Vibration-absorbing and fatigue-resistant epoxy structural adhesive for earthquake region and preparation method of vibration-absorbing and fatigue-resistant epoxy structural adhesive

Through the combination of modified epoxy resin and nanoparticles, the problem of the decrease in strength of epoxy structural glue in the seismic environment is solved, and the high toughness and anti-aging performance are improved, which is suitable for building reinforcement in earthquake areas.

CN118995113APending Publication Date: 2024-11-22SICHUAN INSITITUTE OF BUILDING RES
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410784399.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The strength of the existing epoxy structural adhesives decreases during toughening, making it difficult to meet the requirements of fatigue resistance, aging resistance and vibration absorption capabilities in the earthquake-zone environment.

Method used

Using modified epoxy resin and modified nanoparticles, styrene is introduced into the Mannich reaction for long chaining, combined with coupling agent and active diluent, a vibration-absorbing and fatigue-resistant epoxy structural glue for earthquake zones is prepared. Enhance its toughness and anti-aging properties.

Benefits of technology

While not reducing the strength of epoxy structural glue, it significantly improves its toughness and anti-aging properties, enhances stress tolerance and impact energy absorption capacity, and is suitable for building reinforcement projects in earthquake areas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004898171540000011
    Figure BDA0004898171540000011
  • Figure BDA0004898171540000101
    Figure BDA0004898171540000101
  • Figure BDA0004898171540000111
    Figure BDA0004898171540000111
Patent Text Reader

Abstract

The invention belongs to the technical field of adhesives, and discloses a vibration-absorbing fatigue-resistant epoxy structural adhesive for a seismic region and a preparation method thereof, the vibration-absorbing fatigue-resistant epoxy structural adhesive is mainly used for reinforcing engineering of buildings in the seismic region, and the vibration-absorbing fatigue-resistant epoxy structural adhesive comprises the following components in parts by weight: 100-110 parts of modified epoxy resin, 1-5 parts of modified nanoparticles, 3-6 parts of a first coupling agent, 0-5 parts of a reactive diluent and 30-50 parts of a flexible chain curing agent; wherein the flexible chain curing agent is prepared by mixing modified Mannich base prepared from polyamine, formaldehyde and styrene modified phenol with at least two of alicyclic amine, aliphatic amine, heterocyclic compound and modified amine. According to the vibration-absorbing and fatigue-resistant epoxy structural adhesive for the earthquake region, the modified epoxy resin is used, the modified nano-particles are introduced, and the modified Mannich base which is obtained by introducing styrene for long chain is selected, so that the epoxy structural adhesive is toughened, a reinforcing effect can be achieved, and the anti-aging capability of the structural adhesive can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of adhesives, and specifically relates to a vibration-absorbing and fatigue-resistant epoxy structural adhesive for use in earthquake zones and a preparation method thereof. Background Art

[0002] Epoxy structural adhesives are polymers that form a three-dimensional network through the reaction of epoxy groups and curing agents. They have many advantages, such as high bonding strength, low shrinkage, creep resistance, good processing performance, excellent electrical insulation performance, and chemical corrosion resistance. They are widely used in the fields of construction, aviation, and electronics. After the Wenchuan earthquake in Sichuan, epoxy structural adhesives were used extensively in building reinforcement projects, which placed strict requirements on the fatigue resistance, aging resistance, stress resistance, and vibration absorption capabilities of the adhesives.

[0003] In order to improve the vibration absorption and fatigue resistance of epoxy structural adhesives, rubber elastomers are generally used in the industrial field to toughen epoxy resins. However, the strength of most epoxy structural adhesives will decrease while being toughened, which seriously affects the performance of epoxy structural adhesives in seismic environments.

[0004] Therefore, a new epoxy structural adhesive is needed to overcome its current technical defects. Summary of the invention

[0005] The problem that the present application aims to solve is to provide a vibration-absorbing and fatigue-resistant epoxy structural adhesive for use in earthquake zones and a preparation method thereof, using modified epoxy resin and introducing modified nanoparticles, and at the same time selecting a modified Mannich base that introduces styrene for long-chaining, which can not only toughen the epoxy structural adhesive, but also have a reinforcing effect and can improve the anti-aging ability of the structural adhesive.

