Piezoelectric photocatalytic fog seal pavement material as well as preparation method and application thereof
By introducing piezoelectric effect into photocatalytic pavement materials, using piezoelectric photocatalysts combined with g-C3N4 and BaTiO3, the problems of low degradation efficiency and easy catalyst deactivation in the prior art are solved, and efficient and zero carbon emissions are achieved Car exhaust degradation effect.
Patent Information
- Application Number
- CN202411100755.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-22
AI Technical Summary
The existing photocatalytic pavement materials are not effective in degrading automobile exhaust efficiency, low light energy utilization rate, and easy catalyst deactivation, resulting in the inability to effectively degrade pollutants generated during transportation operations.
Using piezoelectric photocatalytic atomized layer pavement material, the piezoelectric photocatalyst with core-shell structure is formed by compounding g-C3N4 and BaTiO3, and combined with emulsified asphalt and fine aggregates, and synergistically catalyzed with solar light and mechanical energy to improve electrons. and hole separation efficiency, enhancing catalyst activity and degradation efficiency.
The ability to effectively degrade automobile exhausts under the lack of light conditions has been achieved, the degradation efficiency has been increased by 1.62 to 2.34 times, the catalyst activity has been significantly improved, and the material has zero carbon emissions, low energy consumption, and green characteristics, which are suitable for road surface applications.
Smart Images

Figure CN118994929A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of pavement materials, and in particular to a piezoelectric photocatalytic mist seal pavement material and a preparation method and application thereof. Background Art
[0002] Photocatalytic pavement materials are green, low energy consumption, and low cost, and can effectively degrade automobile exhaust generated during traffic operations. Automobile exhaust is the main pollutant in the current vehicle driving process. Its main components include: carbon monoxide, nitrogen oxides, hydrocarbons, smoke particles, odor, etc. Among them, nitrogen oxides will form photochemical smog after combining with the atmosphere, which will cause irreversible damage to human health and the environment.
[0003] In order to solve the above technical problems, technicians in this field have proposed a variety of technical solutions. For example, the prior art CN107473633A proposes to add TiO2 instead of mineral powder in equal proportion on the basis of traditional asphalt mixture to give asphalt mixture the property of photocatalytic degradation of exhaust gas. Although this method can improve the photocatalytic degradation performance of asphalt mixture to a certain extent, the effective catalyst distributed on the surface of asphalt mixture obtained by this method is less, and sunlight can only irradiate the surface, and the internal catalyst cannot play a role, resulting in extremely low utilization of light energy and catalyst.
[0004] The prior art CN110777606A proposes to combine nano-TiO2 with a fog seal material to encapsulate the catalyst in the fog seal to increase the content of effective catalyst on the surface of the photocatalytic pavement material. Although this method can improve the utilization efficiency of light energy and the contact with pollutants to a certain extent, its catalyst activity is difficult to effectively improve the efficiency of exhaust gas degradation.
[0005] Prior art CN108822564A proposes to improve the degradation efficiency by compounding g-C3N4 with TiO2 to form a photocatalyst and spraying the photocatalyst on the surface of the emulsified asphalt that is about to be demulsified. Although this method can improve the photocatalytic effect of the material to a certain extent, the electron-hole recombination rate of the catalyst after light excitation is still very high, and the photocatalytic effect cannot be effectively exerted; and the photocatalytic degradation of exhaust gas cannot be exerted in the absence of light. Moreover, it is easy to be worn and lose activity when sprayed only on the surface of the emulsified asphalt, making it difficult for the material to stably exert the photocatalytic degradation of exhaust gas.
[0006] To this end, the present invention provides a piezoelectric photocatalytic mist seal pavement material and a preparation method and application thereof. Summary of the invention
[0007] In view of the shortcomings of the prior art such as poor degradation efficiency, low light energy utilization, and easy deactivation of catalysts, the purpose of the present invention is to provide a piezoelectric photocatalytic mist seal pavement material and a preparation method and application thereof.
[0008] The piezoelectric photocatalytic mist seal pavement material and its preparation method and application are realized by the following technical solutions:
[0009] The first object of the present invention is to provide a piezoelectric photocatalytic mist seal pavement material, the raw materials for its preparation are composed of the following components in parts by weight:
[0010] 100 parts of emulsified asphalt, 1 to 5 parts of piezoelectric photocatalyst, 2 to 10 parts of water and 20 parts of fine aggregate.
[0011] It should be noted that the present invention takes into account that piezoelectric photocatalytic materials can not only utilize the light energy provided by sunlight, but also absorb the mechanical energy generated by external loads to cooperate with photocatalysis, form a built-in electric field inside the catalyst, greatly improve the separation efficiency of electrons and holes after light excitation, and cause directional migration, thereby improving the degradation efficiency and increasing the activity of the catalyst. The fog seal pavement material is applied to the road surface and is the first contactor to remove automobile exhaust. It has the characteristics of large contact area and high contact concentration, and is an ideal carrier for piezoelectric photocatalytic materials to degrade exhaust gas. Therefore, in some preferred embodiments of the present invention, a piezoelectric photocatalyst with a core-shell structure is formed by compounding g-C3N4 and BaTiO3, and a piezoelectric photocatalyst with a BaTiO3 core and a g-C3N4 shell is combined with a fog seal pavement material, and compounded with water and fine aggregate to form a piezoelectric photocatalytic fog seal pavement material, so that it can be applied to the road surface, and does not require any mechanical force from the outside. It absorbs the additional mechanical energy generated by the driving load to coordinate photocatalysis, and gives full play to the piezoelectric coordinated photocatalytic efficient exhaust degradation mechanism, which can degrade automobile exhaust in real time and efficiently, and also has the advantage of zero carbon emissions.
