Silicon-rich anti-reflection coating resin, preparation method thereof and silicon-rich anti-reflection coating

Silicon-rich antireflective coating resin was prepared by adding carbon-carbon double bond monomers with epoxy crosslinking groups and light-absorbing groups to polymethylhydrosiloxane, which solved the stability of the coating The problem of poor performance achieves controllability of high silicon content and optical parameters, and improves storage stability and anti-reflection performance.

CN118995044APending Publication Date: 2024-11-22QIANWAN INST OF CNITECH +1

Patent Information

Application Number
CN202411135094.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing silicon-rich anti-reflective coatings have poor stability and are prone to self-polymerization during storage, which affects the yield and efficiency of chip manufacturing.

Method used

Silicon-rich antireflective coating resin was prepared by adding carbon-carbon double bond monomers containing epoxy crosslinking groups and light absorbing groups to polymethylhydrogen siloxane, and by adjusting the molar ratio Achieve controllability of high silicon content and optical parameters.

Benefits of technology

It improves the stability and storage period of silicon-rich anti-reflective coating resin, reduces storage costs, and meets the etching rate and anti-reflective performance requirements in different application scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118995044A_ABST
    Figure CN118995044A_ABST
Patent Text Reader

Abstract

The invention discloses a silicon-rich anti-reflection coating resin, a preparation method thereof and a silicon-rich anti-reflection coating, the silicon-rich anti-reflection coating resin has a structure as shown in a formula (I), R1 is selected from an epoxy group containing 1-10 straight-chain carbon atoms or an epoxy group containing 1-10 loop-chain carbon atoms, R2 is selected from an epoxy group containing 1-10 straight-chain carbon atoms or an epoxy group containing 1-10 loop-chain carbon atoms, and R3 is selected from an epoxy group containing 1-10 straight-chain carbon atoms or an epoxy group containing 1-10 loop-chain carbon atoms; r2 is selected from groups containing phenyl, naphthyl, pyridyl, thienyl and benzyl; the ratio of x to y to z is (7-10): (0.4-1): (0.3-1), and the weight-average molecular weight of the silicon-rich anti-reflection coating resin is 70000-100000. A carbon-carbon double-bond monomer containing an epoxy cross-linking group and a light-absorbing group is added on polymethylhydrosiloxane, so that the silicon-rich anti-reflection coating with a large number of Si-H bonds and containing the light-absorbing group and the epoxy cross-linking group is obtained, regulation and control of optical parameters and the cross-linking degree can be realized, the stability of resin is effectively improved, the storage life of the resin is effectively prolonged, and the application range of the silicon-rich anti-reflection coating is widened. The storage cost is reduced, and the requirements on the etching rate and the anti-reflection performance of the silicon-rich anti-reflection coating in different application scenes can be met. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer materials, and in particular relates to a silicon-rich anti-reflection coating resin and a preparation method thereof, and a silicon-rich anti-reflection coating. Background Art

[0002] In photolithography, the critical size and resolution of patterns have become important performance indicators. In order to meet the requirements of higher resolution in photoresists, research on the use of deep ultraviolet, (248nm) KrF excimer laser, and (193nm) ArF excimer laser for photolithography has attracted much attention. As the integration of semiconductor devices increases, the line width requirements of semiconductor components are getting smaller and smaller, and the control of critical dimensions is becoming more and more important. In order to prepare smaller and more sophisticated semiconductor devices, higher requirements are placed on photolithography processes and materials.

[0003] However, as the wavelength of photolithography exposure decreases, the surface of the wafer is affected by the interference of reflected light and incident light, forming a standing wave effect and multi-layer exposure inside the photoresist, and ripples appear on the side walls of the pattern, which seriously affects the clarity and resolution of the pattern. And when performing ultra-fine pattern processes at some technology nodes below 45nm, the thickness of the photoresist will generally be less than 150nm. In this case, such a thin photoresist cannot effectively block the etching of the plasma, resulting in the photoresist being consumed before the pattern is completely etched onto the wafer, resulting in the failure of the photolithography pattern transfer. Therefore, in order to alleviate the standing wave effect and improve the etching resistance, multi-layer photolithography technology was applied.

[0004] Inorganic coatings adjust the refractive index by changing the composition of inorganic particles. The disadvantages are that the vapor deposition process is complicated, the equipment is expensive, and it is difficult to etch the titanium oxynitride coating. Compared with inorganic coatings, organic coatings are generally obtained by spin coating, and the absorption of ultraviolet light by the dyeing groups in organic polymers is used to reduce the reflectivity of the substrate. The preparation process is simple and easy to etch.

