface of the halloysite / chitosan composite aerogel treated with glutaraldehyde / ethanol solution by vacuum impregnation. Since the adsorption and deposition of ferric chloride and pyrrole are both performed under vacuum conditions, a uniform polypyrrole conductive coating can be obtained on the surface of the halloysite / chitosan composite aerogel, thereby improving the performance of the material. In the prepared composite material, the halloysite / chitosan composite aerogel serves as a porous skeleton and the polypyrrole serves as a conductive source, which helps to produce a strong multiple reflection effect and microwave absorption effect, thereby obtaining greater conductivity and better electromagnetic shielding performance.
[0034] Another object of the present invention is to provide a halloysite / chitosan / polypyrrole composite material prepared by any of the above methods. The composite material provided by the scheme of the present invention uses halloysite and chitosan as the skeleton of the aerogel, attaches ferric chloride to the surface of the aerogel sheet by vacuum adsorption, and forms a polypyrrole coating on the surface after adsorption with pyrrole, thereby obtaining a halloysite / chitosan / polypyrrole composite material.
[0035] In a preferred embodiment, the compressive strength of the halloysite / chitosan / polypyrrole composite material can reach 3 MPa, and the electrical conductivity can reach 6.062×10 -5 S / m.
[0036] Compared with the prior art, the technical solution of the present invention has the following advantages:
[0037] 1) The technical solution provided by the present invention is to use halloysite and chitosan as the skeleton of aerogel, attach ferric chloride to the surface of the aerogel layer by vacuum adsorption, and form a polypyrrole coating on the surface after adsorption with pyrrole, thereby obtaining a halloysite / chitosan / polypyrrole composite material.
[0038] 2) In the preparation process of the present invention, the concentration of ferric chloride can be adjusted to control the amount of polypyrrole on the surface of the aerogel layer, thereby achieving control of the electromagnetic shielding performance of the halloysite / chitosan / polypyrrole composite material.
[0039] 3) The preparation conditions of the present invention are simple, the operation is simple, the cost is low, and it is particularly suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] These and / or other aspects and advantages of the present invention will become more clear and easier to understand from the following detailed description of the embodiments of the present invention in conjunction with the accompanying drawings, in which:
[0041] Figure 1 The scanning electron microscope images of the halloysite / chitosan / polypyrrole composite aerogels prepared in Examples 1-3 of the present invention, wherein (a), (b), and (c) correspond to Examples 1, 2, and 3, respectively;
[0042] Figure 2 Graphs showing the electromagnetic shielding performance of the halloysite / chitosan / polypyrrole composite aerogels prepared in Examples 1-3 of the present invention, wherein (a), (b), and (c) correspond to Examples 1, 2, and 3, respectively. DETAILED DESCRIPTION
[0043] In order to enable those skilled in the art to better understand the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific implementation methods, but it should be understood that the protection scope of the present invention is not limited to the specific implementation methods.
[0044] The present invention provides a halloysite / chitosan / polypyrrole composite material and a preparation method thereof, thereby solving the problem that the electromagnetic interference shielding material in the prior art cannot have low density, high conductivity and excellent mechanical properties.
[0045] The technical solution of the present application is described in detail below through specific embodiments:
[0046] Unless otherwise specified, the technical means used in the present invention are conventional means well known to those skilled in the art, and the various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods. The reagents used in the present invention are analytically pure unless otherwise specified.
[0047] Example 1
[0048] 1) Prepare a mixed solution of halloysite / chitosan. Add 7.5 g of chitosan to 150 ml of 4% acetic acid solution and stir in an ultrasonic cleaner. After the chitosan is completely dissolved, add 2.1 g of halloysite powder and continue stirring. After stirring evenly, crush the cells twice for 10 minutes each time.
[0049] 2) Preparation of Halloysite / Chitosan Aerogel The mixed solution obtained in step 1) was injected into molds, 8 mL per mold, and after bidirectional freezing, was placed in a freeze dryer for freeze drying for 4 days.
[0050] 3) Take 6 of the halloysite / chitosan aerogels obtained in step 2) and place them in a suction filtration container, add 150 ml of 4% glutaraldehyde / ethanol solution and vacuum adsorb for 3 hours. After the adsorption is completed, soak the sample in 4% glutaraldehyde / ethanol solution for 8 hours, pour out the solution, put it in a fume hood and let it stand for 24 hours to allow it to dry naturally.