[0012] In order to ensure that the piezoelectric photocatalyst used can achieve the above-mentioned effects, in some preferred embodiments of the present invention, the piezoelectric photocatalyst is prepared by the following steps:
[0013] 1) Mix g-C3N4 precursor and BaTiO3 in water to obtain a suspension.
[0014] Wherein, the g-C3N4 precursor is any one of urea, dicyandiamide and melamine.
[0015] The present invention takes into account that the calcination of dicyandiamide will produce highly toxic fumes of cyanide and nitrogen oxides. The main gases produced by the calcination of melamine include ammonia, nitrogen, cyanide and nitric oxide. The full calcination of urea mainly produces ammonia with less toxicity, and the cost of urea is very low relative to the cost, followed by melamine, and the cost of dicyandiamide is relatively high. Therefore, based on the comprehensive consideration of green environmental protection and cost, in some preferred embodiments of the present invention, urea is preferably used as a g-C3N4 precursor.
[0016] In some preferred embodiments of the present invention, the mass ratio of the g-C3N4 precursor to BaTiO3 is 100g:0.5g~3g to meet the synergy of piezoelectricity and photocatalysis. When the amount of BT is too small, the piezoelectric effect is not enough to promote the photocatalytic effect; when the amount of BT is too large, the active sites of the highly active photocatalytic material are reduced and the photocatalytic effect is weakened. In some preferred embodiments of the present invention, the amount ratio of water to BaTiO3 is 500mL:1g~5g.
[0017] 2) performing an evaporation treatment on the suspension to evaporate the water in the suspension to obtain a solid component.
[0018] In some preferred embodiments of the present invention, the evaporation treatment is achieved by heating under stirring conditions, and the heating temperature is 70° C. to 90° C., and the heating is performed until the water is completely evaporated.
[0019] 3) The solid component is calcined at 500° C. to 600° C. and ground to obtain the piezoelectric photocatalyst.
[0020] In some preferred embodiments of the present invention, the calcination treatment time is 1 h to 3 h.
[0021] In some preferred embodiments of the present invention, the fine aggregate consists of the following components in mass percentage:
[0022] The first quartz sand is 95% to 100%, the second quartz sand is 5% to 10%, the third quartz sand is 0 to 5% and the fourth quartz sand is 0 to 1%, totaling 100%.
[0023] Among them, the particle size of the first quartz sand is 0.31mm~0.6mm; the particle size of the second quartz sand is 0.16mm~0.3mm; the particle size of the third quartz sand is 0.08mm~0.15mm; the particle size of the fourth quartz sand is ≤0.075mm, so that quartz sands of various sizes are compounded and used together as fine aggregates to meet the anti-skid and durability requirements of the road surface.
[0024] The second object of the present invention is to provide a method for preparing the above-mentioned piezoelectric photocatalytic mist seal pavement material, comprising:
[0025] Step 1: according to the ratio of the piezoelectric photocatalytic mist seal pavement material, weigh the corresponding mass of each preparation raw material and set aside.
[0026] It should be noted that, according to the ratio of 100 parts of emulsified asphalt, 1 part to 5 parts of piezoelectric photocatalyst, 2 parts to 10 parts of water and 20 parts of fine aggregate, the corresponding masses of various preparation raw materials are weighed.
[0027] Step 2: Disperse the weighed piezoelectric photocatalyst in water to obtain a piezoelectric photocatalyst dispersion.
[0028] It should be noted that, during the research process, the present invention found that due to the large specific surface area and small density of the catalyst, if the catalyst is directly added to the emulsified asphalt, agglomeration is likely to occur, resulting in difficulty in mixing the various components evenly. Therefore, the present invention preferably disperses the piezoelectric photocatalyst in water first to form a uniformly dispersed piezoelectric photocatalyst dispersion, and then mixes it with fine aggregate and emulsified asphalt to ensure that the catalyst can be evenly mixed with other components.
[0029] In some preferred embodiments of the present invention, the weighed piezoelectric photocatalyst is dispersed in water by ultrasound; and the ultrasound time is 10 min to 20 min to ensure that the piezoelectric photocatalyst can be evenly dispersed in water to form a piezoelectric photocatalyst dispersion with uniform components.
[0030] Step 3: Disperse the weighed fine aggregate and emulsified asphalt in the piezoelectric photocatalyst dispersion, stir and mix well, and obtain a piezoelectric photocatalytic mist seal pavement material.
[0031] It should be noted that the present invention does not limit specific stirring process parameters, and stirring is sufficient until the mixture is completely mixed.
