High-toughness phenolic resin-based composite material and preparation method thereof
By adding modified ramie fibers and eloite nanotubes to the phenolic resin-based composite materials to form a crosslinking network structure, the problem of insufficient toughness of phenolic resin is solved, and its mechanical properties and impact resistance are significantly improved.
Patent Information
- Application Number
- CN202411364008.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-28
- Publication Date
- 2024-11-22
AI Technical Summary
The toughness of phenolic resins is poor, resulting in poor impact resistance, and it is difficult for the prior art to effectively improve their mechanical properties.
By adding ramie fibers to the phenolic resin-based composite material and modifying silane coupling agent, a cross-linking network structure is formed, and the Elosite nanotubes are combined to improve the interface compatibility and adhesion properties of ramie fibers and phenolic resins. Strengthen the toughness of the material.
The toughness and mechanical properties of phenolic resin-based composite materials have been significantly improved, and their resistance to shocks has been enhanced.
Smart Images

Figure BDA0005065682220000071 
Figure BDA0005065682220000081
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of polymer materials, and in particular to a high-toughness phenolic resin-based composite material and a preparation method thereof. Background Art
[0002] Phenolic resin refers to an organic high molecular polymer produced by condensation reaction under alkaline or acidic conditions with phenol and aldehyde as the main raw materials. It has excellent high temperature resistance and can maintain structural stability and integrity through high residual carbon rate even at very high ambient temperatures.
[0003] However, since all types of phenols used in phenolic resin raw materials contain benzene rings, after the condensation reaction of phenol and aldehyde, the rigid aromatic rings connected to the methylene group are tightly stacked, which will cause the cured phenolic resin to have poor toughness and poor impact resistance. Summary of the invention
[0004] In order to improve the toughness of phenolic resin so as to improve the mechanical properties of phenolic resin-based composite materials, the present application provides a high-toughness phenolic resin-based composite material and a preparation method thereof.
[0005] In the first aspect, the present application provides a high-toughness phenolic resin-based composite material, which adopts the following technical solution: a high-toughness phenolic resin-based composite material, including 120-160 parts of phenolic resin, 15-22 parts of ramie fiber, 22-28 parts of calcium carbonate, and 9-13 parts of catechol.
[0006] By adopting the above technical solution, the phenolic resin-based composite material produced by using ramie fiber as one of the raw materials has higher toughness. The specific solution analysis is as follows: Ramie fiber has strong flexibility, so adding ramie fiber to the phenolic resin-based composite material makes the phenolic resin-based composite material have stronger toughness, thereby improving the mechanical properties of the phenolic resin-based composite material.
[0007] Preferably, the ramie fiber is prepared by the following modification steps: The silane coupling agent is added into the ethanol aqueous solution and stirred evenly to obtain a silane coupling agent solution. Then, the ramie fiber is put into the silane coupling agent solution, subjected to ultrasonic treatment and then dried to obtain the modified ramie fiber.
[0008] By adopting the above technical solution, since the surface of the ramie fiber contains a large amount of hydroxyl groups and impurities, it is easy to cause the interface compatibility between the ramie fiber and the phenolic resin to be poor.
[0009] The silane coupling agent is hydrolyzed and reacted to produce a cross-linked network structure, and a cross-linked network film is formed on the surface of the ramie fiber. Therefore, when preparing a phenolic resin-based composite material, the phenolic resin may penetrate into the cross-linked network structure, thereby increasing the interaction between the ramie fiber and the phenolic resin.
[0010] In addition, the hydroxyl groups after hydrolysis of the silane coupling agent react with the hydroxyl groups on the surface of the ramie fiber to form covalent bonds or hydrogen bonds, so that the silane coupling agent is bound to the surface of the ramie fiber, so that the adhesion performance between the ramie fiber and the phenolic resin is improved, and the interface compatibility between the ramie fiber and the phenolic resin is effectively improved, thereby improving the toughness of the phenolic resin-based composite material.
[0011] Preferably, halloysite nanotubes are further added during the modification and preparation process of the ramie fiber, and the ramie fiber is prepared by the following modification steps: A silane coupling agent is added to an ethanol aqueous solution and stirred evenly to obtain a silane coupling agent solution. Halloysite nanotubes are then added to the silane coupling agent solution and stirred evenly to obtain a mixture. Finally, ramie fiber is added to the mixture, ultrasonically treated, and then dried to obtain modified ramie fiber.