[0005] Multilayer photolithography is achieved by alternating organic and inorganic layers, and the pattern transfer of photoresist is achieved by selective plasma etching between different layers. Multilayer photolithography can be achieved by chemical vapor deposition or spin coating or a combination of both. Since spin coating is simple and easy to use, it is usually used as one of the main methods of photolithography.

[0006] Silicon-rich anti-reflective coating is an important component of the spin-coated three-layer structure in multi-layer lithography technology. The spin-coated three-layer is composed of photoresist, silicon-rich anti-reflective coating and spin-coated carbon layer. They have large differences in different plasma rates, which improves the overall etching resistance of the three-layer structure. At the same time, the silicon-rich anti-reflective coating and the spin-coated carbon layer play an anti-reflective role for ultraviolet light during the lithography process, effectively reducing the standing wave effect, swing effect and notch effect.

[0007] The molecular structure design of silicon-rich anti-reflective coatings should take into account the influence of multiple factors: (1) The silicon content mainly affects the etching rate. As the silicon content increases, the fluorine plasma etching rate becomes faster to protect the Si layer, and the oxygen plasma etching rate becomes slower to protect the C layer, reducing the consumption of photoresist. Therefore, the higher the silicon content, the greater the improvement in overall anti-etching ability; (2) The refractive index n and absorption coefficient k of the silicon-rich anti-reflective coating should match the application scenarios such as the photolithography process to achieve a good phase shift, form subtractive interference, eliminate the reflected light of the substrate, and play an anti-reflection role; (3) The surface properties of the silicon-rich anti-reflective coating should match the photoresist to ensure good adhesion between the silicon-rich anti-reflective coating and the photoresist and avoid the collapse of the photoresist during the development process.

[0008] At present, most of the research and patents in the field of silicon-rich anti-reflective coatings are mainly carried out around the sol method. However, the stability of siloxane polymers prepared by the sol method is poor, and self-polymerization reactions are prone to occur during storage. This process cannot be prevented, and the rate of self-polymerization reactions can only be reduced by lowering the storage temperature, adding stabilizers, etc. The super-large polysiloxane molecules formed by the self-polymerization reaction will form gel particles. The increase in the particle content will reduce the film quality, thereby affecting the yield rate of the chip manufacturing lithography process, and seriously affecting the chip manufacturing cost and efficiency. Therefore, it is of great significance to find a highly stable silicon-rich anti-reflective coating for use in lithography technology. Summary of the invention

[0009] In view of the shortcomings of the prior art, the present invention provides a silicon-rich anti-reflective coating resin and a preparation method thereof, and a silicon-rich anti-reflective coating. The silicon-rich anti-reflective coating resin of the present invention has high stability, solvent resistance and a long shelf life, and can achieve high silicon content and fully controllable optical parameters of the silicon-rich anti-reflective coating by regulating the molecular structure of the resin.

[0010] The first aspect of the present invention provides a silicon-rich anti-reflective coating resin, the structure of which is shown in formula (I):

[0011]

[0012] Among them, R 1 is selected from epoxy groups containing 1 to 10 straight-chain carbon atoms or epoxy groups containing 1 to 10 cyclic carbon atoms; R 2 A group selected from the group containing phenyl, naphthyl, pyridyl, thienyl, benzyl;

[0013] The ratio of x, y and z is 7-10:0.4-1:0.3-1, and the weight average molecular weight of the silicon-rich anti-reflective coating resin is 70,000-100,000.

[0014] The second aspect of the present invention provides a method for preparing the silicon-rich anti-reflective coating resin, comprising the following steps:

[0015] (1) dissolving polymethyl hydrogen siloxane in solvent 1 to obtain a mixed solution A;

[0016] (2) dissolving a carbon-carbon double bond monomer containing an epoxy crosslinking group, a carbon-carbon double bond monomer containing a light absorbing group, and a catalyst in a second solvent to obtain a mixed solution B;

[0017] (3) Adding mixed solution B dropwise to mixed solution A to carry out a reaction, and performing reduced pressure distillation after the reaction is completed to obtain the silicon-rich anti-reflective coating resin.