[0006] In order to solve the above technical problems, this application adopts the following technical solutions:

[0007] In one aspect, the present application provides a vibration-absorbing and fatigue-resistant epoxy structural adhesive for use in earthquake-prone areas. The vibration-absorbing and fatigue-resistant epoxy structural adhesive for use in earthquake-prone areas comprises, by weight:

[0008]

[0009] The method for preparing the flexible chain curing agent includes: adding styrene and a first catalyst to phenol, performing a Friedel-Wohn substitution reaction, and obtaining a modified phenol; adding one of a first diamine and a first polyamine to the modified phenol, performing a first stirring, and obtaining a mixed solution; adding formaldehyde to the mixed solution, performing a Mannich reaction, and obtaining a brown-red transparent liquid; performing a first drying on the brown-red transparent liquid to obtain a modified Mannich base; and mixing at least two of alicyclic amines, fatty amines, heterocyclic compounds, and modified amines with the modified Mannich base to obtain the flexible chain curing agent.

[0010] In the above technical scheme, the modified epoxy resin itself has good toughness. The addition of modified nanoparticles can further improve the toughness without destroying the strength of the epoxy structural adhesive. The use of coupling agents can promote the combination of modified epoxy resin and modified nanoparticles, increase the strength and toughness of the epoxy structural adhesive, and prevent the nanoparticles from agglomerating, so that they are evenly dispersed in the epoxy resin matrix. The addition of active diluents can improve the viscosity and fluidity of the adhesive, control the curing speed, and participate in the curing reaction. The flexible chain curing agent can improve the flexibility and impact resistance of the epoxy structural adhesive. The conjugated double bonds of styrene have good reactivity and can participate in the Mannich base reaction. After using styrene to modify phenol, it can react with aldehydes and amines to obtain a modified Mannich base with a long-chain molecular structure, which improves the toughness of the epoxy structural adhesive. Mixing the modified Mannich base with other amines can further improve the toughness of the adhesive and improve the aging resistance of the structural adhesive.

[0011] In some embodiments, the weight ratio of the phenol to the styrene is 1:1.

[0012] In the above technical solution, limiting the weight ratio of phenol to styrene can greatly improve the toughness and strength of the final epoxy structural adhesive.

[0013] In some embodiments, the weight ratio of one of the first diamine and the first polyamine to the modified phenol is 1:1.5-2.

[0014] In the above technical solution, limiting the weight ratio of modified phenol to polyamine can greatly improve the toughness and strength of the final epoxy structural adhesive.

[0015] In some embodiments, the first coupling agent includes one of KH550 and KH560.

[0016] In some examples, the KH550 is the KH550 produced by Guangdong Zhongyu Wohao, and the KH560 is the KH560 produced by Guangdong Zhongyu Wohao.

[0017] In the above technical solution, KH550 or KH560 can effectively improve the compatibility between the modified nanoparticles and the modified epoxy resin, enhance the interfacial bonding force between the two, improve the overall performance of the epoxy structural adhesive, and can improve the mechanical strength and weather resistance of the material.

[0018] In some embodiments, the first catalyst comprises NaOH.

[0019] In the above technical solution, NaOH has a high catalytic efficiency and can make the reaction of phenol and styrene to prepare modified phenol complete faster.

[0020] In some embodiments, the first diamine includes one of hexamethylenediamine and toluenediamine.

[0021] In some embodiments, the first polyamine comprises diethylenetriamine.

[0022] In some embodiments, the alicyclic amine includes one of m-isophoronediamine and menthanediamine.

[0023] In the above technical solution, limiting the types of fatty amines can improve the flexural strength and chemical resistance of the epoxy structural adhesive.

[0024] In some embodiments, the heterocyclic compound comprises N-aminoethylpiperazine.

[0025] In the above technical solution, limiting the types of heterocyclic compounds can improve the bending strength and chemical resistance of the epoxy structural adhesive.

[0026] In some embodiments, the fatty amine comprises a polyether amine.

[0027] In the above technical solution, limiting the types of fatty amines can improve the flexural strength and chemical resistance of the epoxy structural adhesive.

[0028] In some embodiments, the modified amine includes a modified amine obtained by reacting one of an epoxy compound and an unsaturated nitrile compound with a second diamine and a second polyamine, the epoxy compound includes one of epichlorohydrin and butylene oxide, the unsaturated nitrile compound includes acrylonitrile, the second diamine includes one of hexamethylenediamine and meta-xylylenediamine, and the second polyamine includes diethylenetriamine.