[0012] By adopting the above technical solution, halloysite nanotubes, a nanocrystalline material, have a large specific surface area and a unique hollow tubular structure, which makes it have excellent reinforcement performance. Therefore, halloysite nanotubes are added as one of the raw materials to the phenolic resin-based composite material, so that the toughness of the phenolic resin-based composite material is improved, thereby improving the mechanical properties of the phenolic resin-based composite material.
[0013] When halloysite nanotubes are added to the modification process of ramie fiber with silane coupling agent, not only the halloysite nanotubes are evenly distributed, but also the amount of halloysite nanotubes bound to the surface of ramie fiber is increased, and the roughness of the surface of ramie fiber is improved, so that ramie fiber and phenolic resin can be effectively bonded.
[0014] In addition, the halloysite nanotubes can be better dispersed in the cross-linked network structure formed by the phenolic resin, thereby improving the interface bonding force between the halloysite nanotubes and the phenolic resin, and effectively improving the mechanical properties of the phenolic resin-based composite material.
[0015] Preferably, the mass ratio of the ramie fiber, the silane coupling agent and the halloysite nanotube is (110-150):1:(1.3-1.5).
[0016] By adopting the above technical solution and controlling the mass ratio of ramie fiber, silane coupling agent and halloysite nanoparticles within the above range, the mechanical properties of the phenolic resin-based composite material can be effectively improved.
[0017] Preferably, the silane coupling agent is KH-550.
[0018] Preferably, the ramie fiber is pretreated before modification and preparation, and the pretreatment of the ramie fiber comprises the following steps: The ramie fiber is immersed in a sodium hydroxide aqueous solution, subjected to ultrasonic treatment, and then sequentially washed and dried to obtain the pretreated ramie fiber.
[0019] By adopting the above technical scheme, after the ramie fiber is treated with sodium hydroxide, impurities such as lignin and pectin on the surface of the ramie fiber are removed, so that the surface of the ramie fiber has obvious grooves, thereby increasing the roughness of the surface of the ramie fiber, which is beneficial to increase the contact area between the ramie fiber and the phenolic resin.
[0020] Preferably, the halloysite nanotubes are prepared by the following modification steps: Polyethyleneimine is added into deionized water to prepare a polyethyleneimine aqueous solution, and then halloysite nanotubes are added into the polyethyleneimine aqueous solution, and stirred evenly to prepare an aqueous phase suspension, which is then filtered, washed, and dried in sequence to prepare modified halloysite nanotubes.
[0021] By adopting the above technical solution, the Zeta potential of the halloysite nanotubes is negative, so that they can interact with the cationic polymer polyethyleneimine through electrostatic force, thereby improving the roughness and specific surface area of the halloysite nanotube surface, thereby enhancing the positive effect of adding halloysite nanotubes to phenolic resin-based materials on improving mechanical properties.
[0022] Preferably, the mass ratio of the halloysite nanotubes to polyethyleneimine is 1:(0.12-0.16).
[0023] By adopting the above technical solution and controlling the mass ratio of halloysite nanotubes to polyethyleneimine within the above range, the surface roughness and specific surface area of the halloysite nanotubes can be effectively improved.
[0024] In a second aspect, the present application provides a method for preparing a high-toughness phenolic resin-based composite material as in the first aspect, which adopts the following technical solution: A method for preparing a high-toughness phenolic resin-based composite material comprises the following steps: The phenolic resin, ramie fiber, calcium carbonate and catechol are mixed and stirred evenly to prepare a high-toughness phenolic resin-based composite material.
[0025] In summary, the present application includes at least one of the following beneficial technical effects: 1. Ramie fiber has strong flexibility, so adding ramie fiber to phenolic resin-based composite materials makes the phenolic resin-based composite materials have stronger toughness, thereby improving the mechanical properties of the phenolic resin-based composite materials.