[0018] The silicon-rich anti-reflective coating resin is prepared by the silicon hydroaddition polymerization method, and a carbon-carbon double bond monomer containing an epoxy cross-linking group and a light-absorbing group is added to polymethyl hydrogen siloxane to finally obtain a chain polysiloxane. This method has a simple reaction, easy synthesis, and the raw materials of the carbon-carbon double bond monomer are easily available; the reaction product contains a large number of Si-H bonds to ensure that the high Si content effectively improves the overall anti-etching ability; it also contains light-absorbing groups and epoxy cross-linking groups to meet the regulation of optical parameters and cross-linking degree, effectively improves the stability of the resin, increases the shelf life of the silicon-rich anti-reflective coating product, and reduces the storage cost of the silicon-rich anti-reflective coating product.

[0019] Preferably, the solvent one or solvent two includes but is not limited to pentane, hexane, heptane, octane, benzene, toluene, xylene, isopropanol, acetone, 2-methoxyethyl acetate, propylene glycol methyl ether, propylene glycol ethyl ether, propylene glycol propyl ether, propylene glycol butyl ether, dipropylene glycol methyl ether, propylene glycol methyl ether acetate, propylene glycol ethyl ether acetate, propylene glycol-1,2-dimethyl ether, propylene glycol diacetate, dimethyl ketone, cyclohexanone, diisobutyl ketone, ethyl acetate, butyl acetate, 2-methylpropyl acetate, 3-methylbutyl acetate, ethyl lactate, methyl 3-methoxypropionate, cyclopentyl methyl ether, 4-hydroxy-4-methyl-2-pentanone, diethyl ether, dibutyl ether, dimethyl phthalate, and tetrahydrofuran.

[0020] Preferably, the polymethylhydrogensiloxane includes but is not limited to one or more polymethylhydrogensiloxanes with any hydrogen content. Preferably, the hydrogen content of the polymethylhydrogensiloxane is 1.4-1.8wt%. More preferably, the hydrogen content of the polymethylhydrogensiloxane is about 1.6wt%. The polymethylhydrogensiloxane with this hydrogen content can provide a large number of Si-H bonds, which can ensure that there are more Si-H bonds in the reaction product and obtain a stable product.

[0021] Preferably, the carbon-carbon double bond monomer containing an epoxy crosslinking group is an epoxy carbon-carbon double bond monomer containing 1 to 10 straight-chain carbon atoms or an epoxy carbon-carbon double bond monomer containing 1 to 10 cyclic carbon atoms.

[0022] More preferably, the carbon-carbon double bond monomer containing epoxy crosslinking groups includes, but is not limited to, one or more of allyl glycidyl ether, epoxybutene, 1,2-epoxy-5-cyclooctene, 3,4-epoxy-1-cyclohexene, 1,2-epoxy-5-hexene, 4-vinyl epoxycyclohexane, 1,2-epoxy-9-decene, and 1,2-epoxy-4-vinylcyclohexane. The carbon-carbon double bond monomer containing epoxy crosslinking groups is easy to react, the monomer is cheap and easy to obtain, and the generated product has excellent solvent resistance and high temperature resistance.

[0023] Preferably, the carbon-carbon double bond monomer containing a light absorbing group is a carbon-carbon double bond monomer containing a phenyl group, a naphthyl group, a pyridyl group, a thienyl group, a benzyl group, or the like.

[0024] More preferably, the carbon-carbon double bond monomer containing a light absorbing group includes, but is not limited to, one or more of styrene, 1-vinylnaphthalene, 6-methoxy-2-naphthylethylene, tetrakis-(3-pyridylbiphenyl)ethylene, 1,1,2,2-tetrakis(pyridin-4-yl)ethylene, 2-vinylpyridine, 1-phenyl-1-trimethylsiloxyethylene, 2,2-(1,2-vinyl)bithiophene, 2-vinylthiophene, benzyl vinyl ether, and 4-vinylbenzyl alcohol. The carbon-carbon double bond monomer containing a light absorbing group is easy to react, and the generated product meets the requirements of optical parameter regulation and anti-reflection performance under different conditions.

[0025] Preferably, the molar ratio of the repeating unit -(CH3)SiO(H)-, the carbon-carbon double bond monomer containing an epoxy crosslinking group, and the carbon-carbon double bond monomer containing a light absorbing group in the polymethyl hydrogen siloxane is 7-10:0.4-1:0.3-1. More preferably, the molar ratio of the repeating unit -(CH3)SiO(H)-, the carbon-carbon double bond monomer containing an epoxy crosslinking group, and the carbon-carbon double bond monomer containing a light absorbing group in the polymethyl hydrogen siloxane is 10:0.4-1:0.3-1. The present invention can directly regulate the composition of the silicon-rich anti-reflective coating resin by regulating the molar ratio of the repeating unit in the polymethyl hydrogen siloxane, the carbon-carbon double bond monomer containing an epoxy crosslinking group, and the carbon-carbon double bond containing a light absorbing group. By controlling the molar ratio of the three within the above range, a silicon-rich anti-reflective coating resin with excellent performance can be obtained.