[0029] In the above technical scheme, limiting the types of modified amines can improve bending strength, chemical resistance, impact resistance or toughness, and limiting the types of epoxy compounds, unsaturated nitrile compounds, diamines and polyamines can make the obtained modified amines have good thermal stability, mechanical strength and chemical resistance.

[0030] In some embodiments, the Friedel substitution reaction is carried out under heating with magnetic stirring, the temperature of the Friedel substitution reaction is 100-150° C., and the time of the Friedel substitution reaction is 2-4 h.

[0031] In the above technical solution, limiting the temperature of the Friedel-Wolfsson substitution reaction can make the reaction of styrene and phenol more thorough, and carrying out the reaction under magnetic stirring can accelerate the reaction speed.

[0032] In some embodiments, the temperature of the Mannich reaction is 70-80° C., and the time of the Mannich reaction is 50-70 min.

[0033] In the above technical solution, limiting the temperature of the Mannich reaction can make the reaction of formaldehyde, modified phenol and hexamethylenediamine more thorough.

[0034] In some embodiments, the first stirring method includes vacuum stirring. For example, the temperature of the vacuum stirring is 60°C.

[0035] In the above technical solution, vacuum stirring can improve the mixing efficiency of hexamethylenediamine and modified phenol, and at the same time, it helps to eliminate bubbles and residues in the mixed solution, thereby ensuring the purity of the modified Mannich base obtained subsequently.

[0036] In some embodiments, the method of adding formaldehyde to the mixed solution includes uniform dripping, for example, the uniform dripping speed is 5 mL / min.

[0037] In the above technical solution, formaldehyde is uniformly added dropwise to the mixed solution of hexamethylenediamine and modified phenol at a speed of 5 mL / min, which can effectively prevent explosion.

[0038] In some embodiments, the first drying method includes vacuum dehydration. For example, the first drying temperature is 50° C. and the first drying time is 4 hours.

[0039] In the above technical solution, the vacuum dehydration method is used to remove the water and other substances generated during the reaction, thereby improving the purity of the modified Mannich base and preventing the modified Mannich base from being oxidized or contaminated by oxygen and other gases.

[0040] In some embodiments, the method for preparing the modified epoxy resin comprises:

[0041] After the polyol is dried for a second time, isocyanate and a second catalyst are added, and a second stirring and addition reaction is performed to obtain a polyurethane prepolymer; and the polyurethane prepolymer is added to an epoxy resin to perform a grafting reaction to obtain the modified epoxy resin.

[0042] In the above technical solution, the introduction of polyurethane prepolymer to graft-modify epoxy resin can enhance the toughness of the epoxy resin itself.

[0043] In some embodiments, the weight ratio of the polyol to the isocyanate is 1:0.9-1.3.

[0044] In the above technical solution, limiting the weight ratio of polyol to isocyanate can achieve a faster reaction rate.

[0045] In some embodiments, the weight ratio of the polyurethane prepolymer to the epoxy resin is 1:15-20.

[0046] In the above technical solution, limiting the weight ratio of the polyurethane prepolymer to the epoxy resin can greatly improve the toughness of the obtained modified epoxy resin.

[0047] In some embodiments, the isocyanate includes dicyclohexylmethylene diisocyanate.

[0048] In the above technical solution, the adhesive prepared using dicyclohexylmethylene diisocyanate has excellent properties such as strength, toughness and wear resistance.

[0049] In some embodiments, the second catalyst comprises triethylenediamine.

[0050] In the above technical solution, triethylenediamine has extremely high catalytic activity for the reaction of isocyanate and polyol.

[0051] In some embodiments, the polyol comprises polytetramethylene glycol.

[0052] In the above technical solution, the product made from polytetrahydrofuran alcohol has the advantages of good flexibility, wear resistance, high mechanical strength and aging resistance.

[0053] In some embodiments, the epoxy resin includes one of E51 and E44, such as E51 epoxy resin and E44 epoxy resin of Baling Petrochemical Co., Ltd.

[0054] In the above technical solution, E51 epoxy resin and E44 resin have extremely strong bonding force and can firmly adhere to the surfaces of various materials.

