Bio-based polyurethane composite material and preparation method thereof
By using phosphophenylbenzotriazole-based modified bio-based polyurethane and biomass fibers in bio-based polyurethane materials, an interpenetrating network cross-linking structure is formed, and the mechanical and mechanical properties and resistance of bio-based polyurethane materials are solved. The problem of insufficient combustion and heat-resistant aging performance has achieved significant improvement in performance and degradability, making it suitable for large-scale production.
Patent Information
- Application Number
- CN202411200118.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing bio-based polyurethane materials have shortcomings in mechanical and mechanical properties, flame retardant and heat-resistant aging properties, which limits their development and actual use.
Using phosphophenylbenzotriazolyl modified bio-polyurethane and biomass fibers, coupling agents, isocyanoethyl methacrylate, tris(2-acryloyloxyethyl) isocyanurate and other raw materials The combination of the bio-based polyurethane composite material is prepared by a twin-screw extrusion process to form an interpenetrating network cross-linking structure under multiple actions.
It significantly improves the mechanical and mechanical properties, flame retardant and heat-resistant aging properties of bio-based polyurethane composite materials, while maintaining degradability and environmental protection. It has simple process and convenient operation, and is suitable for continuous and large-scale production.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite materials, and in particular to a bio-based polyurethane composite material and a preparation method thereof. Background Art
[0002] Polyurethane is a common polymer resin on the market. With its good physical and mechanical properties, easily controllable chemical structure and good biocompatibility, it is widely used in agricultural production, civil life, construction, biomedicine and other fields. However, with people's continuous pursuit of high-quality life, the shortcomings exposed by traditional polyurethane products are gradually difficult to be accepted by people. The most obvious one is that in the preparation process of traditional polyurethane, non-renewable petroleum and its derivatives are used as monomer raw materials, and the synthesis of monomer raw materials requires the use of toxic gas phosgene, which will pollute the natural environment. Therefore, in order to meet social challenges and respond to the country's sustainable and "dual carbon" policies, synthesizing bio-based polyurethane products through studying biomass resources and giving products degradability have become hot research topics in the industry.
[0003] Bio-based polyurethane materials refer to high molecular weight compounds prepared by using polyols or polyisocyanates synthesized from biological resources to partially or completely replace petroleum-based monomer raw materials and participate in the addition polymerization process of polyurethane. At present, bio-based polyurethane materials on the market have more or less technical defects such as low strength, poor flame retardancy, and insufficient heat resistance, which limit their development and practical use.
[0004] In order to solve the above problems, the current conventional practice is to add functional additives to bio-based polyurethane materials to make bio-based polyurethane composites. However, due to compatibility issues, these functional additives are prone to seep out of the composites during long-term use, and the addition of a large amount of functional additives will also cause defects such as poor material processing fluidity.
[0005] For example, the Chinese invention patent with application publication number CN116790111A discloses a novel bio-based thermoplastic polyurethane elastomer composite material and its preparation method, which includes TPU material, cellulose nanocrystal material, wood cellulose nanocrystal and boron-nitrogen coordination crosslinking agent. The invention adopts cellulose nanocrystal material instead of wood powder fiber. During the preparation, the material structure of the fiber nanocrystal itself is not easily destroyed after the staged temperature rise. The cellulose nanocrystal is more uniform than the cellulose powder and TPU melt blending, and it is not easy to have fibers and gaps in the composite material section, so that the composite material obtained by rapid cooling and crystallization has higher strength. Cellulose nanocrystals have a good ability to transfer loads, and the effect on the tensile properties of TPU after blending is lower than that of wood powder fiber. However, the mechanical properties, flame retardancy and heat aging resistance of the bio-based polyurethane composite material still need to be further improved. Summary of the invention
[0006] The purpose of the present invention is to overcome the deficiencies of the prior art and to provide a bio-based polyurethane composite material having good mechanical properties, excellent flame retardancy and heat aging resistance and a preparation method thereof.