[0026] Preferably, the catalyst includes but is not limited to Speier catalyst, Custer catalyst, or complex catalyst formed by chloroplatinic acid and ketones, cyclopentadiene, esters, alcohols, crown ethers, crown ethers containing heteroatoms and polysiloxanes.

[0027] Specifically, the catalyst can be one or more of chloroplatinic acid (H2PtCl6·6H2O, H2PtCl6 / i-PrOH, H2PtCl6 / THF), platinum (0)-1,3-diethyl-1,1,3,3-tetramethyldisiloxane, platinum chloride, platinum-plated carbon, platinum black, ruthenium chloride, iridium chloride, (Ph3P)4Pd, (Ph3P)2PdCl2, (PhCN)2PdCl2, [RhCl(CO)2]2, (Ph3P)2(CO)RhCl, (Et3P)2(CO)RhCl, (Ph3P)3RhCl, Co(CO)8, Ni(CO)(Ph3P)2NiCl2. The present invention preferably uses platinum (0)-1,3-diethyl-1,1,3,3-tetramethyldisiloxane, which is easy to react and easy to remove after the reaction.

[0028] Preferably, the amount of the catalyst added is 0.0088%-0.01% of the total molar number of carbon-carbon double bonds in the raw material.

[0029] Preferably, in step (3), the reaction temperature is 30-120° C., and the reaction time is 10-72 h.

[0030] Preferably, the pressure of the reduced pressure distillation is 10 mmHg, the temperature is 40-100° C., and the time is 40-60 min.

[0031] The parameter control in the above preparation process is to ensure that the hydrosilane addition polymerization reaction proceeds to an appropriate degree of polymerization, and the coating obtained after the prepared silicon-rich anti-reflective coating resin is spin-coated and baked can ensure that the silicon content and optical parameters of the silicon-rich anti-reflective coating in the application scenario are met.

[0032] The third aspect of the present invention provides a silicon-rich anti-reflective coating, which is obtained by spin coating the silicon-rich anti-reflective coating resin on a semiconductor substrate and baking it. The silicon-rich anti-reflective coating of the present invention has excellent stability, and the silicon content and optical parameters in the coating can be finely controlled, which can meet the requirements of the etching rate and anti-reflective performance of the silicon-rich anti-reflective coating in different application scenarios, and has broad application prospects in the field of photolithography technology.

[0033] Compared with the prior art, the present invention has at least the following beneficial effects:

[0034] 1. The present invention adopts a hydrosilane addition polymerization method to prepare a silicon-rich anti-reflective coating resin, and adds a carbon-carbon double bond monomer containing an epoxy crosslinking group and a light-absorbing group to polymethyl hydrogen siloxane, thereby obtaining a silicon-rich anti-reflective coating resin having a large number of Si-H bonds to ensure a high Si content, and containing light-absorbing groups and epoxy crosslinking groups. The present invention optimizes the molecular structure of polysiloxane to meet the regulation of optical parameters and crosslinking degree, fundamentally improves the storage stability of the silicon-rich anti-reflective coating resin, prolongs the shelf life of the silicon-rich anti-reflective coating product, reduces the storage cost of the silicon-rich anti-reflective coating product, and has high value in practical applications.

[0035] 2. The present invention can achieve fine control of the silicon content and optical parameters of the silicon-rich anti-reflective coating to meet the requirements for the etching rate and anti-reflective performance of the silicon-rich anti-reflective coating in different application scenarios.