[0032] The third object of the present invention is to provide an application of the above-mentioned piezoelectric photocatalytic mist seal pavement material in the degradation of exhaust gas. It should be noted that the piezoelectric photocatalytic mist seal pavement material is laid on the road surface, and after curing, a piezoelectric photocatalytic mist seal pavement layer is formed on the road surface. Under the synergistic effect of vehicle load and light, the piezoelectric photocatalytic mist seal pavement layer degrades automobile exhaust gas in real time.
[0033] In some preferred embodiments of the present invention, when the piezoelectric photocatalytic mist seal pavement material is sprayed on the pavement, the spraying amount is 0.6 kg / m 2 ~1kg / m 2The present invention uses a smaller spraying amount. By spraying a thin layer on the asphalt pavement, the exhaust gas can be degraded at the first time of discharge and has a certain durability. Compared with other forms such as roadbed mixing, micro-surfacing and ultra-thin covering, the present invention has the characteristics of simple material preparation, high catalyst activity, utilization of vehicle load, high effective catalyst content, efficient exhaust gas degradation, low paving cost, zero carbon emission, low energy consumption, green and so on, and has a wide range of application value.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] The present invention mixes g-C3N4 precursor and BaTiO3 in water, and then evaporates and calcines them to form a piezoelectric photocatalyst with a core-shell structure. The electrons and holes in the piezoelectric photocatalyst of the present invention are separated to generate free radicals required for the redox reaction. The vibration can force BT to exert its piezoelectric properties, forming a built-in electric field inside the catalyst to promote the separation of electrons and holes and directional migration. Under the synergistic effect of light and vibration, the efficiency of degrading automobile exhaust is 1.62 and 2.34 times that of light alone and vibration alone, respectively, and 2.19 times that of the g-C3N4 catalyst, indicating that its activity and degradation effect are better than other photocatalysts under the same conditions.
[0036] The present invention utilizes the piezoelectric photocatalyst to efficiently degrade automobile exhaust gas, and combines it with the mist seal layer to prepare a piezoelectric photocatalytic mist seal layer pavement material with the ability to degrade automobile exhaust gas. Just spray a thin layer on the asphalt pavement, and the exhaust gas can be degraded as soon as it is discharged, and it has a certain durability.
[0037] The piezoelectric photocatalytic mist seal pavement material of the present invention can not only utilize solar energy, but also fully absorb the mechanical energy generated by the traffic load on the road surface, and exert the piezoelectric synergistic photocatalytic effect to efficiently degrade automobile exhaust, so that the degradation effect and activity are greatly improved. The piezoelectric photocatalytic mist seal pavement material of the present invention is relatively flexible in the way of degrading exhaust gas, without specific temperature restrictions, and in special scenarios where there is a lack of light, it can also stimulate its piezoelectric effect through the traffic load to produce piezoelectric catalytic degradation of automobile exhaust. The piezoelectric photocatalytic mist seal pavement material of the present invention can fully utilize the mechanical force generated by the traffic load to synergistically photocatalyze and degrade automobile exhaust in real time without the need for any external mechanical force from the outside world, which belongs to a zero-carbon emission, green degradation of automobile exhaust technology. And the piezoelectric photocatalytic mist seal pavement material of the present invention, under the synergistic effect of vehicle load and light, has an efficiency of degrading automobile exhaust that is 1.48 and 2.38 times that of only light and only traffic load.
[0038] Compared with other forms such as roadbed admixture, micro-surfacing and ultra-thin covering, the present invention has the characteristics of simple material preparation, high catalyst activity, utilization of vehicle load, high effective catalyst content, efficient degradation of exhaust gas, low paving cost, zero carbon emission, low energy consumption, green and has wide application value.
[0039] The raw materials for the preparation of the invention are easy to obtain and the preparation process is simple, which is beneficial to engineering practice. In actual engineering, the material can be mixed and prepared on site or prefabricated in a factory, and the mixing method is simple, fast and flexible. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 This is the scanning electron microscope image of g-C3N4 in Comparative Example 1.
[0041] Figure 2 This is a scanning electron microscope image of the CNBT prepared in the present invention.
[0042] Figure 3 XRD patterns of g-C3N4, BT and CNBT.
[0043] Figure 4 The luminescence spectra of g-C3N4, BT and CNBT catalysts.
[0044] Figure 5 Ultraviolet absorption spectra of g-C3N4, BT and CNBT catalysts.
[0045] Figure 6 The results of the CNBT catalyst degradation efficiency test under different conditions are shown.
[0046] Figure 7 These are the test results of the degradation efficiency of automobile exhaust gas of the piezoelectric photocatalytic mist seal pavement materials of Examples 1 to 5.
[0047] Figure 8 These are the test results of the efficiency of the piezoelectric photocatalytic mist seal layer of Example 2 in degrading automobile exhaust gas under different conditions.
[0048] Fig. 9 These are the test results of the efficiency of the piezoelectric photocatalytic mist seal layer of Example 2 in degrading automobile exhaust gas at different spraying rates.
[0049] Fig.10 This is the degradation efficiency cycle test result of automobile exhaust gas of the piezoelectric photocatalytic mist seal pavement material of Example 2.