[0007] To achieve the above-mentioned purpose, the technical scheme adopted by the present invention is: a bio-based polyurethane composite material, comprising the following raw materials in parts by weight: 100 parts of phosphaphenanthrylbenzotriazole-modified bio-based polyurethane, 10-20 parts of biomass fiber, 1-3 parts of coupling agent, 3-5 parts of isocyanoethyl methacrylate, 2-4 parts of tris(2-acryloyloxyethyl)isocyanurate, 0.8-1.2 parts of initiator, 0.8-1.2 parts of catalyst A, 0.3-0.6 parts of antioxidant, and 0.7-1 parts of plasticizer; the phosphaphenanthrylbenzotriazole-modified bio-based polyurethane comprises the following monomer-introduced structural units: 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthryl-10-oxide, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, bio-based diol, and bio-based diisocyanate.
[0008] Preferably, the plasticizer is epoxidized soybean oil.
[0009] Preferably, the antioxidant is at least one of antioxidant 1010 and antioxidant 168.
[0010] Preferably, the catalyst A is dibutyltin dilaurate.
[0011] Preferably, the initiator is a mixture of dicumyl peroxide, benzoyl peroxide and 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane in a mass ratio of 1:(0.8-1.2):(1-2).
[0012] Preferably, the coupling agent is at least one of silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570.
[0013] Preferably, the biomass fiber is at least one of bamboo pulp fiber and hemp pulp fiber.
[0014] Preferably, the average diameter of the biomass fiber is 3-9 μm, and the aspect ratio is (20-30):1.
[0015] Preferably, the preparation method of the phosphaphenanthrylbenzotriazole-modified bio-based polyurethane comprises the following steps: adding 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthryl-10-oxide, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, bio-based diol, bio-based diisocyanate, and dibutyltin dilaurate to a high boiling point solvent, stirring and reacting at 76-90° C. in an inert gas atmosphere for 4-6 hours, then heating to 95-98° C. and continuing to stir and react for 8-12 hours, then adding a reaction chain terminator, continuing to stir and react for 0.1-0.3h, precipitating in water after the reaction is completed, washing the precipitated polymer with ethanol for 3-6 times, and finally removing the residual solvent by rotary evaporation to obtain the phosphaphenanthrylbenzotriazole-modified bio-based polyurethane.
[0016] Preferably, the molar ratio of the 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, N-[(4-methyl-1H-benzotriazol-1-yl)methyl]diethanolamine, bio-based diol, bio-based diisocyanate, dibutyltin dilaurate, high boiling point solvent, and reaction chain terminator is 0.1:0.1:0.8:1:(0.8-1.2):(9-15):(0.03-0.05).
[0017] Preferably, the bio-based diol is any one of 1,3-propylene glycol, 1,4-butanediol, NX-9212 cashew nut shell oil diol, and PO3GH500 polytrimethylene ether glycol.
[0018] Preferably, the bio-based diisocyanate is any one of 1,5-pentane diisocyanate and L-lysine diisocyanate.
[0019] Preferably, the reaction chain terminator is 1,3-propylene glycol.
[0020] Preferably, the high boiling point solvent is dimethyl sulfoxide; the inert gas is any one of nitrogen, helium, neon and argon.
[0021] Another object of the present invention is to provide a method for preparing the bio-based polyurethane composite material, comprising the following steps: mixing the raw materials uniformly by weight to obtain a mixture, adding the mixture to a twin-screw extruder for melt extrusion to obtain the bio-based polyurethane composite material.
[0022] Preferably, the extrusion temperature of the twin-screw extruder is 160-180° C., the screw aspect ratio is 55:1, and the screw speed is 210-280 rpm.
