Roller sleeve rubber material for charged roller of laser printer and preparation method of roller sleeve rubber material

By using nitrile rubber and copolychlorinated rubber in the charged roller of the laser printer, combining conductive carbon black and silver-carrying polyaniline-carbon nanotube composite materials, a uniform three-dimensional conductive network is solved, and the uneven charging and unsmooth surface is not smooth. Problem, improving the printing quality and service life of laser printers.

CN118994747APending Publication Date: 2024-11-22GUANGDONG JIANGYU ZHONGDING RUBBER PRODS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411142579.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing laser printer live rollers have problems such as uneven charging, poor conductivity and unsmooth surface, resulting in a lower quality of the printed image.

Method used

Nitrile rubber and copolychlorinated alcohol rubber are used as the main material, conductive carbon black and silver-carrying polyaniline-carbon nanotube composite materials are added, and a uniform three-dimensional conductive network is formed through high-temperature and high-pressure vulcanization treatment to improve conductivity and dispersion. , ensure charging uniformity and surface smoothness.

Benefits of technology

The charging uniformity and surface smoothness of the live roller are achieved, and the printing quality and service life of the laser printer are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005001301820000061
    Figure BDA0005001301820000061
Patent Text Reader

Abstract

The invention discloses a roller sleeve rubber material for a charged roller of a laser printer. The roller sleeve rubber material is prepared from the following raw materials in parts by mass: 60-100 parts of nitrile butadiene rubber NBR, 10-40 parts of copolymerized epichlorohydrin rubber ECO, 10-50 parts of conductive carbon black, 2-5 parts of a silver-loaded polyaniline-carbon nanotube composite material, 1.5-2.5 parts of a vulcanizing agent, 1-3 parts of an assistant crosslinker, 3-10 parts of zinc oxide and 1-2 parts of a dispersing agent. The charged roller made of the roller sleeve rubber material for the charged roller of the laser printer has excellent charging uniformity and is stable in electric conduction in the using process, the surface smoothness of a roller body is good, and therefore the high definition and the long service life of the laser printer are guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rubber materials, in particular to a rubber material for a roller cover of a laser printer charged roller and a preparation method thereof. Background Art

[0002] Laser printers are a type of printing output device that combines laser scanning technology with electronic photography technology. They have the advantages of fast printing speed and high imaging quality, and are widely used. During the operation of a laser printer, a negatively charged roller needs to contact the photoreceptor so that static electricity is attached to the photoreceptor. The charged roller used in a laser printer is usually composed of a core shaft and a rubber roller sleeve located on the periphery of the core shaft. The performance of the charged roller has a very important influence on the printing effect of the laser printer. However, the existing laser printer charged rollers usually have problems such as uneven charging, poor conductive stability and rough surface, which reduce the quality of the printed image. Therefore, it is necessary to further optimize the rubber material for the charged roller sleeve to improve the printing effect of the laser printer. Summary of the invention

[0003] Based on the technical problems existing in the background technology, the present invention proposes a rubber material for a roller cover of a laser printer charged roller and a preparation method thereof.

[0004] The present invention provides a rubber material for a laser printer charged roller sleeve, which comprises the following raw materials in parts by weight: 60-100 parts of nitrile rubber NBR, 10-40 parts of copolychlorohydrin rubber ECO, 10-50 parts of conductive carbon black, 2-5 parts of silver-loaded polyaniline-carbon nanotube composite material, 1.5-2.5 parts of vulcanizing agent, 1-3 parts of co-crosslinking agent, 3-10 parts of zinc oxide, and 1-2 parts of dispersant.

[0005] Preferably, the preparation method of the silver-loaded polyaniline-carbon nanotube composite material comprises: adding carbon nanotubes and aniline to a nitric acid solution for uniform ultrasonic dispersion, then sequentially adding a silver nitrate solution and an ammonium persulfate solution, stirring for reaction, and after completion of the reaction, performing solid-liquid separation, washing and drying the obtained solid matter.

[0006] Preferably, the ratio of carbon nanotubes, aniline, nitric acid solution, silver nitrate solution, and ammonium persulfate solution is 1 g: (0.2-0.4) mL: (200-400) mL: (50-200) mL: (50-200) mL.

[0007] Preferably, the concentration of the nitric acid solution is 0.5-2 mol / L, the concentration of the silver nitrate solution is 0.05-0.2 mol / L, and the concentration of the ammonium persulfate solution is 0.1-0.2 mol / L.

[0008] Preferably, in the method for preparing the silver-loaded polyaniline-carbon nanotube composite material, the stirring reaction time is 12 to 24 hours.