[0050] Fig.11 These are the test results of the degradation efficiency of automobile exhaust gas by the piezoelectric photocatalytic mist seal pavement material of Example 2 and the photocatalytic mist seal pavement material of Comparative Example 1. DETAILED DESCRIPTION
[0051] The technical solutions in the embodiments of the present invention will be described clearly and completely below. For ease of description, in the following embodiments of the present invention, BT will be used to represent BaTiO3.
[0052] It should be noted that the piezoelectric photocatalysts used in the following Examples 1 to 3 of the present invention are all prepared by the following steps:
[0053] 1) Using urea as the precursor of g-C3N4, 100 g urea and 1 g BT were put into 500 ml deionized water to prepare a suspension.
[0054] 2) Place the suspension in a hydrothermal magnetic stirrer and stir it at 80°C until all the water in the suspension evaporates.
[0055] 3) The evaporated solid was placed in a muffle furnace and calcined at 550° C. for 2 h, and ground. The obtained product was a piezoelectric photocatalyst, which was labeled as CNBT.
[0056] It should also be noted that the following Examples 1 to 5 of the present invention and Comparative Example 1 all use the following mass percentage components of fine aggregate to prepare piezoelectric photocatalytic mist seal pavement materials:
[0057] The first quartz sand is 93%, the second quartz sand is 4%, the third quartz sand is 2% and the fourth quartz sand is 1%, totaling 100%.
[0058] Among them, the particle size of the first quartz sand is 0.31mm-0.6mm; the particle size of the second quartz sand is 0.16mm-0.3mm; the particle size of the third quartz sand is 0.08mm-0.15mm; and the particle size of the fourth quartz sand is ≤0.075mm.
[0059] Example 1
[0060] This embodiment provides a piezoelectric photocatalytic mist seal pavement material, which is prepared by the following steps:
[0061] Step 1, weigh 0.8 g of CNBT, disperse it in 1.6 g of deionized water, and keep it in ultrasound for 15 minutes to obtain a piezoelectric photocatalyst dispersion.
[0062] Step 2, weigh 14.4 g of fine aggregate and 55.2 g of emulsified asphalt, disperse them in the above-mentioned piezoelectric photocatalyst dispersion, stir and mix, and obtain a piezoelectric photocatalytic mist seal pavement material.
[0063] In this embodiment, the dosage of CNBT is 1%.
[0064] Example 2
[0065] This embodiment provides a piezoelectric photocatalytic mist seal pavement material, which is prepared by the following steps:
[0066] Step 1, weigh 2.2 g of CNBT, disperse it in 4.4 g of deionized water, and keep it in ultrasound for 15 minutes to obtain a piezoelectric photocatalyst dispersion.
[0067] Step 2, weigh 14.4 g of fine aggregate and 51.0 g of emulsified asphalt, disperse them in the above-mentioned piezoelectric photocatalyst dispersion, stir and mix, and obtain a piezoelectric photocatalytic mist seal pavement material.
[0068] In this embodiment, the dosage of CNBT is 3%.
[0069] Example 3
[0070] This embodiment provides a piezoelectric photocatalytic mist seal pavement material, which is prepared by the following steps:
[0071] Step 1, weigh 3.6 g of CNBT, disperse it in 7.2 g of deionized water, and keep it in ultrasound for 15 minutes to obtain a piezoelectric photocatalyst dispersion.
[0072] Step 2, weigh 14.4 g of fine aggregate and 46.8 g of emulsified asphalt, disperse them in the above-mentioned piezoelectric photocatalyst dispersion, stir and mix, and obtain a piezoelectric photocatalytic mist seal pavement material.
[0073] In this embodiment, the dosage of CNBT is 5%.
[0074] Example 4
[0075] This embodiment provides a piezoelectric photocatalytic mist seal pavement material, which is prepared by the following steps:
[0076] Step 1, weigh 1.44 g of CNBT, disperse it in 2.88 g of deionized water, and keep it in ultrasound for 15 minutes to obtain a piezoelectric photocatalyst dispersion.
[0077] Step 2, weigh 14.4 g of fine aggregate and 53.28 g of emulsified asphalt, disperse them in the above-mentioned piezoelectric photocatalyst dispersion, stir and mix, and obtain a piezoelectric photocatalytic mist seal pavement material.
[0078] In this embodiment, the dosage of CNBT is 2%.
[0079] Example 5
[0080] This embodiment provides a piezoelectric photocatalytic mist seal pavement material, which is prepared by the following steps:
[0081] Step 1, weigh 2.88 g of CNBT, disperse it in 5.76 g of deionized water, and keep it in ultrasound for 15 minutes to obtain a piezoelectric photocatalyst dispersion.
[0082] Step 2, weigh 14.4 g of fine aggregate and 48.96 g of emulsified asphalt, disperse them in the above-mentioned piezoelectric photocatalyst dispersion, stir and mix, and obtain a piezoelectric photocatalytic mist seal pavement material.
[0083] In this embodiment, the dosage of CNBT is 4%.
[0084] Comparative Example 1
[0085] This embodiment provides a photocatalytic mist seal pavement material, which is prepared by the following steps:
[0086] Step 1: Use urea as a precursor of g-C3N4, put 10 g of urea into a muffle furnace and calcine at 550° C. for 2 h, grind, and obtain g-C3N4.