[0023] Due to the application of the above technical solution, the present invention has the following beneficial effects:
[0024] (1) The preparation method of the bio-based polyurethane composite material disclosed in the present invention only requires the raw materials to be uniformly mixed and then melt-extruded. The process is simple, the operation and control are convenient, the dependence on equipment is low, the capital investment is small, the energy consumption is low, the preparation efficiency and the qualified rate of finished products are high, and it is suitable for continuous large-scale production and has a high value for promotion and application.
[0025] (2) The bio-based polyurethane composite material disclosed in the present invention comprises the following raw materials in parts by weight: 100 parts of phosphaphenanthrylbenzotriazole-modified bio-based polyurethane, 10-20 parts of biomass fiber, 1-3 parts of coupling agent, 3-5 parts of isocyanoethyl methacrylate, 2-4 parts of tris(2-acryloyloxyethyl)isocyanurate, 0.8-1.2 parts of initiator, 0.8-1.2 parts of catalyst A, 0.3-0.6 parts of antioxidant, and 0.7-1 parts of plasticizer; the phosphaphenanthrylbenzotriazole-modified bio-based polyurethane comprises the following monomer-introduced structural units: 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthryl-10-oxide, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, bio-based diol, and bio-based diisocyanate. Through the mutual cooperation between the raw materials, the composite material has good mechanical properties, excellent flame retardancy and heat aging resistance.
[0026] (3) The bio-based polyurethane composite material disclosed in the present invention, the phosphaphenanthryl benzotriazole-modified bio-based polyurethane includes the following monomer-introduced structural units: 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, bio-based diols, and bio-based diisocyanates; the use of raw materials such as bio-based diols, bio-based diisocyanates and biomass fibers makes the composite material degradable and safe and environmentally friendly to use; at the same time, the introduced structures such as phosphaphenanthrene, benzotriazole, polyurethane, etc., under the multiple effects of electronic effect, steric effect and conjugation effect, make the manufactured material product have good mechanical properties, flame retardancy and heat aging resistance. In the preparation process of phosphaphenanthrylbenzotriazole-modified bio-based polyurethane, 1,3-propylene glycol is used as a reaction chain terminator, so that the molecular chain end is hydroxyl, which can react chemically with the isocyanate group on isocyanoethyl methacrylate. At the same time, tri(2-acryloyloxyethyl)isocyanurate and isocyanoethyl methacrylate containing unsaturated olefinic bonds can copolymerize to form an interpenetrating network cross-linked structure, further improving the mechanical properties, flame retardancy and heat aging resistance of the manufactured material products. DETAILED DESCRIPTION
[0027] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art may think of other obvious variations.
[0028] Example 1
[0029] A bio-based polyurethane composite material is prepared from the following raw materials in parts by weight: 100 parts of phosphaphenanthrylbenzotriazole-modified bio-based polyurethane, 10 parts of biomass fiber, 1 part of coupling agent, 3 parts of isocyanoethyl methacrylate, 2 parts of tris(2-acryloyloxyethyl)isocyanurate, 0.8 parts of initiator, 0.8 parts of catalyst A, 0.3 parts of antioxidant, and 0.7 parts of plasticizer; the phosphaphenanthrylbenzotriazole-modified bio-based polyurethane comprises structural units introduced by the following monomers: 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthryl-10-oxide, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, bio-based diol, and bio-based diisocyanate.
[0030] The plasticizer is epoxidized soybean oil; the antioxidant is antioxidant 1010; the catalyst A is dibutyltin dilaurate; the initiator is a mixture of diisopropylbenzene peroxide, benzoyl peroxide, and 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane in a mass ratio of 1:0.8:1; the coupling agent is silane coupling agent KH550; the biomass fiber is bamboo pulp fiber; the average diameter of the biomass fiber is 3 μm, and the aspect ratio is 20:1.