[0009] In the present invention, the carbon nanotubes may also be subjected to an acid activation treatment, and the specific steps may include: mixing concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 3:1 to obtain a mixed acid solution, then adding the carbon nanotubes to the mixed acid solution, and ultrasonically treating for more than 12 hours to obtain the carbon nanotubes after the acid activation treatment.

[0010] Preferably, the vulcanizing agent is at least one of tert-butyl peroxide, dicumyl peroxide and tert-butyl cumene peroxide.

[0011] Preferably, the auxiliary cross-linking agent is at least one of polytriallyl isocyanurate, triallyl cyanurate, and quinone oxime.

[0012] Preferably, the dispersant is at least one of stearic acid, polyethylene wax and erucamide.

[0013] A laser printer charging roller comprises a roller core and a rubber coating layer covering the outer side of the roller core, wherein the raw material of the rubber coating layer is the laser printer charging roller sleeve rubber material.

[0014] Preferably, the roller core is made of steel.

[0015] In the present invention, the processing method of the roller core is not particularly limited, and the roller core can be obtained by a conventional processing method, such as cutting.

[0016] A method for preparing a laser printer charging roller comprises the following steps:

[0017] S1, weighing the raw materials of the rubber coating layer by mass, adding them into an internal mixer and mixing them to obtain a rubber mix;

[0018] S2, coating the mixed rubber on the surface of the roller core to form it, and then performing high temperature and high pressure vulcanization treatment to obtain a laser printer charged roller.

[0019] Preferably, the high temperature and high pressure vulcanization treatment is carried out at a pressure of 10 to 15 MPa, a temperature of 165 to 175° C., and a time of 8 to 15 min.

[0020] The beneficial effects of the present invention are as follows:

[0021] The present invention selects nitrile rubber NBR and copolymerized ECO as main materials, uses conductive carbon black and silver-loaded polyaniline-carbon nanotube composite materials to compound, and adds a dispersant that is beneficial to the dispersibility of conductive carbon black and silver-loaded polyaniline-carbon nanotube composite materials, which not only ensures the dispersibility of conductive carbon black and silver-loaded polyaniline-carbon nanotube composite materials, but also reduces the shear force in the mixing process. At the same time, the silver-loaded polyaniline-carbon nanotube composite materials have excellent conductivity and can improve the compatibility of carbon nanotubes and rubber matrix, can be evenly dispersed in the rubber matrix, so that carbon nanotubes and carbon black form a uniform three-dimensional conductive network in the rubber matrix, thereby improving the charging uniformity of the charged roller and ensuring that the colloid surface has excellent smoothness. The charged roller manufactured by the roller sleeve rubber material of the laser printer of the present invention overcomes the shortcomings of uneven charging and rough surface of the existing charged roller, has excellent discharge uniformity, stable conductivity during use, and good roller surface smoothness, thereby ensuring the high definition and long service life of the laser printer. DETAILED DESCRIPTION

[0022] The technical solution of the present invention is described in detail below through specific embodiments.

[0023] In the following examples and comparative examples, the carbon nanotubes were subjected to an acid activation treatment before use. The specific steps included: mixing concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 3:1 to obtain a mixed acid solution, then adding the carbon nanotubes to the mixed acid solution, and ultrasonically treating for 12 hours to obtain the carbon nanotubes after the acid activation treatment.

[0024] Example 1

[0025] A rubber material for a roller cover of a laser printer charging roller comprises the following raw materials in parts by mass: 80 parts of nitrile rubber NBR, 20 parts of copolychlorohydrin rubber ECO, 30 parts of conductive carbon black, 4 parts of silver-loaded polyaniline-carbon nanotube composite material, 2 parts of diisopropyl peroxide, 2 parts of triallyl cyanurate, 5 parts of zinc oxide, and 1.5 parts of polyethylene wax.

[0026] The preparation method of the silver-loaded polyaniline-carbon nanotube composite material comprises: adding carbon nanotubes and aniline to a nitric acid solution with a concentration of 1 mol / L for uniform ultrasonic dispersion, then sequentially adding a silver nitrate solution with a concentration of 0.1 mol / L and an ammonium persulfate solution with a concentration of 0.1 mol / L, stirring for reaction for 12 hours, separating the solid from the liquid after the reaction is completed, washing and drying the obtained solid matter, and obtaining the composite material; wherein the ratio of the carbon nanotubes, aniline, nitric acid solution, silver nitrate solution and ammonium persulfate solution is 1 g: 0.2 mL: 200 mL: 100 mL: 100 mL.