[0036] 3. The present invention adopts the hydrosilylation method to directly polymerize into a chain polymer. The method is simple and easy to operate, and also provides a new method for preparing silicon-rich anti-reflective coating resin. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 This is a photo of the silicon-rich anti-reflective coating resin in Example 1 of the present invention;

[0038] Figure 2 is an infrared spectrum of the silicon-rich anti-reflective coating resin in Example 1 of the present invention;

[0039] Figure 3 This is the hydrogen nuclear magnetic resonance spectrum of the silicon-rich anti-reflective coating resin in Example 1 of the present invention. DETAILED DESCRIPTION

[0040] Example 1

[0041] Add 120 g of xylene and 60 g of polymethylhydrogensiloxane (hydrogen content 1.6%) into a 500 mL three-necked reactor, install a condensation reflux device, stir and heat to 60°C in a N2 atmosphere, then slowly drop 11.42 g of allyl glycidyl ether, 10.4 g of styrene, 2.2 ppm of platinum (0)-1,3-diethene-1,1,3,3-tetramethyldisiloxane catalyst and 60 g of xylene into the three-necked flask. After the addition is complete, react at a constant temperature for 24 hours, and separate by vacuum distillation to obtain a silicon-rich anti-reflective coating resin at a pressure of 10 mmHg, a temperature of 40°C and a time of 60 min.

[0042] Figure 1 is a photograph of the silicon-rich anti-reflective coating resin prepared in Example 1. Figure 2 is the infrared spectrum of the silicon-rich anti-reflection coating resin prepared in Example 1. It can be seen from the figure that 2964cm -1The peak of methyl CH stretching vibration is 2874 cm -1 The absorption peak of CH in -OCH3 is 1604cm -1 、1496cm -1 、1450cm -1 、1407cm -1 The peak of benzene ring skeleton stretching vibration is 1260cm -1 The Si-C bending vibration peak is at 1080cm -1 The Si-O-Si absorption peak is at 800 cm -1 The absorption peak is Si-C.

[0043] Figure 3 This is the hydrogen nuclear magnetic resonance spectrum of the silicon-rich anti-reflective coating resin prepared in Example 1. It can be seen from the figure that the peak at 2.05ppm is the characteristic peak of deuterated acetone, 7.2-7.7ppm is the characteristic peak of the hydrogen atom of the benzene ring, 4.7ppm is the characteristic peak of Si-H, the absorption peak at 1.5-3.8ppm is the absorption peak of the hydrogen atom in the glycidyl ether oxypropyl group, and the absorption peak at 0.24ppm is the characteristic peak of Si-CH3.

[0044] Example 2

[0045] The only difference from Example 1 is that 68 g of polymethyl hydrogen siloxane (hydrogen content 1.6%), 7.81 g of styrene, and 6.42 g of allyl glycidyl ether are added to Example 2, and the rest is the same as Example 1. For further explanation, Example 2 is as follows:

[0046] Add 120 g of xylene and 68 g of polymethylhydrogensiloxane (hydrogen content 1.6%) into a 500 mL three-necked reactor, install a condensation reflux device, stir and heat to 60°C in a N2 atmosphere, then slowly drop 6.42 g of allyl glycidyl ether, 7.81 g of styrene, 2.2 ppm of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum (0) catalyst and 60 g of xylene into the three-necked flask. After the addition is complete, react at a constant temperature for 24 hours, and separate by vacuum distillation to obtain a silicon-rich anti-reflective coating resin at a pressure of 10 mmHg and a temperature of 40°C for 60 minutes.

[0047] Example 3

[0048] The only difference from Example 1 is that 68.4 g of polymethyl hydrogen siloxane (hydrogen content 1.6%), 5.86 g of styrene, and 6.42 g of allyl glycidyl ether are added to Example 3, and the rest is the same as Example 1. For further explanation, Example 3 is as follows:

[0049] Add 120 g of xylene and 68.4 g of polymethylhydrogensiloxane (hydrogen content 1.6%) into a 500 mL three-necked reactor, install a condensation reflux device, stir and heat to 60°C in a N2 atmosphere, then slowly drop 6.42 g of allyl glycidyl ether, 5.86 g of styrene, 2.2 ppm of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum (0) catalyst and 60 g of xylene into the three-necked flask. After the addition is complete, react at a constant temperature for 24 hours, and separate by vacuum distillation to obtain a silicon-rich anti-reflective coating resin at a pressure of 10 mmHg and a temperature of 40°C for 60 minutes.

[0050] Example 4

[0051] The only difference from Example 1 is that benzyl vinyl ether is added in place of styrene and epoxybutene is added in place of allyl glycidyl ether, and the rest is the same as Example 1. For further explanation, Example 4 is as follows:

[0052] Add 120 g of xylene and 69.9 g of polymethylhydrogensiloxane (hydrogen content 1.6%) into a 500 mL three-necked reactor, install a condensation reflux device, stir and heat to 60°C in a N2 atmosphere, then slowly drop 7.1 g of epoxybutene, 13.42 g of benzyl vinyl ether, 2.2 ppm of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum (0) catalyst and 60 g of xylene into the three-necked flask. After the addition is complete, react at a constant temperature for 24 hours, and separate by vacuum distillation to obtain a silicon-rich anti-reflective coating resin at a pressure of 10 mmHg and a temperature of 40°C for 60 minutes.