[0031] The preparation method of the phosphaphenanthrylbenzotriazole-modified bio-based polyurethane comprises the following steps: adding 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthryl-10-oxide, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, bio-based diol, bio-based diisocyanate and dibutyltin dilaurate to a high boiling point solvent, stirring and reacting for 4 hours at 76°C in an inert gas atmosphere, then heating to 95°C and continuing to stir and react for 8 hours, then adding a reaction chain terminator, continuing to stir and react for 0.1h, precipitating in water after the reaction is completed, washing the precipitated polymer with ethanol for 3 times, and finally removing the residual solvent by rotary evaporation to obtain the phosphaphenanthrylbenzotriazole-modified bio-based polyurethane. The functional thermoplastic polyurethane is prepared by mixing 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, bio-based diol, bio-based diisocyanate, dibutyltin dilaurate, high boiling point solvent and reaction chain terminator in a molar ratio of 0.1:0.1:0.8:1:0.9:11:0.035; the bio-based diol is 1,3-propylene glycol; the bio-based diisocyanate is 1,5-pentanediisocyanate; the reaction chain terminator is 1,3-propylene glycol; the high boiling point solvent is dimethyl sulfoxide; the inert gas is nitrogen; and the M of the functional thermoplastic polyurethane is measured by GPC test. n =14517 g / mol, M W / M n =1.377; through elemental analysis, infrared analysis and weight change calculation, the molar ratio of the structural units introduced by 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, bio-based diol and bio-based diisocyanate in the phosphaphenanthrene-benzotriazole-modified bio-based polyurethane is the same as the theoretical value.
[0032] A preparation method of the bio-based polyurethane composite material comprises the following steps: uniformly mixing the raw materials according to weight parts to obtain a mixture, adding the mixture into a twin-screw extruder for melt extrusion to obtain the bio-based polyurethane composite material; the extrusion temperature of the twin-screw extruder is 160°C, the screw aspect ratio is 55:1, and the screw speed is 210rpm.
[0033] Example 2
[0034] A bio-based polyurethane composite material is prepared from the following raw materials in parts by weight: 100 parts of phosphaphenanthrylbenzotriazole-modified bio-based polyurethane, 13 parts of biomass fiber, 1.5 parts of coupling agent, 3.5 parts of isocyanoethyl methacrylate, 2.5 parts of tris(2-acryloyloxyethyl)isocyanurate, 0.9 parts of initiator, 0.9 parts of catalyst A, 0.4 parts of antioxidant, and 0.8 parts of plasticizer; the phosphaphenanthrylbenzotriazole-modified bio-based polyurethane comprises structural units introduced by the following monomers: 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthryl-10-oxide, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, bio-based diol, and bio-based diisocyanate.
[0035] The plasticizer is epoxidized soybean oil; the antioxidant is antioxidant 168; the catalyst A is dibutyltin dilaurate; the initiator is a mixture of diisopropylbenzene peroxide, benzoyl peroxide, and 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane in a mass ratio of 1:0.9:1.2; the coupling agent is silane coupling agent KH560; the biomass fiber is hemp pulp fiber; the average diameter of the biomass fiber is 5 μm, and the aspect ratio is 23:1.
[0036] The preparation method of the phosphaphenanthryl benzotriazole-modified bio-based polyurethane comprises the following steps: adding 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthryl-10-oxide, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, bio-based diol, bio-based diisocyanate and dibutyltin dilaurate to a high boiling point solvent, stirring and reacting at 80°C for 4.5 hours in an inert gas atmosphere, then heating to 96°C and continuing to stir and react for 9 hours, then adding a reaction chain terminator, continuing to stir and react for 0.15 hours, precipitating in water after the reaction is completed, washing the precipitated polymer with ethanol for 4 times, and finally removing the residual solvent by rotary evaporation to obtain Phosphaphenanthrylbenzotriazole-modified bio-based polyurethane; the molar ratio of the 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, bio-based diol, bio-based diisocyanate, dibutyltin dilaurate, high boiling point solvent, and reaction chain terminator is 0.1:0.1:0.8:1:0.9:11:0.035; the bio-based diol is 1,4-butanediol; the bio-based diisocyanate is L-lysine diisocyanate; the reaction chain terminator is 1,3-propylene glycol; the high boiling point solvent is dimethyl sulfoxide; and the inert gas is helium.