[0087] Step 2, weigh 2.2 g of g-C3N4, disperse it in 4.4 g of deionized water, and keep it in ultrasound for 15 minutes to obtain a photocatalyst dispersion.
[0088] Step 3, weigh 14.4 g of fine aggregate and 51.0 g of emulsified asphalt, disperse them in the above-mentioned photocatalyst dispersion, stir and mix well, and obtain a photocatalytic mist seal pavement material.
[0089] Experimental Section
[0090] (I) Microscopic morphology test
[0091] The present invention takes the g-C3N4 in Comparative Example 1 and the CNBT prepared by the present invention as examples, and performs electron scanning electron microscopy tests on them respectively, and the test results are as follows: Figure 1 and Figure 2 shown.
[0092] Figure 1 This is the SEM image of g-C3N4 in Comparative Example 1. Figure 1 It can be seen that the surface of g-C3N4 prepared by urea has more pores, forming more active sites, creating conditions for the adsorption of more pollutants and the occurrence of redox reactions. Under the same conditions, the degradation effect is better than other unmodified catalysts, such as TiO2.
[0093] Figure 2 This is a scanning electron microscope image of the CNBT prepared in the present invention. Figure 2It can be seen that the addition of BT to g-C3N4 does not destroy its original microstructure. Instead, BT is completely wrapped by g-C3N4 to form a core-shell structure with BT as the core and g-C3N4 as the shell. Among them, the g-C3N4 in the shell can improve the activity of g-C3N4 through the piezoelectric polarization generated by the BT in the core, and efficiently degrade pollutants. Moreover, in the absence of light, BT can release the piezoelectric effect to force the g-C3N4 in the shell to undergo redox reactions to degrade pollutants, which is beneficial to promote the degradation of pollutants.
[0094] (ii) XRD test
[0095] The present invention takes the g-C3N4 in Comparative Example 1, the BT used in the present invention and the CNBT prepared in the present invention as examples, and performs XRD tests on them respectively, and the test results are as follows: Figure 3 shown.
[0096] Figure 3 The XRD patterns of g-C3N4, BT and CNBT are shown in Figure 2. Figure 3 It can be seen that the composite of g-C3N4 and BT does not destroy their respective lattice structures, and the composite materials maintain their original properties.
[0097] (III) Optical performance test
[0098] The present invention takes the g-C3N4 in Comparative Example 1, the BT used in the present invention and the CNBT prepared in the present invention as examples, and performs photoluminescence and absorption spectrum tests on them respectively, and the test results are as follows: Figure 4 and Figure 5 shown.
[0099] Figure 4 The photoluminescence spectra of g-C3N4, BT and CNBT catalysts are shown in Figure 2. Figure 4 It can be seen that the peak intensity of CNBT is the lowest, followed by BT, and CN has the highest peak intensity, indicating that the prepared CNBT material has good carrier separation efficiency and low charge recombination rate, which is conducive to the efficient degradation of pollutants.
[0100] Figure 5 The absorption spectra of g-C3N4, BT and CNBT catalysts are shown in Figure 2. Figure 5 It can be seen that the original absorption edges of CN and BT are 437 mm and 398 mm, while the absorption edge of CNBT is blue-shifted to 428 mm, indicating that the energy band structure of CNBT is between CN and BT, which meets the redox potential required for NO degradation in exhaust gas and is beneficial to improving the catalyst activity.
[0101] (IV) Automobile exhaust degradation performance test
[0102] 1) Effect of catalytic conditions on the efficiency of CNBT catalyst in degrading automobile exhaust
[0103] In order to explore the influence of catalytic conditions on the efficiency of CNBT catalyst in degrading automobile exhaust, the present invention uses the CNBT catalyst prepared by the present invention as a catalyst, uses NO to simulate automobile exhaust, and tests the efficiency of CNBT catalyst in degrading automobile exhaust under different catalytic conditions, and the test method is as follows:
[0104] The automobile exhaust degradation test of the CNBT catalyst prepared by the present invention is carried out in a prepared reaction box. The reaction box is sealed by six 1m×1m transparent acrylic plates, and a 20mm×20mm high-transmittance glass is installed directly above the reaction box. A 300W xenon lamp light source is placed above the high-transmittance glass to simulate sunlight, and a vibration table is placed inside the reaction box to provide vibration. Switch-controlled air inlets are installed on the left and right sides, the right side is the air inlet connected to the NO gas cylinder, and the left side is the air outlet connected to the NO analyzer.
[0105] First, the prepared CNBT was dispersed in deionized water in a 20 cm diameter petri dish and placed on a vibrating table. -1 NO gas was passed through the pipe at a rate of 50s and stabilized for about 20min until the gas concentration reached 5ppm. Finally, the automobile exhaust degradation test was started. The test duration was 2h. The NO analyzer continuously collected and recorded the gas at the outlet. The test results are shown in the figure below. Figure 6 shown.
[0106] Figure 6 The results of the CNBT catalyst degradation efficiency test under different conditions are shown.