[0053] Example 5

[0054] The only difference from Example 1 is that 1-vinylnaphthalene is added in place of styrene and epoxybutene is added in place of allyl glycidyl ether, and the rest is the same as Example 1. For further explanation, Example 5 is as follows:

[0055] Add 120 g of xylene and 60 g of polymethylhydrogensiloxane (hydrogen content 1.6%) into a 500 mL three-necked reactor, install a condensation reflux device, stir and heat to 60°C in a N2 atmosphere, then slowly drop 7.1 g of epoxybutene, 15.42 g of 1-vinylnaphthalene, 2.2 ppm of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum (0) catalyst, and 60 g of xylene into the three-necked flask. After the addition is complete, react at a constant temperature for 24 hours, and separate by vacuum distillation to obtain a silicon-rich anti-reflective coating resin at a pressure of 10 mmHg and a temperature of 40°C for 60 minutes.

[0056] Example 6

[0057] The only difference from Example 1 is that 2-vinylpyridine is added in place of styrene, and 1,2-epoxy-5-hexene is added in place of allyl glycidyl ether, and the rest is the same as Example 1. For further explanation, Example 6 is as follows:

[0058] Add 120 g of xylene and 60 g of polymethylhydrogensiloxane (hydrogen content 1.6%) into a 500 mL three-necked reactor, install a condensation reflux device, stir and heat to 60°C in a N2 atmosphere, then slowly drop 1,2-epoxy-5-hexene 12.42 g, 2-vinylpyridine 10.51 g, 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum (0) catalyst 2.2 ppm, and 60 g of xylene into the three-necked flask. After the addition is complete, react at a constant temperature for 24 hours, and separate by vacuum distillation to obtain a silicon-rich anti-reflective coating resin at a pressure of 10 mmHg and a temperature of 40°C for 60 minutes.

[0059] Example 7

[0060] Add 120 g of toluene and 60 g of polymethylhydrogensiloxane (hydrogen content 1.6%) into a 500 mL three-necked reactor, install a condensation reflux device, stir and heat to 60° C. in a N2 atmosphere, then slowly drop 11.42 g of allyl glycidyl ether, 10.4 g of styrene, 2 g of catalyst H2PtCl6·6H2O, and 60 g of toluene into the three-necked flask. After the addition is completed, react at a constant temperature for 24 hours, and separate by vacuum distillation to obtain a silicon-rich anti-reflective coating resin at a pressure of 10 mmHg and a temperature of 40° C. for 60 minutes.

[0061] The silicon-rich anti-reflective coating resins of Examples 1-7 above were subjected to gel chromatography analysis to obtain the molecular weight and molecular weight distribution, as shown in Table 1.

[0062] Table 1 Molecular weight and molecular weight distribution of silicon-rich anti-reflective coating resin materials of Examples 1-7

[0063]

[0064] Application Example 1

[0065] The silicon-rich anti-reflection coating resin prepared in Example 1 was filtered using a PTFE filter membrane (pore size of 0.1 μm), and 0.2 g of the resin was dissolved in 9.8 g of propylene glycol ethyl ether solvent to obtain a silicon-rich anti-reflection coating sample 1.

[0066] The silicon-rich anti-reflective coating sample 1 was spin-coated into a film 1 .

[0067] Application Example 2

[0068] The silicon-rich anti-reflection coating resin prepared in Example 2 was filtered using a PTFE filter membrane (pore size of 0.1 μm), and 0.2 g of the resin was dissolved in 9.8 g of propylene glycol ethyl ether solvent to obtain a silicon-rich anti-reflection coating sample 2.

[0069] The silicon-rich anti-reflective coating sample 2 was spin-coated into a film 2 .

[0070] Application Example 3

[0071] The silicon-rich anti-reflection coating resin prepared in Example 3 was filtered using a PTFE filter membrane (pore size of 0.1 μm), and 0.2 g of the resin was dissolved in 9.8 g of propylene glycol ethyl ether solvent to obtain a silicon-rich anti-reflection coating sample 3.