[0055] In some embodiments, the temperature of the addition reaction is 70-80° C., and the time of the addition reaction is 1.5-2.5 h.

[0056] In the above technical solution, limiting the temperature of the addition reaction can make the reaction between isocyanate and polyol more thorough.

[0057] In some embodiments, the grafting reaction time is 1.5 to 2.5 hours.

[0058] In the above technical solution, limiting the time of the grafting reaction can make the grafting reaction of the polyurethane prepolymer and the epoxy resin more thorough.

[0059] In some embodiments, the second drying method includes vacuum dehydration. For example, the second drying temperature is 60° C., and the second drying time is 2 hours.

[0060] In the above technical solution, the vacuum dehydration method is adopted to remove the water and other substances in the polyol, thereby improving the purity of the obtained polyurethane prepolymer.

[0061] In some embodiments, the second stirring method includes magnetic stirring.

[0062] In the above technical solution, magnetic stirring can improve the mixing efficiency of isocyanate, catalyst and polyol, and can react during the stirring process, so that the reaction rate is effectively improved.

[0063] In some embodiments, the method of preparing the modified nanoparticles comprises:

[0064] The nanoparticles are dispersed in an ethanol aqueous solution to obtain a dispersion; a second coupling agent is added to the dispersion, and a third stirring and suction filtration are performed to obtain a precipitate; and the precipitate is dried for a third time to obtain modified nanoparticles.

[0065] In some embodiments, the amount of the nanoparticles is 1 to 10 parts.

[0066] In some embodiments, the second coupling agent is used in an amount of 2 to 8 parts.

[0067] In some embodiments, the third stirring method includes vacuum stirring. For example, the temperature of the vacuum stirring is 20-35° C., and the time of the vacuum stirring is 45 minutes.

[0068] In the above technical solution, the vacuum stirring method is adopted to enable the coupling agent to introduce more reaction sites on the surface of the nanoparticles.

[0069] In some embodiments, the third drying method includes vacuum drying. For example, the vacuum drying temperature is 80° C. to 120° C., and the vacuum drying time is 3 hours.

[0070] In the above technical solution, the vacuum drying method is adopted to remove the moisture, bubbles and other substances in the modified nanoparticles, thereby improving the purity of the obtained modified nanoparticles.

[0071] In some examples, the nanoparticles include gas-phase SiO 2 nanoparticles.

[0072] In the above technical solution, the gas-phase SiO2 nanoparticles have a small particle size and a large specific area, and can be better dispersed in the epoxy resin, forming an effective toughening network in the epoxy resin matrix, thereby improving the toughness of the material.

[0073] In some examples, the second coupling agent includes KH550.

[0074] Exemplarily, the KH550 is the KH550 produced by Guangdong Zhongyu Wohao.

[0075] In the above technical solution, the coupling agent KH550 is used to modify the SiO2 nanoparticles, which can improve the compatibility of the SiO2 nanoparticles with the epoxy resin and improve the overall performance of the epoxy structural adhesive.

[0076] On the other hand, the present application provides a method for preparing the above-mentioned vibration-absorbing and fatigue-resistant epoxy structural adhesive for earthquake zones. The method comprises the following steps: adding the modified nanoparticles, the first coupling agent and the reactive diluent to the modified epoxy resin, performing a fourth stirring to obtain a mixture; and mixing the mixture with the flexible chain curing agent to obtain the vibration-absorbing and fatigue-resistant epoxy structural adhesive for earthquake zones.

[0077] In the above technical solution, the modified nanoparticles can be evenly dispersed in the epoxy resin, which can improve the toughness of the epoxy resin while also increasing the strength of the epoxy resin.

[0078] In some embodiments, the fourth stirring method includes vacuum stirring. For example, the temperature of the vacuum stirring is 20° C., and the time of the vacuum stirring is 40 minutes.

[0079] In the above technical solution, the vacuum stirring method is adopted to improve the mixing efficiency of the modified epoxy resin, modified nanoparticles, coupling agent and active diluent, and at the same time, it helps to eliminate bubbles and residues in the mixed liquid, thereby ensuring the purity of the subsequently obtained epoxy resin adhesive.