[0026] 2. The silane coupling agent reacts after hydrolysis to form a cross-linked network film on the surface of the ramie fiber, which effectively improves the interaction between the ramie fiber and the phenolic resin; the hydroxyl groups of the hydrolyzed silane coupling agent react with the hydroxyl groups on the surface of the ramie fiber to form covalent bonds or hydrogen bonds, so that the silane coupling agent is bonded to the surface of the ramie fiber, which effectively improves the interface compatibility between the ramie fiber and the phenolic resin, thereby improving the toughness of the phenolic resin-based composite material. DETAILED DESCRIPTION
[0027] The present application is further described in detail below in conjunction with the examples and comparative examples. The raw materials involved in the present application can all be obtained commercially, among which the phenolic resin is provided by Shanghai MacLean Biochemical Technology Co., Ltd., and the polyethyleneimine is provided by Shanghai Hanluo New Materials Co., Ltd.
[0028] Example 1 The high-toughness phenolic resin-based composite material includes the following raw materials by weight: 120 g of phenolic resin, 15 g of ramie fiber, 22 g of calcium carbonate, and 9 g of catechol.
[0029] The preparation method of the high-toughness phenolic resin-based composite material comprises the following steps: The phenolic resin, ramie fiber, calcium carbonate and catechol are mixed and stirred evenly to prepare a high-toughness phenolic resin-based composite material.
[0030] Example 2 The high-toughness phenolic resin-based composite material includes the following raw materials by weight: 160 g of phenolic resin, 22 g of ramie fiber, 28 g of calcium carbonate, and 13 g of catechol.
[0031] The preparation method of the high-toughness phenolic resin-based composite material comprises the following steps: The phenolic resin, ramie fiber, calcium carbonate and catechol are mixed and stirred evenly to prepare a high-toughness phenolic resin-based composite material.
[0032] Example 3 The high-toughness phenolic resin-based composite material includes the following raw materials by weight: 140 g of phenolic resin, 18 g of ramie fiber, 25 g of calcium carbonate, and 11 g of catechol.
[0033] The preparation method of the high-toughness phenolic resin-based composite material comprises the following steps: The phenolic resin, ramie fiber, calcium carbonate and catechol are mixed and stirred evenly to prepare a high-toughness phenolic resin-based composite material.
[0034] Example 4 The difference between Example 4 and Example 3 is that the ramie fiber is prepared by the following modification steps: 1 g of silane coupling agent was added to 300 g of ethanol aqueous solution (the mass concentration of ethanol aqueous solution was 20%), and magnetic stirring was performed at 25°C for 30 minutes to obtain a silane coupling agent solution. Then 110 g of ramie fiber was placed in the silane coupling agent solution, and after ultrasonic treatment for 60 minutes, the fiber was placed in a 100°C drying oven for drying to obtain modified ramie fiber.
[0035] The silane coupling agent is KH-550.
[0036] Example 5 The difference between Example 5 and Example 3 is that the ramie fiber is prepared by the following modification steps: 1 g of silane coupling agent was added to 300 g of ethanol aqueous solution (the mass concentration of the ethanol aqueous solution was 20%), and magnetic stirring was performed at 25°C for 30 minutes to obtain a silane coupling agent solution. Then 150 g of ramie fiber was placed in the silane coupling agent solution, and after ultrasonic treatment for 60 minutes, the fiber was placed in a 100°C drying oven for drying to obtain modified ramie fiber.
[0037] The silane coupling agent is KH-550.
[0038] Example 6 The difference between Example 6 and Example 3 is that the ramie fiber is prepared by the following modification steps: 1 g of silane coupling agent was added to 300 g of ethanol aqueous solution (the mass concentration of the ethanol aqueous solution was 20%), and magnetic stirring was performed at 25°C for 30 minutes to obtain a silane coupling agent solution. Then 130 g of ramie fiber was placed in the silane coupling agent solution, and after ultrasonic treatment for 60 minutes, the fiber was placed in a 100°C drying oven for drying to obtain modified ramie fiber.
[0039] The silane coupling agent is KH-550.
[0040] Example 7 The difference between Example 7 and Example 6 is that the mass ratio of ramie fiber to KH-550 is 90:1.
[0041] Example 8 The difference between Example 8 and Example 6 is that the mass ratio of ramie fiber to KH-550 is 170:1.
[0042] Example 9 The difference between Example 9 and Example 6 is that halloysite nanotubes are further added during the modification and preparation process of ramie fiber, and the ramie fiber is prepared by the following modification steps: 1 g of silane coupling agent was added to 300 g of ethanol aqueous solution (the mass concentration of the ethanol aqueous solution was 20%), and magnetically stirred for 30 minutes at 25°C to obtain a silane coupling agent solution. Then 1.5 g of halloysite nanotubes were added to the silane coupling agent solution, and magnetically stirred at 25°C until a uniform mixture was formed. Then 110 g of ramie fiber was put into the mixture, and after ultrasonic treatment for 60 minutes, the mixture was dried in a 100°C drying oven to obtain modified ramie fiber.