[0037] A preparation method of the bio-based polyurethane composite material comprises the following steps: uniformly mixing the raw materials by weight to obtain a mixture, adding the mixture into a twin-screw extruder for melt extrusion to obtain a bio-based polyurethane composite material; the extrusion temperature of the twin-screw extruder is 165°C, the screw aspect ratio is 55:1, and the screw speed is 230rpm.
[0038] Example 3
[0039] A bio-based polyurethane composite material is prepared from the following raw materials in parts by weight: 100 parts of phosphaphenanthrylbenzotriazole-modified bio-based polyurethane, 15 parts of biomass fiber, 2 parts of coupling agent, 4 parts of isocyanoethyl methacrylate, 3 parts of tris(2-acryloyloxyethyl)isocyanurate, 1 part of initiator, 1 part of catalyst A, 0.45 parts of antioxidant, and 0.85 parts of plasticizer; the phosphaphenanthrylbenzotriazole-modified bio-based polyurethane comprises structural units introduced by the following monomers: 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthryl-10-oxide, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, bio-based diol, and bio-based diisocyanate.
[0040] The plasticizer is epoxidized soybean oil; the antioxidant is antioxidant 1010; the catalyst A is dibutyltin dilaurate; the initiator is a mixture of diisopropylbenzene peroxide, benzoyl peroxide, and 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane in a mass ratio of 1:1:1.5; the coupling agent is silane coupling agent KH570; the biomass fiber is bamboo pulp fiber; the average diameter of the biomass fiber is 6 μm, and the aspect ratio is 25:1.
[0041] The preparation method of the phosphaphenanthryl benzotriazole-modified bio-based polyurethane comprises the following steps: adding 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthryl-10-oxide, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, bio-based diol, bio-based diisocyanate and dibutyltin dilaurate to a high boiling point solvent, stirring and reacting for 5 hours at 84°C in an inert gas atmosphere, then heating to 97°C and continuing stirring and reacting for 10 hours, then adding a reaction chain terminator, continuing stirring and reacting for 0.2 hours, precipitating in water after the reaction is completed, washing the precipitated polymer with ethanol for 5 times, and finally removing the residual solvent by rotary evaporation to obtain the phosphaphenanthryl benzotriazole-modified bio-based polyurethane. The invention discloses a bio-based polyurethane modified with benzotriazole; the molar ratio of the 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, bio-based diol, bio-based diisocyanate, dibutyltin dilaurate, high boiling point solvent and reaction chain terminator is 0.1:0.1:0.8:1:1:13:0.04; the bio-based diol is NX-9212 cashew nut shell oil diol; the bio-based diisocyanate is L-lysine diisocyanate; the reaction chain terminator is 1,3-propylene glycol; the high boiling point solvent is dimethyl sulfoxide; and the inert gas is neon.
[0042] A preparation method of the bio-based polyurethane composite material comprises the following steps: uniformly mixing the raw materials according to weight to obtain a mixture, adding the mixture into a twin-screw extruder for melt extrusion to obtain the bio-based polyurethane composite material; the extrusion temperature of the twin-screw extruder is 170°C, the screw aspect ratio is 55:1, and the screw speed is 260rpm.
[0043] Example 4
[0044] A bio-based polyurethane composite material is prepared from the following raw materials in parts by weight: 100 parts of phosphaphenanthrylbenzotriazole-modified bio-based polyurethane, 18 parts of biomass fiber, 2.5 parts of coupling agent, 4.5 parts of isocyanoethyl methacrylate, 3.5 parts of tris(2-acryloyloxyethyl)isocyanurate, 1.1 parts of initiator, 1.1 parts of catalyst A, 0.55 parts of antioxidant, and 0.95 parts of plasticizer; the phosphaphenanthrylbenzotriazole-modified bio-based polyurethane comprises structural units introduced by the following monomers: 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthryl-10-oxide, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, bio-based diol, and bio-based diisocyanate.