[0072] The silicon-rich anti-reflective coating sample 3 was spin-coated into Film 3 .

[0073] Application Example 4

[0074] The silicon-rich anti-reflection coating resin prepared in Example 4 was filtered using a PTFE filter membrane (pore size of 0.1 μm), and 0.2 g of the resin was dissolved in 9.8 g of propylene glycol ethyl ether solvent to obtain a silicon-rich anti-reflection coating sample 4.

[0075] The silicon-rich anti-reflective coating sample 4 was spin-coated into a film 4 .

[0076] Application Example 5

[0077] The silicon-rich anti-reflection coating resin prepared in Example 5 was filtered using a PTFE filter membrane (pore size of 0.1 μm), and 0.2 g of the resin was dissolved in 9.8 g of propylene glycol ethyl ether solvent to obtain a silicon-rich anti-reflection coating sample 5.

[0078] The silicon-rich anti-reflective coating sample 5 was spin-coated into a film 5 .

[0079] Application Example 6

[0080] The silicon-rich anti-reflection coating resin prepared in Example 6 was filtered using a PTFE filter membrane (pore size of 0.1 μm), and 0.2 g of the resin was dissolved in 9.8 g of propylene glycol ethyl ether solvent to obtain a silicon-rich anti-reflection coating sample 6.

[0081] The silicon-rich anti-reflective coating sample 6 was spin-coated into a film 6 .

[0082] Application Example 7

[0083] The silicon-rich anti-reflection coating resin prepared in Example 7 was filtered using a PTFE filter membrane (pore size of 0.1 μm), and 0.2 g of the resin was dissolved in 9.8 g of propylene glycol ethyl ether solvent to obtain a silicon-rich anti-reflection coating sample 7.

[0084] The silicon-rich anti-reflective coating sample 7 was spin-coated into a film 7 .

[0085] Application Example 8

[0086] The silicon-rich anti-reflective coating sample 1 was immersed in the PGMEA solvent for 1 minute, and then the excess solvent was spin-coated.

[0087] Application Example 9

[0088] The silicon-rich anti-reflection coating sample 1 was stored in a constant temperature box at 40° C. for 30 days, then spin-coated on a 2-inch silicon wafer and baked to obtain a silicon-rich anti-reflection coating.

[0089] The optical parameters of the silicon-rich anti-reflection coatings of the above application examples 1-7 were characterized at 193 nm to obtain n, k values ​​and film thickness, as shown in Table 2.

[0090] Table 2 Si content, optical parameters and film thickness of silicon-rich anti-reflection coatings in Examples 1-7

[0091]

[0092] FL is the thickness of the silicon-rich anti-reflective coating obtained by spin coating and baking the newly prepared silicon-rich anti-reflective coating samples in Application Examples 1-7. In Application Example 8, FL is the thickness of the silicon-rich anti-reflective coating obtained by spin coating and baking the newly prepared silicon-rich anti-reflective coating sample after the solvent resistance test. In Application Example 9, FL is the thickness of the silicon-rich anti-reflective coating obtained by spin coating and baking the silicon-rich anti-reflective coating sample after heat preservation in a constant temperature box at 40°C for 30 days. It can be seen from Table 2 that the values ​​of FL in Application Example 1, Application Example 8 and Application Example 9 are similar, indicating that the silicon-rich anti-reflective coating has excellent storage stability and solvent resistance, and can still form a film layer with similar thickness and excellent solvent resistance after storage at a higher temperature for 30 days.

[0093] In summary, the present invention forms a linear polysiloxane by addition polymerization of a carbon-carbon double bond monomer containing an epoxy crosslinking group and a light-absorbing group on polymethylhydrogensiloxane, and prepares a silicon-rich anti-reflective coating resin by a silicon hydrogen addition polymerization reaction. This method improves the disadvantage of poor stability in preparing the resin, and fundamentally improves the storage stability and solvent resistance of the silicon-rich anti-reflective coating resin. There are a large number of Si-H bonds to ensure a high Si content, and at the same time, it contains light-absorbing groups to meet the regulation of optical parameters and contains epoxy crosslinking groups to regulate the crosslinking degree, which can meet the requirements for the etching rate and anti-reflection ability of the silicon-rich anti-reflective coating in different application scenarios.