[0043] The silane coupling agent is KH-550.
[0044] Example 10 The difference between Example 10 and Example 6 is that halloysite nanotubes are further added during the modification and preparation process of ramie fiber, and the ramie fiber is prepared by the following modification steps: 1 g of silane coupling agent was added to 300 g of ethanol aqueous solution (the mass concentration of the ethanol aqueous solution was 20%), and magnetically stirred for 30 minutes at 25°C to obtain a silane coupling agent solution. Then 1.3 g of halloysite nanotubes were added to the silane coupling agent solution, and magnetically stirred at 25°C until a uniform mixture was formed. Then 150 g of ramie fiber was put into the mixture, and after ultrasonic treatment for 60 minutes, the mixture was dried in a 100°C drying oven to obtain modified ramie fiber.
[0045] The silane coupling agent is KH-550.
[0046] Embodiment 11 The difference between Example 11 and Example 6 is that halloysite nanotubes are further added during the modification and preparation process of ramie fiber, and the ramie fiber is prepared by the following modification steps: 1 g of silane coupling agent was added to 300 g of ethanol aqueous solution (the mass concentration of the ethanol aqueous solution was 20%), and magnetically stirred for 30 minutes at 25°C to obtain a silane coupling agent solution. Then 1.4 g of halloysite nanotubes were added to the silane coupling agent solution, and magnetically stirred at 25°C until a uniform mixture was formed. Then 130 g of ramie fiber was put into the mixture, and after ultrasonic treatment for 60 minutes, the mixture was dried in a 100°C drying oven to obtain modified ramie fiber.
[0047] The silane coupling agent is KH-550.
[0048] Example 12 The difference between Example 12 and Example 11 is that the mass ratio of ramie fiber, KH-550 and halloysite nanotube is 130:1:1.1.
[0049] Embodiment 13 The difference between Example 13 and Example 11 is that the mass ratio of ramie fiber, KH-550 and halloysite nanotube is 130:1:1.7.
[0050] Embodiment 14 The difference between Example 14 and Example 11 is that the ramie fiber is pretreated before the preparation and modification, and the pretreatment of the ramie fiber includes the following steps: The ramie fiber was immersed in a sodium hydroxide aqueous solution (the mass concentration of the sodium hydroxide aqueous solution was 5%), and ultrasonically treated for 60 minutes at 25°C, and then washed with deionized water for multiple times until the pH of the washing water was neutral, and then dried in a 100°C oven to obtain pretreated ramie fiber.
[0051] Embodiment 15 The difference between Example 15 and Example 14 is that the halloysite nanotubes are prepared by modification through the following steps: 12 g of polyethyleneimine was added to 160 g of deionized water to obtain a polyethyleneimine aqueous solution, and then 100 g of halloysite nanotubes were added to the polyethyleneimine aqueous solution. The suspension was rotated at 100 r / min for 100 min at 25°C to obtain an aqueous suspension. The suspension was then filtered and washed, and dried in a vacuum oven at 60°C for 24 h to obtain modified halloysite nanotubes.
[0052] Example 16 The difference between Example 16 and Example 14 is that the halloysite nanotubes are prepared by modification through the following steps: 16 g of polyethyleneimine was added to 160 g of deionized water to obtain a polyethyleneimine aqueous solution, and then 100 g of halloysite nanotubes were added to the polyethyleneimine aqueous solution. The suspension was rotated at 100 r / min for 100 min at 25°C to obtain an aqueous suspension. The suspension was then filtered and washed, and dried in a vacuum oven at 60°C for 24 h to obtain modified halloysite nanotubes.
[0053] Embodiment 17 The difference between Example 17 and Example 14 is that the halloysite nanotubes are prepared by modification through the following steps: 14 g of polyethyleneimine was added to 160 g of deionized water to obtain a polyethyleneimine aqueous solution, and then 100 g of halloysite nanotubes were added to the polyethyleneimine aqueous solution. The suspension was rotated at 100 r / min for 100 min at 25°C to obtain an aqueous suspension. The suspension was then filtered and washed, and dried in a vacuum oven at 60°C for 24 h to obtain modified halloysite nanotubes.