[0080] This application has the following beneficial effects:

[0081] 1. The present application provides a vibration-absorbing and fatigue-resistant epoxy structural adhesive for use in earthquake zones, in which a polyurethane prepolymer is introduced into the epoxy resin for grafting modification, thereby toughening the epoxy resin itself and ultimately improving the toughness of the epoxy structural adhesive.

[0082] 2. The present application provides a vibration-absorbing and fatigue-resistant epoxy structural adhesive for use in earthquake zones. In the preparation of a flexible chain curing agent, styrene-modified phenol is used to carry out a Mannich base reaction to obtain a modified Mannich base, which can introduce flexible long chains into the molecular structure to solve the problems of high brittleness and poor toughness of the epoxy structural adhesive. The modified Mannich base is then mixed with a variety of amines to further improve the toughness of the epoxy structural adhesive.

[0083] 3. The present application provides a vibration-absorbing and fatigue-resistant epoxy structural adhesive for use in earthquake zones. The modified nanoparticles used in the epoxy resin adhesive can be evenly dispersed in the epoxy resin, which toughens the epoxy structural adhesive without reducing the strength of the epoxy structural adhesive.

[0084] 4. The present application provides a vibration-absorbing and fatigue-resistant epoxy structural adhesive for use in earthquake zones. The modified epoxy resin, flexible chain curing agent and modified nanoparticles will all participate in the curing reaction and will not reduce the cross-linking density of the adhesive and affect the strength of the adhesive. DETAILED DESCRIPTION

[0085] The technical solutions in some embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments provided by the present application, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present application.

[0086] In the following, the terms "first", "second", etc. are used for descriptive purposes only and are not to be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first", "second", etc. may explicitly or implicitly include one or more of the features.

[0087] When describing some embodiments, the expression "A and / or B" may be used. It is easy to understand that "A and / or B" includes the following three combinations: only A, only B, and a combination of A and B.

[0088] When describing some embodiments, the expressions "at least one of A, B and C" and "at least one of A, B or C" may be used, both of which have the same meaning and include the following combinations of A, B and C: A only, B only, C only, the combination of A and B, the combination of A and C, the combination of B and C, and the combination of A, B and C.

[0089] Example 1

[0090] The modified SiO2 nanoparticles were prepared as follows:

[0091] S11. Dispersing 1 part of gas-phase SiO2 nanoparticles in an aqueous solution of ethanol to obtain a dispersion;

[0092] S12. Add 2 parts of KH550 to the above dispersion, stir under vacuum at 20°C for 45 minutes, and then filter to obtain a precipitate;

[0093] S13. The above precipitate was dried under vacuum at 80°C for 3 h to obtain modified SiO2 nanoparticles.

[0094] Example 2

[0095] The method for preparing modified SiO2 nanoparticles in this embodiment refers to Example 1; wherein, the difference between Example 2 and Example 1 is only that:

[0096] In S11, the amount of the gas-phase SiO2 nanoparticles is 5 parts;

[0097] In S12, the amount of KH550 is 5 parts, and the temperature of the vacuum stirring is 28° C.;

[0098] In S13, the vacuum drying temperature is 100°C.

[0099] Example 3

[0100] The method for preparing modified SiO2 nanoparticles in this embodiment refers to Example 1; wherein, the difference between Example 3 and Example 1 is only that:

[0101] In S11, the amount of the gas-phase SiO2 nanoparticles is 10 parts;

[0102] In S12, the amount of KH550 is 8 parts, and the temperature of the vacuum stirring is 35° C.;

[0103] In S13, the vacuum drying temperature is 120°C.

[0104] Example 4

[0105] The modified epoxy resin was prepared according to the following preparation method:

[0106] S21. After 7 parts of polytetrahydrofuran alcohol were vacuum dehydrated at 60° C. for 2 h, 6.3 parts of dicyclohexylmethylene diisocyanate and 1 part of triethylenediamine were added, and after stirring and mixing, an addition reaction was carried out at 70° C. for 1.5 h to obtain a polyurethane prepolymer;

[0107] S22. Add 7 parts of the above polyurethane prepolymer to 105 parts of E51 epoxy resin and carry out grafting reaction for 1.5 hours to obtain a modified epoxy resin.