[0107] Depend on Figure 6 It can be seen from the test results that the degradation efficiency of the CNBT prepared by the present invention under piezoelectric catalysis and photocatalysis is 35.6% and 48.9% respectively, indicating that the CNBT prepared by the present invention has piezoelectric catalysis and photocatalysis properties, and can degrade NO through external mechanical force and light, providing theoretical support for the application of pavement materials with the performance of degrading automobile exhaust. At the same time, the degradation effect of the CNBT prepared by the present invention under the synergistic effect of the two is enhanced to 77.9%, which is 2.19 times that of the previous piezoelectric catalysis and 1.60 times that of the photocatalysis, proving that CNBT has the ability to efficiently degrade NO through piezoelectric synergy and photocatalysis.
[0108] 2) Effect of piezoelectric photocatalyst dosage on the efficiency of piezoelectric photocatalytic degradation of automobile exhaust gas by seal-coated pavement materials
[0109] The test objects are:
[0110] The present invention takes the piezoelectric photocatalytic mist seal pavement materials of Examples 1 to 5 as examples and tests their efficiency in degrading automobile exhaust to explore the effects of different dosages of piezoelectric photocatalysts on the efficiency of piezoelectric photocatalytic mist seal pavement materials in degrading automobile exhaust.
[0111] The test method is:
[0112] The automobile exhaust degradation tests of the piezoelectric photocatalytic mist seal pavement materials of Examples 1 to 5 were all carried out in a modified wheel tracker. In order to ensure that there is no leakage, all the internal and external joints of the wheel tracker are sealed with transparent tape. The wheel tracker wheels roll back and forth to simulate the operation of road vehicles, and light is irradiated by an external light source. Two air holes are set on both sides of the wheel tracker, which are respectively connected to the exhaust gas cylinder and the NO analyzer. First, put the wheel track plate sprayed with the piezoelectric photocatalytic mist seal pavement material into the wheel tracker. Then, at 1L / min -1 NO gas was passed at a rate of 50s and stabilized for about 20min until the gas concentration reached 5ppm. Finally, the automobile exhaust degradation test was started. The test duration was 1h. The NO analyzer continuously collected and recorded the gas at the outlet. The test results are as follows: Figure 7 The piezoelectric photocatalytic mist seal pavement materials of Examples 1 to 5 were all heated at 0.8 kg / m 2 Pour the spray area amount into the spreader and spray on the rutting board.
[0113] Figure 7 These are the test results of the degradation efficiency of automobile exhaust gas of the piezoelectric photocatalytic mist seal pavement materials of Examples 1 to 5.
[0114] Depend on Figure 7 It can be seen that the piezoelectric photocatalytic mist seal pavement materials with five different dosages all have the property of degrading automobile exhaust. Among them, the best degradation effect is the 3% by mass dosage. This may be because the piezoelectric photocatalytic material with a mass ratio of 3% can be evenly dispersed in the mist seal and fully exert its degradation effect. The catalyst in the mist seal with a mass ratio of 1% and 5% is insufficient and excessive, which affects the degradation of automobile exhaust.
[0115] 3) Effect of catalytic conditions on the efficiency of piezoelectric photocatalytic mist seal pavement materials in degrading automobile exhaust
[0116] In order to explore the influence of catalytic conditions on the efficiency of piezoelectric photocatalytic mist seal pavement materials in degrading automobile exhaust, the present invention takes the piezoelectric photocatalytic mist seal pavement material of Example 2 as an example, uses NO to simulate automobile exhaust, and tests the efficiency of degrading automobile exhaust of the piezoelectric photocatalytic mist seal pavement material of Example 2 under the catalytic conditions of piezoelectric catalysis, photocatalysis and piezoelectric photocatalysis synergistic action, and the test method is as follows:
[0117] The test of the piezoelectric photocatalytic mist seal layer in Example 2 for degrading automobile exhaust under different conditions was carried out in a modified wheel tracker. In order to ensure that there is no leakage, all the internal and external joints of the wheel tracker are sealed with transparent tape. The wheel tracker wheels roll back and forth to simulate the operation of road vehicles, and light is irradiated by an external light source. Two air holes are set on both sides of the wheel tracker, which are respectively connected to the exhaust gas cylinder and the NO analyzer. First, put the wheel track plate sprayed with the piezoelectric photocatalytic mist seal layer pavement material into the wheel tracker. Then, at 1L / min -1 NO gas was passed at a rate of 50s and stabilized for about 20min until the gas concentration reached 5ppm. Finally, the automobile exhaust degradation test was started. The test duration was 1h. The NO analyzer continuously collected and recorded the gas at the outlet. The test results are as follows: Figure 8 The piezoelectric photocatalytic mist seal pavement material of Example 2 is 0.8 kg / m 2 Pour the spray area amount into the spreader and spray on the rutting board.
[0118] Figure 8 These are the test results of the efficiency of the piezoelectric photocatalytic mist seal layer of Example 2 in degrading automobile exhaust gas under different conditions.
[0119] Depend on Figure 8 The test results show that the piezoelectric photocatalytic mist seal layer has the properties of automobile exhaust degradation under piezoelectric catalysis, photocatalysis and synergistic effects, which meets the original design effect. It also proves the feasibility of efficiently degrading automobile exhaust under piezoelectric catalysis, photocatalysis and synergistic effects.