[0054] Embodiment 18 The difference between Example 18 and Example 17 is that the mass ratio of halloysite nanotubes to polyethyleneimine is 1:0.10.
[0055] Embodiment 19 The difference between Example 19 and Example 17 is that the mass ratio of halloysite nanotubes to polyethyleneimine is 1:0.18.
[0056] Comparative Example 1 The difference between Comparative Example 1 and Example 3 is that the high-toughness phenolic resin-based composite material does not contain ramie fiber.
[0057] The high-toughness phenolic resin-based composite material includes the following raw materials by weight: 140 g of phenolic resin, 24 g of calcium carbonate, and 11 g of catechol.
[0058] The preparation method of the high-toughness phenolic resin-based composite material comprises the following steps: The phenolic resin, calcium carbonate and catechol are mixed and stirred evenly to prepare a high-toughness phenolic resin-based composite material.
[0059] Performance Testing The high-toughness phenolic resin-based composite materials prepared in Examples 1-19 and Comparative Example 1 were placed in a custom mold (with a mold release agent, dimethyl silicone oil, evenly applied to the mold surface), and then the mold was placed on a flat vulcanizer for heating and pressing at a pressure of 5 MPa, a temperature of 140°C, and a time of 60 minutes to prepare the sample. After heating, the temperature of the flat vulcanizer was adjusted to 25°C, and the pressure was released and the sample strip was taken out and the following was performed.
[0060] Mechanical properties testing: According to the relevant provisions of GB-T1040-1992 "Test Method for Tensile Properties of Plastics", the tensile strength test was carried out. Each sample was tested 6 times, and the average value of 6 groups was taken as the result and recorded in Table 1.
[0061] According to the relevant provisions of GB-T1843-1996 "Plastic Izod Beam Impact Test Method", the tensile impact strength test was carried out. Each sample was tested 6 times, and the average value of 6 groups was taken as the result and recorded in Table 1.
[0062] Table 1 Specifically, in combination with the test results of Examples 4-6 and Example 3, the tensile strength of Examples 4-6 is 28.32-28.47 MPa, and the impact strength is 6.59-6.68 kJ / m 2 The tensile strength of Example 3 is 25.51 MPa and the impact strength is 5.71 kJ / m 2, it can be seen that the mechanical properties of Example 4-6 are better than those of Example 3, and the analysis is as follows: The difference between Example 4-6 and Example 3 is that after the ramie fiber is modified with a silane coupling agent, not only a cross-linked network film is formed on the surface of the ramie fiber, but also the silane coupling agent is bonded to the surface of the ramie fiber to improve the interface compatibility between the ramie fiber and the phenolic resin, thereby improving the toughness of the phenolic resin-based composite material, and then effectively improving the mechanical properties of the phenolic resin-based composite material.
[0063] Specifically, in combination with the test results of Examples 9-11 and Example 6, the tensile strength of Examples 9-11 is 30.68-30.79 MPa, and the impact strength is 7.69-7.73 kJ / m 2 The tensile strength of Example 6 is 28.47MPa and the impact strength is 6.68kJ / m 2 , it can be seen that the mechanical properties of Examples 9-11 are better than those of Example 6, and the analysis is as follows: The difference between Examples 9-11 and Example 6 is that halloysite nanotubes are also added to the ramie fiber during the modification process of the silane coupling agent. On the one hand, the amount of halloysite nanotubes bound to the surface of the ramie fiber is increased, which effectively improves the roughness of the surface of the ramie fiber, thereby improving the effective adhesion between the ramie fiber and the phenolic resin. On the other hand, the halloysite nanotubes can be better dispersed in the cross-linked network structure formed by the phenolic resin, thereby improving the interfacial bonding force between the halloysite nanotubes and the phenolic resin, thereby improving the mechanical properties of the phenolic resin-based composite material.
[0064] Specifically, in combination with the test results of Example 14 and Example 11, the tensile strength of Example 14 is 31.24 MPa and the impact strength is 7.97 kJ / m 2 The tensile strength of Example 11 is 30.79 MPa and the impact strength is 7.73 kJ / m 2 , it can be seen that the mechanical properties of Example 14 are better than those of Example 11, and the analysis is as follows: The difference between Example 14 and Example 11 is that after the ramie fiber is treated with sodium hydroxide, there are obvious grooves on the surface of the ramie fiber, thereby increasing the roughness of the ramie fiber surface, so that the contact area between the ramie fiber and the phenolic resin is increased, thereby improving the mechanical properties of the phenolic resin-based composite material.