[0027] A laser printer charging roller comprises a roller core and a rubber coating layer covering the outer side of the roller core, wherein the raw material of the rubber coating layer is the above-mentioned laser printer charging roller sleeve rubber material; and the preparation method thereof comprises:

[0028] S1, weighing the raw materials of the rubber coating layer by mass, adding them into an internal mixer and mixing them to obtain a rubber mix;

[0029] S2. Cutting the steel material to obtain a roller core; coating the mixed rubber on the surface of the roller core to form it, and then vulcanizing it at high temperature and high pressure at 10-15 MPa and 165-175° C. for 10 minutes to obtain a laser printer charged roller.

[0030] Example 2

[0031] A rubber material for a roller cover of a laser printer charging roller comprises the following raw materials in parts by mass: 60 parts of nitrile rubber NBR, 40 parts of copolychlorohydrin rubber ECO, 10 parts of conductive carbon black, 5 parts of silver-loaded polyaniline-carbon nanotube composite material, 1.5 parts of dicumyl peroxide, 1 part of triallyl cyanurate, 3 parts of zinc oxide, and 1 part of stearic acid.

[0032] The preparation method of the silver-loaded polyaniline-carbon nanotube composite material comprises: adding carbon nanotubes and aniline to a nitric acid solution with a concentration of 0.5 mol / L for uniform ultrasonic dispersion, then sequentially adding a silver nitrate solution with a concentration of 0.05 mol / L and an ammonium persulfate solution with a concentration of 0.1 mol / L, stirring for reaction for 12 hours, separating the solid from the liquid after the reaction is completed, washing and drying the obtained solid matter, and obtaining the composite material; wherein the ratio of the carbon nanotubes, aniline, nitric acid solution, silver nitrate solution and ammonium persulfate solution is 1 g: 0.2 mL: 200 mL: 50 mL: 50 mL.

[0033] The preparation method of the laser printer charging roller is the same as that in Example 1.

[0034] Example 3

[0035] A rubber material for a laser printer charged roller sleeve comprises the following raw materials in parts by mass: 100 parts of nitrile rubber NBR, 10 parts of copolychlorohydrin rubber ECO, 50 parts of conductive carbon black, 5 parts of silver-loaded polyaniline-carbon nanotube composite material, 2.5 parts of diisopropyl peroxide, 3 parts of triallyl cyanurate, 10 parts of zinc oxide, and 2 parts of polyethylene wax.

[0036] The preparation method of the silver-loaded polyaniline-carbon nanotube composite material comprises: adding carbon nanotubes and aniline to a nitric acid solution with a concentration of 2 mol / L for uniform ultrasonic dispersion, then sequentially adding a silver nitrate solution with a concentration of 2 mol / L and an ammonium persulfate solution with a concentration of 0.2 mol / L, stirring for reaction for 24 hours, separating the solid from the liquid after the reaction is completed, washing and drying the obtained solid matter, and obtaining the composite material; wherein the ratio of the carbon nanotubes, aniline, nitric acid solution, silver nitrate solution and ammonium persulfate solution is 1 g: 0.4 mL: 400 mL: 200 mL: 200 mL.

[0037] The preparation method of the laser printer charging roller is the same as that in Example 1.

[0038] Comparative Example 1

[0039] A rubber material for a laser printer charged roller sleeve comprises the following raw materials in parts by mass: 80 parts of nitrile rubber NBR, 20 parts of copolychlorohydrin rubber ECO, 30 parts of conductive carbon black, 4 parts of carbon nanotubes, 2 parts of dicumyl peroxide, 2 parts of triallyl cyanurate, 5 parts of zinc oxide, and 1.5 parts of polyethylene wax.

[0040] The preparation method of the laser printer charging roller is the same as that in Example 1.

[0041] Comparative Example 2

[0042] A rubber material for a laser printer charged roller sleeve comprises the following raw materials in parts by mass: 80 parts of nitrile rubber NBR, 20 parts of copolychlorohydrin rubber ECO, 30 parts of conductive carbon black, 4 parts of polyaniline-carbon nanotube composite material, 2 parts of diisopropylbenzene peroxide, 2 parts of triallyl cyanurate, 5 parts of zinc oxide, and 1.5 parts of polyethylene wax.

[0043] The preparation method of a polyaniline-carbon nanotube composite material comprises: adding carbon nanotubes and aniline to a nitric acid solution with a concentration of 1 mol / L, ultrasonically dispersing them uniformly, then adding an ammonium persulfate solution with a concentration of 0.1 mol / L, stirring and reacting for 12 hours, separating the solid and the liquid after the reaction is completed, washing and drying the obtained solid material, and obtaining the composite material; wherein the ratio of the carbon nanotubes, aniline, nitric acid solution and ammonium persulfate solution is 1 g: 0.2 mL: 200 mL: 100 mL.