[0045] The plasticizer is epoxidized soybean oil; the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 3:2; the catalyst A is dibutyltin dilaurate; the initiator is a mixture of diisopropylbenzene peroxide, benzoyl peroxide and 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane in a mass ratio of 1:1.1:1.8; the coupling agent is a mixture of silane coupling agent KH550, silane coupling agent KH560 and silane coupling agent KH570 in a mass ratio of 1:2:3; the biomass fiber is a mixture of bamboo pulp fiber and hemp pulp fiber in a mass ratio of 1:3; the average diameter of the biomass fiber is 8 μm, and the aspect ratio is 28:1.
[0046] The preparation method of the phosphaphenanthryl benzotriazole-modified bio-based polyurethane comprises the following steps: adding 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, bio-based diol, bio-based diisocyanate and dibutyltin dilaurate to a high boiling point solvent, stirring and reacting at 88° C. for 5.5 hours in an inert gas atmosphere, then heating to 97° C. and continuing stirring and reacting for 11 hours, then adding a reaction chain terminator, continuing stirring and reacting for 0.25 hours, and after the reaction is completed The product was precipitated in water, and the precipitated polymer was washed with ethanol for 6 times. Finally, the residual solvent was removed by rotary evaporation to obtain a phosphaphenanthrylbenzotriazole-modified bio-based polyurethane; the molar ratio of the 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, bio-based diol, bio-based diisocyanate, dibutyltin dilaurate, high boiling point solvent, and reaction chain terminator was 0.1:0.1:0.8:1:1.1:14:0.045; the bio-based diol was PO3G H500 polytrimethylene ether glycol; the bio-based diisocyanate was 1,5-pentanediisocyanate; the reaction chain terminator was 1,3-propylene glycol; the high boiling point solvent was dimethyl sulfoxide; and the inert gas was argon.
[0047] A preparation method of the bio-based polyurethane composite material comprises the following steps: uniformly mixing the raw materials by weight to obtain a mixture, adding the mixture into a twin-screw extruder for melt extrusion to obtain a bio-based polyurethane composite material; the extrusion temperature of the twin-screw extruder is 175°C, the screw aspect ratio is 55:1, and the screw speed is 270rpm.
[0048] Example 5
[0049] A bio-based polyurethane composite material is prepared from the following raw materials in parts by weight: 100 parts of phosphaphenanthrylbenzotriazole-modified bio-based polyurethane, 20 parts of biomass fiber, 3 parts of coupling agent, 5 parts of isocyanoethyl methacrylate, 4 parts of tris(2-acryloyloxyethyl)isocyanurate, 1.2 parts of initiator, 1.2 parts of catalyst A, 0.6 parts of antioxidant, and 1 part of plasticizer; the phosphaphenanthrylbenzotriazole-modified bio-based polyurethane comprises structural units introduced by the following monomers: 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthryl-10-oxide, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, bio-based diol, and bio-based diisocyanate.
[0050] The plasticizer is epoxidized soybean oil; the antioxidant is antioxidant 1010; the catalyst A is dibutyltin dilaurate; the initiator is a mixture of diisopropylbenzene peroxide, benzoyl peroxide, and 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane in a mass ratio of 1:1.2:2; the coupling agent is silane coupling agent KH550; the biomass fiber is bamboo pulp fiber; the average diameter of the biomass fiber is 9 μm, and the aspect ratio is 30:1.