[0065] Specifically, in combination with the test results of Examples 15-17 and Example 14, the tensile strength of Examples 15-17 is 33.82-33.88 MPa, and the impact strength is 8.80-8.86 kJ / m 2 The tensile strength of Example 14 is 31.24 MPa and the impact strength is 7.97 kJ / m 2, it can be seen that the mechanical properties of Examples 15-17 are better than those of Example 14, and the analysis is as follows: The difference between Examples 15-17 and Example 14 is that after the halloysite nanotubes are modified with polyethyleneimine, the surface roughness and specific surface area of the halloysite nanotubes are improved, thereby enhancing the positive effect of adding halloysite nanotubes to phenolic resin-based materials on improving the mechanical properties.
[0066] Specifically, in combination with the test results of Example 3 and Comparative Example 1, the tensile strength of Example 3 is 25.51 MPa and the impact strength is 5.71 kJ / m 2 The tensile strength of comparative example 1 is 17.43MPa and the impact strength is 4.15kJ / m 2 , it can be seen that the strength of Example 3 is better than that of Comparative Example 1, and the analysis is as follows: The difference between Example 3 and Comparative Example 1 is that ramie fiber is added to the phenolic resin-based material, and the ramie fiber has strong flexibility and can improve the toughness of the phenolic resin-based composite material, thereby improving the mechanical properties of the phenolic resin-based composite material.
[0067] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A high-toughness phenolic resin-based composite material, characterized in that: The invention comprises 120-160 parts of phenolic resin, 15-22 parts of ramie fiber, 22-28 parts of calcium carbonate and 9-13 parts of catechol.
2. A high-toughness phenolic resin-based composite material according to claim 1, characterized in that: The ramie fiber is prepared by the following modification steps: The silane coupling agent is added into the ethanol aqueous solution and stirred evenly to obtain a silane coupling agent solution. Then, the ramie fiber is put into the silane coupling agent solution, subjected to ultrasonic treatment and then dried to obtain the modified ramie fiber.
3. A high-toughness phenolic resin-based composite material according to claim 2, characterized in that: Halloysite nanotubes are also added during the modification and preparation process of the ramie fiber. The ramie fiber is prepared by the following modification steps: A silane coupling agent is added to an ethanol aqueous solution and stirred evenly to obtain a silane coupling agent solution. Halloysite nanotubes are then added to the silane coupling agent solution and stirred evenly to obtain a mixture. Finally, ramie fiber is added to the mixture, ultrasonically treated, and then dried to obtain modified ramie fiber.
4. A high-toughness phenolic resin-based composite material according to claim 3, characterized in that: The mass ratio of the ramie fiber, the silane coupling agent and the halloysite nanotube is (110-150):1:(1.3-1.5).
5. The high-toughness phenolic resin-based composite material according to claim 3, characterized in that: The silane coupling agent is KH-550.
6. The high-toughness phenolic resin-based composite material according to claim 3, characterized in that: The ramie fiber is also pretreated before modification and preparation, and the pretreatment of the ramie fiber includes the following steps: The ramie fiber is immersed in a sodium hydroxide aqueous solution, subjected to ultrasonic treatment, and then sequentially washed and dried to obtain the pretreated ramie fiber.
7. The high-toughness phenolic resin-based composite material according to claim 1, characterized in that: The halloysite nanotubes are prepared by the following modification steps: Polyethyleneimine is added into deionized water to prepare a polyethyleneimine aqueous solution, and then halloysite nanotubes are added into the polyethyleneimine aqueous solution, and stirred evenly to prepare an aqueous phase suspension, which is then filtered, washed, and dried in sequence to prepare modified halloysite nanotubes.
8. The high-toughness phenolic resin-based composite material according to claim 7, characterized in that: The mass ratio of the halloysite nanotubes to polyethyleneimine is 1:(0.12-0.16).
9. A method for preparing a high-toughness phenolic resin-based composite material as claimed in claim 1, characterized in that: The steps include: The phenolic resin, ramie fiber, calcium carbonate and catechol are mixed and stirred evenly to prepare a high-toughness phenolic resin-based composite material.