[0108] Example 5

[0109] The method for preparing the modified epoxy resin in this embodiment refers to Example 4; wherein, the difference between Example 5 and Example 4 is only that:

[0110] In S21, the amount of dicyclohexylmethylene diisocyanate is 7.7 parts, the addition reaction temperature is 75°C, and the addition reaction time is 2 hours;

[0111] In S22, the amount of E51 epoxy resin used was 119 parts, and the grafting reaction time was 2 hours.

[0112] Example 6

[0113] The method for preparing the modified epoxy resin in this embodiment refers to Example 4; wherein, the difference between Example 6 and Example 4 is only that:

[0114] In S21, the amount of dicyclohexylmethylene diisocyanate used is 9.1 parts, the addition reaction temperature is 80°C, and the addition reaction time is 2.5 hours;

[0115] In S22, the amount of E44 epoxy resin used was 140 parts, and the grafting reaction time was 2.5 hours.

[0116] Example 7

[0117] Prepare the modified Mannich base as follows:

[0118] S31. Add 2 parts of styrene and NaOH to 2 parts of phenol, start magnetic stirring, and perform a Fourier substitution reaction at 100° C. for 2 h to obtain modified phenol;

[0119] S32. Add 3 parts of hexamethylenediamine to 2 parts of the modified phenol and stir under vacuum at 60 ° C to obtain a mixed solution;

[0120] S33. Two portions of formaldehyde were uniformly added dropwise to the mixture at a rate of 5 mL / min, and the mixture was heated to 70°C for 50 min for Mannich reaction to obtain a brown-red transparent solution;

[0121] S34. The brown-red transparent solution was dehydrated under vacuum at 50° C. for 4 h to obtain a modified Mannich base.

[0122] Example 8

[0123] The method for preparing the modified Mannich base in this embodiment refers to Example 7; wherein, the difference between Example 8 and Example 7 is only that:

[0124] In S31, the temperature of the Fourier substitution reaction is 125°C, and the Fourier substitution reaction time is 3 h;

[0125] In S32, the amount of m-xylylenediamine is 4 parts;

[0126] In S33, the temperature of the Mannich reaction is 75°C, and the time of the Mannich reaction is 60 minutes.

[0127] Example 9

[0128] The method for preparing the modified Mannich base in this embodiment refers to Example 7; wherein, the difference between Example 9 and Example 7 is only that:

[0129] In S31, the temperature of the Fourier substitution reaction is 150°C, and the Fourier substitution reaction time is 4 h;

[0130] In S32, the amount of diethylenetriamine used is 3.3 parts;

[0131] In S33, the temperature of the Mannich reaction is 80°C, and the time of the Mannich reaction is 70 minutes.

[0132] Example 10

[0133] The modified aromatic amines were prepared as follows:

[0134] S41: 8 parts of NaOH (50%) are added to 100 parts of m-phenylenediamine, and N2 is continuously charged and stirred. At the same time, 10 parts of epichlorohydrin are added dropwise at 60° C., and after the addition is completed, the mixture is reacted for 2 hours, and then heated to 95° C. and reacted for 2 hours to obtain a reaction solution;

[0135] S42: After filtering the reaction solution, heating it to 130°C and performing reduced pressure distillation to obtain a modified aromatic amine.

[0136] Embodiment 11

[0137] The modified fatty amines were prepared as follows:

[0138] S51: 0.1 parts of skeleton nickel are added dropwise to 103 parts of diethylenetriamine, and stirred to obtain a mixed solution;

[0139] S52: 100 parts of butyl propylene oxide are added dropwise to the above mixed solution, heated to 60° C. and reacted for 2 hours to obtain a modified fatty amine.

[0140] Example 12

[0141] Follow these steps to prepare Michael addition modified fatty amines:

[0142] S61: 53 parts of acrylonitrile are added dropwise to 116 parts of an ethanol solution of hexamethylenediamine at a temperature below 50°C, and after the addition is completed, the temperature is raised to 65°C for 2h Michael addition to obtain a reaction solution;

[0143] S62 distills ethanol under reduced pressure to obtain Michael addition modified fatty amine.