[0094] The above is a specific embodiment of the present invention, which is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A silicon-rich anti-reflective coating resin, It is characterized in that It has a structure as shown in formula (I): Among them, R 1 is selected from epoxy groups containing 1 to 10 straight-chain carbon atoms or epoxy groups containing 1 to 10 cyclic carbon atoms; R 2 A group selected from the group containing phenyl, naphthyl, pyridyl, thienyl, benzyl; The ratio of x, y and z is 7-10:0.4-1:0.3-1, and the weight average molecular weight of the silicon-rich anti-reflective coating resin is 70,000-100,000.

2. The method for preparing the silicon-rich anti-reflective coating resin according to claim 1, It is characterized in that The following steps are involved: (1) dissolving polymethyl hydrogen siloxane in solvent 1 to obtain a mixed solution A; (2) dissolving a carbon-carbon double bond monomer containing an epoxy crosslinking group, a carbon-carbon double bond monomer containing a light absorbing group, and a catalyst in a second solvent to obtain a mixed solution B; (3) Adding mixed solution B dropwise into mixed solution A to carry out a reaction to obtain the silicon-rich anti-reflective coating resin.

3. The preparation method according to claim 2, It is characterized in that The hydrogen content of the polymethyl hydrogen siloxane is 1.4-1.8wt%.

4. The preparation method according to claim 2, It is characterized in that The carbon-carbon double bond monomer containing epoxy crosslinking groups is an epoxy carbon-carbon double bond monomer containing 1-10 straight-chain carbon atoms or an epoxy carbon-carbon double bond monomer containing 1-10 cyclic carbon atoms; the carbon-carbon double bond monomer containing light-absorbing groups is a carbon-carbon double bond monomer containing phenyl, naphthyl, pyridyl, thienyl or benzyl groups.

5. The preparation method according to claim 4, It is characterized in that The carbon-carbon double bond monomer containing epoxy crosslinking groups includes one or more of allyl glycidyl ether, epoxybutene, 1,2-epoxy-5-cyclooctene, 3,4-epoxy-1-cyclohexene, 1,2-epoxy-5-hexene, 4-vinyl epoxycyclohexane, 1,2-epoxy-9-decene, and 1,2-epoxy-4-vinylcyclohexane.

6. The preparation method according to claim 4, It is characterized in that The carbon-carbon double bond monomer containing a light-absorbing group includes one or more of styrene, 1-vinylnaphthalene, 6-methoxy-2-naphthylethylene, tetrakis-(3-pyridylbiphenyl)ethylene, 1,1,2,2-tetrakis(pyridin-4-yl)ethylene, 2-vinylpyridine, 1-phenyl-1-trimethylsiloxyethylene, 2,2-(1,2-vinyl)bithiophene, 2-vinylthiophene, benzyl vinyl ether, and 4-vinylbenzyl alcohol.

7. The preparation method according to any one of claims 2 to 6, It is characterized in that The repeating unit in the polymethylhydrogensiloxane is -(CH 3 The molar ratio of )SiO(H)-, the carbon-carbon double bond monomer containing an epoxy crosslinking group and the carbon-carbon double bond monomer containing a light absorbing group is 7-10:0.4-1:0.3-1.

8. The preparation method according to claim 2, It is characterized in that The catalyst comprises a Speier catalyst, a Custer catalyst, or a complex catalyst formed by chloroplatinic acid and ketones, cyclopentadiene, esters, alcohols, crown ethers, or polysiloxanes; the added amount of the catalyst is 0.0088%-0.01% of the total molar number of carbon-carbon double bonds in the raw material.

9. The preparation method according to claim 2, It is characterized in that In step (3), the reaction temperature is 30-120° C. and the reaction time is 10-72 h.

10. A silicon-rich anti-reflective coating, It is characterized in that The anti-reflective coating is obtained by spin coating the silicon-rich anti-reflective coating resin according to claim 1 on a semiconductor substrate and baking it.

Citation Information

Patent Citations

  • Antireflection coating for 193-nano-wavelength photolithography and preparation method and application thereof

    CN102051121A

  • Epoxy / organosilicon co-curing composite material for LED packaging and preparation method

    CN102977554A

  • Phenyl vinyl silicon resin for adhering base as well as preparation method and application thereof

    CN104710621A

  • Preparation method of epoxy modified phenyl hydrogen-containing silicone resin

    CN104961898A

  • Two-component normal-temperature curing epoxy modified MQ silicon resin coating

    CN114574097A

Cited By

  • Silicon-rich anti-reflection resin as well as preparation method and coating thereof

    CN121108488A

  • Silicon-rich anti-reflection resin as well as preparation method and coating thereof

    CN121471526A