[0051] The preparation method of the phosphaphenanthryl benzotriazole-modified bio-based polyurethane comprises the following steps: adding 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthryl-10-oxide, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, bio-based diol, bio-based diisocyanate and dibutyltin dilaurate to a high boiling point solvent, stirring and reacting at 90°C for 6 hours in an inert gas atmosphere, then heating to 98°C and continuing to stir and react for 12 hours, then adding a reaction chain terminator, continuing to stir and react for 0.3 hours, precipitating in water after the reaction is completed, washing the precipitated polymer with ethanol for 6 times, and finally removing the residual solvent by rotary evaporation to obtain the phosphaphenanthryl benzotriazole-modified bio-based polyurethane. Bio-based polyurethane modified by phenanthroline benzotriazole; the molar ratio of the 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, bio-based diol, bio-based diisocyanate, dibutyltin dilaurate, high boiling point solvent, and reaction chain terminator is 0.1:0.1:0.8:1:1.2:15:0.05; the bio-based diol is 1,3-propylene glycol; the bio-based diisocyanate is L-lysine diisocyanate; the reaction chain terminator is 1,3-propylene glycol; the high boiling point solvent is dimethyl sulfoxide; and the inert gas is nitrogen.
[0052] A preparation method of the bio-based polyurethane composite material comprises the following steps: uniformly mixing the raw materials according to weight to obtain a mixture, adding the mixture into a twin-screw extruder for melt extrusion to obtain the bio-based polyurethane composite material; the extrusion temperature of the twin-screw extruder is 180°C, the screw aspect ratio is 55:1, and the screw speed is 280rpm.
[0053] Comparative Example 1
[0054] A bio-based polyurethane composite material and a preparation method thereof are basically the same as those in Example 1, except that a bio-based diol is used instead of 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide.
[0055] Comparative Example 2
[0056] A bio-based polyurethane composite material and a preparation method thereof are basically the same as those in Example 1, except that bio-based diol is used instead of N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine.
[0057] In order to further illustrate the beneficial technical effects of the bio-based polyurethane composite materials involved in each embodiment of the present invention, relevant performance tests were performed on the bio-based polyurethane composite materials involved in Examples 1-5 and Comparative Examples 1-2; the test methods are as follows:
[0058] (1) Tensile strength: Refer to GB / T 1040.1-2018 for tensile strength test.
[0059] (2) Flame retardancy: tested in accordance with UL94 standard.
[0060] (3) Heat aging resistance: The products of each example were placed in hot air at 85°C for artificial accelerated aging for 168 hours. After cooling to room temperature, the tensile strength was measured again according to method (1). The heat aging resistance was measured by the retention rate of tensile strength. The larger the value, the better the heat aging resistance.
[0061] As can be seen from Table 1, the bio-based polyurethane composite materials involved in each embodiment of the present invention have better mechanical properties, flame retardant properties and heat aging resistance than the comparative example products, and the combined use of 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide and N-[(4-methyl-1H-benzotriazol-1-yl)methyl]diethanolamine is beneficial to improving the above properties.
[0062] Table 1
[0063] project Tensile Strength Heat aging resistance Flame retardant unit MPa % class Example 1 52.8 99.85 V-0 Example 2 53.6 99.90 V-0 Example 3 54.7 99.93 V-0 Example 4 55.3 99.95 V-0 Example 5 56.2 99.99 V-0 Comparative Example 1 48.5 98.18 V-1 Comparative Example 2 47.3 98.51 V-1
[0064] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the contents of the present invention and implement them accordingly. They cannot be used to limit the protection scope of the present invention. All equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A bio-based polyurethane composite material, characterized in that: The invention comprises the following raw materials in parts by weight: 100 parts of phosphaphenanthrylbenzotriazole-modified bio-based polyurethane, 10-20 parts of biomass fiber, 1-3 parts of coupling agent, 3-5 parts of isocyanoethyl methacrylate, 2-4 parts of tris(2-acryloyloxyethyl)isocyanurate, 0.8-1.2 parts of initiator, 0.8-1.2 parts of catalyst A, 0.3-0.6 parts of antioxidant and 0.7-1 parts of plasticizer; the phosphaphenanthrylbenzotriazole-modified bio-based polyurethane comprises structural units introduced by the following monomers: 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthryl-10-oxide, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, bio-based diol and bio-based diisocyanate.