[0144] Example 13

[0145] Follow the steps below to prepare a vibration-absorbing, fatigue-resistant epoxy structural adhesive for earthquake zones:

[0146] S71. 5 parts of the modified SiO2 nanoparticles prepared in Example 1, 3 parts of KH550 and 5 parts of a reactive diluent were added to 110 parts of the modified epoxy resin prepared in Example 4, and stirred under vacuum at 20 ° C for 40 min to obtain a mixture;

[0147] S72. 20 parts of the modified Mannich base prepared in Example 7, 20 parts of a polyetheramine and 20 parts of isophorone diamine were stirred and mixed to obtain a flexible chain curing agent;

[0148] S73. Add 30 parts of the above-mentioned flexible chain curing agent to 100 parts of the above-mentioned mixture and mix them evenly to obtain a vibration-absorbing and fatigue-resistant epoxy structural adhesive for earthquake-affected areas.

[0149] Embodiment 14

[0150] The method for preparing the vibration-absorbing and fatigue-resistant epoxy structural adhesive for earthquake zones in this embodiment refers to Example 13; the difference between Example 14 and Example 13 is only that:

[0151] S71. 3 parts of the modified SiO2 nanoparticles prepared in Example 2, 5 parts of KH560 and 3 parts of a reactive diluent were added to 105 parts of the modified epoxy resin prepared in Example 5, and stirred under vacuum at 20 ° C for 40 min to obtain a mixture;

[0152] S72. 15 parts of the modified Mannich base prepared in Example 8, 15 parts of a polyetheramine, 15 parts of a modified aromatic amine prepared in Example 10 and 15 parts of menthane diamine were stirred and mixed to obtain a flexible chain curing agent;

[0153] S73. Add 40 parts of the above-mentioned flexible chain curing agent to 100 parts of the above-mentioned mixture and mix them evenly to obtain a vibration-absorbing and fatigue-resistant epoxy structural adhesive for earthquake-affected areas.

[0154] Embodiment 15

[0155] S71. 1 part of the modified SiO2 nanoparticles prepared in Example 3 and 6 parts of KH550 were added to 100 parts of the modified epoxy resin prepared in Example 6, and stirred for 40 min to obtain a mixture;

[0156] S72. 10 parts of the modified Mannich base prepared in Example 9, 10 parts of the polyetheramine, 10 parts of the modified aromatic amine prepared in Example 10, 10 parts of the modified fatty amine prepared in Example 11, 10 parts of the Michael addition modified fatty amine prepared in Example 12 and 10 parts of N-aminoethylpiperazine were stirred and mixed to obtain a flexible chain curing agent;

[0157] S73. Add 100 parts of the above mixture to 50 parts of the above flexible chain curing agent and mix evenly to obtain a vibration-absorbing and fatigue-resistant epoxy structural adhesive for earthquake-affected areas.

[0158] Comparative Example 1

[0159] The method for preparing the vibration-absorbing and fatigue-resistant epoxy structural adhesive for earthquake zones in this comparative example refers to Example 13; wherein, the difference between Comparative Example 1 and Example 13 is only that:

[0160] In S71, the modified epoxy resin prepared in Example 4 is replaced with epoxy resin E51;

[0161] In S72, the modified Mannich base prepared in Example 7 is replaced with a Mannich base prepared by using phenol, formaldehyde and hexamethylenediamine in a weight ratio of 1:1:1.5.

[0162] Comparative Example 2

[0163] The method for preparing the vibration-absorbing and fatigue-resistant epoxy structural adhesive for earthquake zones in this comparative example is referenced to Example 13; wherein, the difference between Comparative Example 2 and Example 13 is only that:

[0164] In S71, the modified SiO2 nanoparticles prepared in Example 1 are replaced with SiO2 nanoparticles;

[0165] In S72, the modified Mannich base prepared in Example 7 is replaced with a Mannich base prepared by using phenol, formaldehyde and hexamethylenediamine in a weight ratio of 1:1:1.5.

[0166] Comparative Example 3

[0167] The method for preparing the vibration-absorbing and fatigue-resistant epoxy structural adhesive for earthquake zones in this comparative example refers to Example 13; wherein, the difference between Comparative Example 3 and Example 13 is only that:

[0168] In S71, the modified SiO2 nanoparticles prepared in Example 1 are replaced by SiO2 nanoparticles, and the modified epoxy resin prepared in Example 4 is replaced by epoxy resin E51.