[0044] The preparation method of the laser printer charging roller is the same as that in Example 1.

[0045] Test example

[0046] The resistance fluctuation test was performed on the charged rollers of Example 1 and Comparative Examples 1-2. The results are shown in Table 1:

[0047] Table 1

[0048]

[0049] The surface roughness of the charged rollers of Example 1 and Comparative Examples 1 to 2 was tested with reference to HG / T 3078-2001. The results are shown in Table 2:

[0050] Table 2

[0051] Example 1 Comparative Example 1 Comparative Example 2 Surface roughness Ra(μm) 0.48 0.86 0.52

[0052] From the test results of Table 1 and Table 2, it can be seen that the comparative example 1 uses carbon nanotubes and conductive carbon black as the conductive agent, and the resistance uniformity and surface smoothness are poor, which is due to the uneven distribution of carbon nanotubes in the matrix; the comparative example 2 uses polyaniline-carbon nanotube composite material and conductive carbon black as the conductive agent. After the introduction of polyaniline, although the compatibility between the material and the matrix is ​​improved, it is not conducive to forming a uniform three-dimensional network conductive path, so the improvement of resistance uniformity is not ideal. In contrast, the charged roller made of the roller sleeve rubber material of the laser printer of the present invention has excellent discharge uniformity and surface smoothness, which helps to improve the printing quality.

[0053] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A rubber material for a laser printer charged roller cover, characterized in that: The invention comprises the following raw materials in parts by weight: 60 to 100 parts of nitrile rubber NBR, 10 to 40 parts of copolychlorohydrin rubber ECO, 10 to 50 parts of conductive carbon black, 2 to 5 parts of silver-loaded polyaniline-carbon nanotube composite material, 1.5 to 2.5 parts of vulcanizing agent, 1 to 3 parts of auxiliary cross-linking agent, 3 to 10 parts of zinc oxide and 1 to 2 parts of dispersant.

2. The rubber material for the charged roller cover of a laser printer according to claim 1, characterized in that: The preparation method of the silver-loaded polyaniline-carbon nanotube composite material comprises: adding carbon nanotubes and aniline into a nitric acid solution for uniform ultrasonic dispersion, then sequentially adding a silver nitrate solution and an ammonium persulfate solution, stirring for reaction, separating the solid from the liquid after the reaction is completed, washing and drying the obtained solid matter, and obtaining the composite material.

3. The rubber material for the charged roller cover of a laser printer according to claim 2, characterized in that: The ratio of carbon nanotubes, aniline, nitric acid solution, silver nitrate solution, and ammonium persulfate solution is 1 g: (0.2-0.4) mL: (200-400) mL: (50-200) mL: (50-200) mL.

4. The rubber material for the charged roller cover of a laser printer according to claim 2, characterized in that: The concentration of the nitric acid solution is 0.5-2 mol / L, the concentration of the silver nitrate solution is 0.05-0.2 mol / L, and the concentration of the ammonium persulfate solution is 0.1-0.2 mol / L.

5. The rubber material for the charged roller cover of a laser printer according to claim 1, characterized in that: The vulcanizing agent is at least one of tert-butyl peroxide, dicumyl peroxide and tert-butyl cumene peroxide.

6. The rubber material for the charged roller cover of a laser printer according to claim 1, characterized in that: The auxiliary cross-linking agent is at least one of polytriallyl isocyanurate, triallyl cyanurate, and quinone oxime.

7. The rubber material for the charged roller cover of a laser printer according to claim 1, characterized in that: The dispersant is at least one of stearic acid, polyethylene wax and erucamide.

8. A laser printer charging roller, characterized in that: It comprises a roller core and a rubber coating layer covering the outer side of the roller core, wherein the raw material of the rubber coating layer is the rubber material for the roller cover of the laser printer charging roller according to any one of claims 1 to 7.

9. The laser printer charging roller according to claim 8, characterized in that: The material of the roller core is steel.

10. A method for preparing a laser printer charging roller as claimed in claim 8 or 9, characterized in that: The steps include: S1, weighing the raw materials of the rubber coating layer by mass, adding them into an internal mixer and mixing them to obtain a mixed rubber; S2, coating the mixed rubber on the surface of the roller core to form it, and then performing high temperature and high pressure vulcanization treatment to obtain a laser printer charged roller.