[0120] 4) Effect of spraying amount on the efficiency of piezoelectric photocatalytic mist seal pavement material in degrading automobile exhaust
[0121] In order to explore the effect of spraying amount on the degradation efficiency of automobile exhaust gas of piezoelectric photocatalytic mist seal pavement materials, the present invention takes the piezoelectric photocatalytic mist seal pavement material of Example 2 as an example, uses NO to simulate automobile exhaust gas, and sprays the piezoelectric photocatalytic mist seal pavement materials obtained in Example 2 at 0.6 kg / m 2 , 0.8kg / m 2 and 1.0kg / m 2 The spraying area is poured into the spreader and sprayed on the rutting board, and the degradation efficiency of automobile exhaust is tested respectively, and the test method is as follows:
[0122] The test of the piezoelectric photocatalytic mist seal layer in Example 2 for degrading automobile exhaust under different conditions was carried out in a modified wheel tracker. In order to ensure that there is no leakage, all the internal and external joints of the wheel tracker are sealed with transparent tape. The wheel tracker wheels roll back and forth to simulate the operation of road vehicles, and light is irradiated by an external light source. Two air holes are set on both sides of the wheel tracker, which are respectively connected to the exhaust gas cylinder and the NO analyzer. First, put the wheel track plate sprayed with the piezoelectric photocatalytic mist seal layer pavement material into the wheel tracker. Then, at 1L / min -1 NO gas was passed at a rate of 50s and stabilized for about 20min until the gas concentration reached 5ppm. Finally, the automobile exhaust degradation test was started. The test duration was 1h. The NO analyzer continuously collected and recorded the gas at the outlet. The test results are as follows: Fig. 9 shown.
[0123] Fig. 9 These are the test results of the efficiency of the piezoelectric photocatalytic mist seal layer of Example 2 in degrading automobile exhaust gas at different spraying rates.
[0124] Depend on Fig. 9 The test results show that the piezoelectric photocatalytic mist seal pavement materials with three different spraying amounts have a high degradation effect on automobile exhaust, and the spraying amount with the best degradation effect is 0.8kg / m 2 This may be because 0.8kg / m 2 The spraying amount can evenly spray the piezoelectric photocatalytic mist seal layer and fully exert its degradation effect. 2 and 1.0kg / m 2 There are both insufficient and excessive spraying amounts, which in turn affects the degradation of automobile exhaust.
[0125] 5) Effect of cyclic testing on the efficiency of piezoelectric photocatalytic mist seal pavement materials in degrading automobile exhaust.
[0126] In order to explore the effect of cyclic testing on the efficiency of piezoelectric photocatalytic mist seal pavement materials in degrading automobile exhaust, the present invention takes the piezoelectric photocatalytic mist seal pavement material of Example 2 as an example, uses NO to simulate automobile exhaust, and conducts multiple cyclic tests on the efficiency of piezoelectric photocatalytic mist seal pavement materials in Example 2 in degrading automobile exhaust, and the test method is as follows:
[0127] The automobile exhaust degradation test of the piezoelectric photocatalytic mist seal pavement material in Example 2 was carried out in a modified wheel tracker. In order to ensure that there is no leakage, all the internal and external joints of the wheel tracker are sealed with transparent tape. The wheel tracker wheels roll back and forth to simulate the operation of road vehicles, and light is irradiated by an external light source. Two air holes are set on both sides of the wheel tracker, which are respectively connected to the exhaust gas cylinder and the NO analyzer. First, put the wheel track plate sprayed with the piezoelectric photocatalytic mist seal pavement material into the wheel tracker. Then, at 1L / min-1 NO gas was passed at a rate of 50s and stabilized for about 20min until the gas concentration reached 5ppm. Finally, the automobile exhaust degradation test was started. The test duration was 1h. The NO analyzer continuously collected and recorded the gas at the outlet. The test results are as follows: Fig.10 The piezoelectric photocatalytic mist seal pavement materials in Example 2 were all heated to 0.8 kg / m 2 Pour the spray area amount into the spreader and spray on the rutting board.
[0128] Fig.10 This is the degradation efficiency cycle test result of automobile exhaust gas of the piezoelectric photocatalytic mist seal pavement material of Example 2.
[0129] Depend on Fig.10 The test results show that after five cycles, the degradation efficiency decreased by 8.9%, indicating that the piezoelectric photocatalytic mist seal pavement material has good durability.