[0051] 4) The aerogel obtained in step 3) was placed in a suction filtration container, and 150 ml of 0.3 mol / L ferric chloride solution was added for vacuum adsorption for 3 hours. After the adsorption was completed, the sample was immersed in the ferric chloride solution for 8 hours, the solution was poured out, and the sample was frozen in a refrigerator for 24 hours, and then dried in a freeze dryer for 24 hours.
[0052] 5) The aerogel obtained in step 4) is placed in a filtration container, and immersed in ice water at 0°C, 150 ml of pyrrole monomer is added and vacuum adsorbed for 3 hours. After the adsorption is completed, the sample is immersed in the pyrrole monomer and placed in a refrigerator at 0°C. After 7 days, the solution is poured out, and the sample is immersed in an ethanol / water (1:1) solution, and the solution is repeated 3 times. Then, the sample is placed in a fume hood and allowed to stand for 24 hours to remove the ethanol, and then placed in a vacuum oven at 40°C for 24 hours to remove the moisture to obtain a chitosan / halloysite / polypyrrole composite material.
[0053] Example 2
[0054] The difference between this embodiment and Example 1 is that the concentration of ferric chloride added in step 4 is 1 mol / L, and the other steps are exactly the same as those in Example 1.
[0055] Example 3
[0056] The difference between this embodiment and Example 1 is that the concentration of ferric chloride added in step 4 is 2 mol / L, and the other steps are exactly the same as those in Example 1.
[0057] Comparative Example 1
[0058] 1) Prepare a mixed solution of halloysite / chitosan, add chitosan to 4% acetic acid solution and stir in an ultrasonic cleaner, add halloysite powder after the chitosan is completely dissolved and continue stirring, stir evenly and then crush the cells twice for 10 minutes each time;
[0059] 2) Preparation of Halloysite / Chitosan Aerogel The mixed solution obtained in step 1) was injected into molds, 8 mL per mold, and after bidirectional freezing, was placed in a freeze dryer for freeze drying for 4 days.
[0060] The halloysite / chitosan / polypyrrole composite materials prepared in Examples 1 to 3 and Comparative Example 1 were tested for their performance. The results are shown in Tables 1 and Figures 1-2 shown.
[0061] Table 1 Relationship between compressive strength and ferric chloride concentration
[0062]
[0063] Table 1 shows the compressive strength, electrical conductivity and density of the halloysite / chitosan / polypyrrole composite aerogels prepared in Examples 1 to 3 of the present invention and the halloysite / chitosan composite aerogels prepared in Comparative Example 1. As shown in Table 1, with the increase of the concentration of ferric chloride, the compressive strength of the composite aerogel gradually increases, the electrical conductivity gradually increases, and the density gradually increases.
[0064] Figure 1 The scanning electron microscope images of the halloysite / chitosan / polypyrrole composite aerogel prepared in Examples 1 to 3 of the present invention are shown. It can be seen that with the increase of the concentration of ferric chloride, the roughness of the sheet surface also increases, indicating that the polypyrrole on the surface of the halloysite / chitosan aerogel increases with the increase of the ferric chloride content. At the same time, with the increase of the concentration of the adsorbed ferric chloride solution, the structure of the halloysite / chitosan / polypyrrole composite aerogel does not change much, indicating that the adsorption of ferric chloride solutions of different concentrations has no effect on the structure of the aerogel.
[0065] Figure 2This is a graph showing the total electromagnetic shielding effectiveness of the halloysite / chitosan / polypyrrole composite aerogel prepared in Examples 1 to 3 of the present invention. It can be seen that the halloysite / chitosan / polypyrrole composite aerogel exhibits excellent electromagnetic shielding performance, and as the concentration of ferric chloride increases, the total electromagnetic shielding value of the sample continues to rise. When the concentration of ferric chloride reaches 2 mol / L, the total electromagnetic shielding effectiveness reaches 20 dB. This indicates the excellent efficiency of the chitosan / haloysite / polypyrrole composite aerogel in electromagnetic shielding.
[0066] As can be seen from the above, the technical solution provided by the present invention uses halloysite and chitosan as the skeleton of aerogel, attaches ferric chloride to the surface of the aerogel sheet by vacuum adsorption, and forms a polypyrrole coating on the surface after adsorption with pyrrole, thereby obtaining a halloysite / chitosan / polypyrrole composite material. The synthesis conditions are simple, the aerogel obtained is light in weight, low in density, and high in compression strength. The content of polypyrrole attached to the aerogel is controllable, and it has both good electrical conductivity and good electromagnetic shielding properties. The anisotropy shown has high potential application value in the field of electromagnetic shielding.