2. The bio-based polyurethane composite material according to claim 1, characterized in that: The plasticizer is epoxidized soybean oil; the antioxidant is at least one of antioxidant 1010 and antioxidant 168.
3. The bio-based polyurethane composite material according to claim 1, characterized in that: The catalyst A is dibutyltin dilaurate; the initiator is a mixture of diisopropylbenzene peroxide, benzoyl peroxide and 2,5-dimethyl-2,5-di-tert-butylhexane peroxide in a mass ratio of 1:(0.8-1.2):(1-2).
4. The bio-based polyurethane composite material according to claim 1, characterized in that: The coupling agent is at least one of silane coupling agent KH550, silane coupling agent KH560 and silane coupling agent KH570.
5. The bio-based polyurethane composite material according to claim 1, characterized in that: The biomass fiber is at least one of bamboo pulp fiber and hemp pulp fiber; the average diameter of the biomass fiber is 3-9 μm, and the aspect ratio is (20-30):
1.
6. The bio-based polyurethane composite material according to claim 1, characterized in that: The preparation method of the phosphaphenanthrylbenzotriazole-modified bio-based polyurethane comprises the following steps: adding 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthryl-10-oxide, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, bio-based diol, bio-based diisocyanate and dibutyltin dilaurate to a high boiling point solvent, stirring and reacting for 4-6 hours at 76-90° C. in an inert gas atmosphere, then heating to 95-98° C. and continuing to stir and react for 8-12 hours, then adding a reaction chain terminator, continuing to stir and react for 0.1-0.3 hours, precipitating in water after the reaction is completed, washing the precipitated polymer with ethanol for 3-6 times, and finally removing the residual solvent by rotary evaporation to obtain the phosphaphenanthrylbenzotriazole-modified bio-based polyurethane.
7. The bio-based polyurethane composite material according to claim 6, characterized in that: The molar ratio of the 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, bio-based diol, bio-based diisocyanate, dibutyltin dilaurate, high boiling point solvent, and reaction chain terminator is 0.1:0.1:0.8:1:(0.8-1.2):(9-15):(0.03-0.05).
8. The bio-based polyurethane composite material according to claim 6, characterized in that: The bio-based diol is any one of 1,3-propylene glycol, 1,4-butanediol, NX-9212 cashew nut shell oil diol, and PO3G H500 polytrimethylene ether glycol; the bio-based diisocyanate is any one of 1,5-pentane diisocyanate and L-lysine diisocyanate; the reaction chain terminator is 1,3-propylene glycol; the high boiling point solvent is dimethyl sulfoxide; and the inert gas is any one of nitrogen, helium, neon, and argon.
9. A method for preparing the bio-based polyurethane composite material according to any one of claims 1 to 8, characterized in that: The method comprises the following steps: uniformly mixing the raw materials according to weight to obtain a mixture, adding the mixture into a twin-screw extruder for melt extrusion, and obtaining a bio-based polyurethane composite material.
10. The method for preparing the bio-based polyurethane composite material according to claim 9, characterized in that: The extrusion temperature of the twin-screw extruder is 160-180° C., the screw aspect ratio is 55:1, and the screw speed is 210-280 rpm.
Citation Information
Patent Citations
Corrosion-resistant sound-transmission waterproof membrane for wearable equipment and preparation method of corrosion-resistant sound-transmission waterproof membrane
CN118185289A
Breathable polyurethane foam sponge and preparation method thereof
CN118834521A
Preparation method of composite sound-absorbing material for motor home
CN119433829A
Cited By
Preparation method of composite sound-absorbing material for motor home
CN119433829A