[0130] 6) Effect of different catalysts on the degradation efficiency of automobile exhaust gas in fog seal pavement materials
[0131] In order to explore the influence of different catalysts on the degradation efficiency of automobile exhaust gas of fog seal pavement materials, the present invention takes the piezoelectric photocatalytic fog seal pavement material of Example 2 and the photocatalytic fog seal pavement material of Comparative Example 1 as examples, uses NO to simulate automobile exhaust gas, and tests the degradation efficiency of automobile exhaust gas of the piezoelectric photocatalytic fog seal pavement material of Example 2 and the photocatalytic fog seal pavement material of Comparative Example 1, and the test method is as follows:
[0132] The automobile exhaust degradation test of the piezoelectric photocatalytic mist seal pavement material of Example 2 and the mist seal pavement material of Comparative Example 1 was carried out in a modified wheel tracker. In order to ensure that there is no air leakage, all the internal and external joints of the wheel tracker are sealed with transparent tape. The wheel tracker wheels roll back and forth to simulate the operation of road vehicles, and light is irradiated by an external light source. Two air holes are set on both sides of the wheel tracker, which are respectively connected to the exhaust gas cylinder and the NO analyzer. First, put the rutting plate sprayed with the mist seal pavement material into the wheel tracker. Then, at 1L / min -1 NO gas was passed at a rate of 50s and stabilized for about 20min until the gas concentration reached 5ppm. Finally, the automobile exhaust degradation test was started. The test duration was 1h. The NO analyzer continuously collected and recorded the gas at the outlet. The test results are as follows: Fig.11 The fog seal pavement materials of Example 2 and Comparative Example 1 were both 0.8 kg / m 2 Pour the spray area amount into the spreader and spray on the rutting board.
[0133] Fig.11These are the test results of the degradation efficiency of automobile exhaust gas by the piezoelectric photocatalytic mist seal pavement material of Example 2 and the photocatalytic mist seal pavement material of Comparative Example 1.
[0134] Depend on Fig.11 It can be seen from the test results that compared with the g-C3N4 photocatalytic sand-containing mist seal layer of comparative example 1, the CNBT piezoelectric photocatalytic mist seal layer of example 2 exhibits excellent efficiency in degrading automobile exhaust, which also confirms that the prepared CNBT piezoelectric photocatalytic mist seal layer pavement material has a high efficiency in degrading automobile exhaust.
[0135] Obviously, the above embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
Claims
1. A piezoelectric photocatalytic mist seal pavement material, characterized in that: The raw materials for its preparation are composed of the following components in parts by weight: 100 parts of emulsified asphalt, 1 to 5 parts of piezoelectric photocatalyst, 2 to 10 parts of water and 20 parts of fine aggregate; The piezoelectric photocatalyst has a core-shell structure, wherein the core is BaTiO3 and the shell is g-C3N4.
2. The piezoelectric photocatalytic mist seal pavement material according to claim 1, characterized in that: The piezoelectric photocatalyst is prepared by the following steps: In water, a g-C3N4 precursor and BaTiO3 are mixed to obtain a suspension; wherein the g-C3N4 precursor is any one of urea, dicyandiamide and melamine; Performing an evaporation treatment on the suspension to evaporate the water in the suspension to obtain a solid component; The solid component is calcined at 500° C. to 600° C. and ground to obtain the piezoelectric photocatalyst.
3. The piezoelectric photocatalytic mist seal pavement material according to claim 2, characterized in that: The mass ratio of the g-C3N4 precursor to BaTiO3 is 100g:0.5g~3g.
4. The piezoelectric photocatalytic mist seal pavement material according to claim 2, characterized in that: The calcination treatment time is 1 h to 3 h.
5. The piezoelectric photocatalytic mist seal pavement material according to claim 2, characterized in that: The usage ratio of the water to the BaTiO3 is 500mL:1g~5g.
6. The piezoelectric photocatalytic mist seal pavement material according to claim 1, characterized in that: The fine aggregate is composed of the following components in mass percentage: The first quartz sand is 95% to 100%, the second quartz sand is 5% to 10%, the third quartz sand is 0 to 5% and the fourth quartz sand is 0 to 1%, totaling 100%; Wherein, the particle size of the first quartz sand is 0.31 mm to 0.6 mm; The particle size of the second quartz sand is 0.16 mm to 0.3 mm; The particle size of the third quartz sand is 0.08 mm to 0.15 mm; The particle size of the fourth quartz sand is ≤0.075 mm.
7. A method for preparing the piezoelectric photocatalytic mist seal pavement material according to any one of claims 1 to 6, characterized in that: include: According to the ratio of the piezoelectric photocatalytic mist seal pavement material, weigh the corresponding mass of each preparation raw material for use; Dispersing the weighed piezoelectric photocatalyst in water to obtain a piezoelectric photocatalyst dispersion; The weighed fine aggregate and emulsified asphalt are dispersed in the piezoelectric photocatalyst dispersion, stirred and mixed to obtain a piezoelectric photocatalytic mist seal pavement material.
8. The preparation method according to claim 7, characterized in that: The piezoelectric photocatalyst weighed is dispersed in water by ultrasonic method; and the ultrasonic time is 10 minutes to 20 minutes.
9. Use of the piezoelectric photocatalytic mist seal pavement material according to any one of claims 1 to 6 for degrading exhaust gas, characterized in that: The piezoelectric photocatalytic mist seal pavement material is sprayed on the road surface to degrade automobile exhaust in real time under the synergistic effect of vehicle load and light.
10. The use according to claim 9, characterized in that The spraying amount is 0.6kg / m 2 ~1kg / m 2 .
Citation Information
Patent Citations
Photocatalytic asphalt mixture and preparation method thereof
CN107473633A
g-C3N4 / TiO2 photocatalytic emulsified asphalt and preparation method thereof
CN108822564A
Preparing method for sand-mist-containing sealing layer pavement material with automobile exhaust gas degrading function