[0067] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.
Claims
1. A method for preparing a halloysite / chitosan / polypyrrole composite material, characterized in that: The composite material uses the halloysite / chitosan composite aerogel as a porous skeleton and polypyrrole evenly distributed on the surface of the composite aerogel as a conductive source, and includes the following preparation methods: Chitosan is dissolved in acetic acid and mixed with halloysite to prepare a halloysite / chitosan mixed solution; the mixed solution is injected into a mold, and the halloysite / chitosan composite aerogel is obtained through bidirectional freezing and freeze drying; the obtained composite aerogel is vacuum adsorbed in glutaraldehyde / ethanol solution, ferric chloride solution, and pyrrole monomer in sequence, and finally immersed in pyrrole monomer, and after drying, the halloysite / chitosan / polypyrrole composite material is obtained.
2. The method for preparing the halloysite / chitosan / polypyrrole composite material according to claim 1, characterized in that: The preparation method specifically comprises: 1) preparing a mixed solution of halloysite / chitosan: adding chitosan powder to an acetic acid solution and dispersing until completely dissolved, and adding halloysite powder and dispersing until uniform; 2) preparing halloysite / chitosan composite aerogel: injecting the mixed solution obtained in step 1) into a mold, and after bidirectional freezing, placing it in a freeze dryer for freeze drying; 3) placing the halloysite / chitosan composite aerogel obtained in step 2) into a suction filtration container, adding a 4% glutaraldehyde / ethanol solution for vacuum adsorption for 2 to 4 hours, and after the adsorption is completed, soaking the sample in the 4% glutaraldehyde / ethanol solution for 6 to 10 hours, pouring out the solution, and drying naturally; 4) placing the composite aerogel obtained in step 3) into a suction filtration container, adding ferric chloride solution for vacuum adsorption for 2 to 4 hours, and after the adsorption is completed, soaking the sample in the ferric chloride solution for 6 to 10 hours, pouring out the solution, freezing it in a refrigerator for 18 to 30 hours, and then drying it in a freeze dryer for 18 to 30 hours; 5) The composite aerogel obtained in step 4) is placed in a suction filtration container, and is immersed in ice water at 0°C, and pyrrole monomer is added for vacuum adsorption for 2 to 4 hours. After the adsorption is completed, the sample is immersed in pyrrole monomer at 0°C for reaction. After the reaction is completed, the sample is immersed in ethanol / water solution for washing and drying to obtain a chitosan / halloysite / polypyrrole composite material.
3. The method for preparing the halloysite / chitosan / polypyrrole composite material according to claim 2, characterized in that: In step 1), the mass volume ratio of the chitosan powder, the acetic acid solution and the halloysite powder is: (0.18-2.0) g:15 ml:(0.01-1.0) g.
4. The method for preparing the halloysite / chitosan / polypyrrole composite material according to claim 2, characterized in that: In step 2), the volume of the mixed solution in each mold is 6 to 10 mL.
5. The method for preparing the halloysite / chitosan / polypyrrole composite material according to claim 2, characterized in that: In step 3), the mass volume ratio of the composite aerogel to the 4% glutaraldehyde / ethanol solution is: (0.8-1.5) g: (20-80) ml.
6. The method for preparing the halloysite / chitosan / polypyrrole composite material according to claim 2, characterized in that: In step 4), the molar concentration of the ferric chloride solution is 0.01 to 3 mol / L.
7. The method for preparing the halloysite / chitosan / polypyrrole composite material according to claim 2, characterized in that: In step 4), the mass volume ratio of the composite aerogel to the ferric chloride solution is: (0.8-1.5) g: (20-80) ml.
8. The method for preparing the halloysite / chitosan / polypyrrole composite material according to claim 2, characterized in that: In step 5), the mass volume ratio of the composite aerogel to the pyrrole monomer is: (0.8-1.5) g: (20-80) ml.
9. The method for preparing the halloysite / chitosan / polypyrrole composite material according to claim 2, characterized in that: In step 5), the soaking reaction time in the 0° C. pyrrole monomer is 6 to 8 days.
10. The halloysite / chitosan / polypyrrole composite material prepared by the method according to any one of claims 1 to 9.
Citation Information
Cited By
Wave-absorbing high-entropy alloy composite coating and preparation method thereof
CN120425337A
Efficient photo-thermal conversion and wear-resistant super-hydrophobic coating, preparation method thereof and application of coating to ice prevention and deicing
CN121406234A