[0169] Comparative Example 4

[0170] The method for preparing the vibration-absorbing and fatigue-resistant epoxy structural adhesive for earthquake zones in this comparative example refers to Example 13; wherein, the difference between Comparative Example 4 and Example 13 is only that:

[0171] In S71, the modified SiO2 nanoparticles prepared in Example 1 are replaced with SiO2 nanoparticles, and the modified epoxy resin prepared in Example 4 is replaced with epoxy resin E51;

[0172] In S72, the modified Mannich base prepared in Example 7 is replaced with a Mannich base prepared by using phenol, formaldehyde and hexamethylenediamine in a weight ratio of 1:1:1.5.

[0173] Experimental Example 1

[0174] The indexes of structural adhesive for bonding fiber composite materials in GB 50728 were selected as references to test the requirements for mechanical properties and durability of epoxy structural adhesives prepared in Examples 15 to 35 and Comparative Examples 1 to 3. The test results are shown in the following table:

[0175]

[0176]

[0177] Table 1

[0178] It can be seen from the above table that the vibration-absorbing and fatigue-resistant epoxy structural adhesive for earthquake-stricken areas described in the present application uses polyurethane prepolymer to modify the epoxy resin to achieve the purpose of toughening. At the same time, the use of modified SiO2 nanoparticles can not only toughen the epoxy structural adhesive, but also have a reinforcing effect. Moreover, the Mannich base prepared from modified phenol is mixed with other amines to further enhance and toughen the epoxy structural adhesive. The vibration-absorbing and fatigue-resistant epoxy structural adhesive for earthquake-stricken areas provided by the present application not only has good stress bearing capacity, but also has excellent toughness. At the same time, it can disperse and absorb impact energy, and effectively improves the aging resistance, prolongs the service life of the product, and can be widely used in building reinforcement projects in earthquake-stricken areas.

[0179] The above is only a preferred embodiment of the present application. It should be understood that the present application is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the concept described herein through the above teachings or the technology or knowledge in the relevant field. The changes and modifications made by those skilled in the art shall not deviate from the spirit and scope of the present application, and shall be within the scope of protection of the claims attached to the present application.

Claims

1. Vibration-absorbing and fatigue-resistant epoxy structural adhesive for earthquake-affected areas, characterized in that: In parts by weight: Wherein, the method for preparing the flexible chain curing agent comprises: Adding styrene and the first catalyst to phenol to carry out a Friedel-Wohr substitution reaction to obtain modified phenol; Adding one of a first diamine and a first polyamine to the modified phenol, performing a first stirring, and obtaining a mixed solution; Adding formaldehyde to the mixed solution to perform a Mannich reaction to obtain a brown-red transparent liquid; performing a first drying on the brown-red transparent liquid to obtain a modified Mannich base; and At least two of alicyclic amines, fatty amines, heterocyclic compounds and modified amines are mixed with the modified Mannich base to obtain the flexible chain curing agent.

2. The vibration-absorbing and fatigue-resistant epoxy structural adhesive for earthquake-affected areas according to claim 1, characterized in that: The weight ratio of the phenol to the styrene is 1:1; And / or, the weight ratio of one of the first diamine and the first polyamine to the modified phenol is 1:1.5-2.

3. The vibration-absorbing and fatigue-resistant epoxy structural adhesive for earthquake-affected areas according to claim 1, characterized in that: The first coupling agent includes one of KH550 and KH560; and / or, the first catalyst comprises NaOH; and / or, the first diamine comprises one of hexamethylenediamine and toluenediamine; and / or, the first polyamine comprises diethylenetriamine; And / or, the alicyclic amine includes one of m-isophorone diamine and menthane diamine; and / or, the heterocyclic compound comprises N-aminoethylpiperazine; and / or, the fatty amine comprises a polyetheramine; And / or, the modified amine includes a modified amine obtained by reacting one of an epoxy compound and an unsaturated nitrile compound with a second diamine and a second polyamine, the epoxy compound includes one of epichlorohydrin and butylene oxide, the unsaturated nitrile compound includes acrylonitrile, the second diamine includes one of hexamethylenediamine and meta-xylylenediamine, and the second polyamine includes diethylenetriamine.

4. The vibration-absorbing and fatigue-resistant epoxy structural adhesive for earthquake-affected areas according to claim 1, characterized in that: The Fourier substitution reaction is carried out under the condition of magnetic stirring, the temperature of the Fourier substitution reaction is 100-150° C., and the time of the Fourier substitution reaction is 2-4 hours; And / or, the temperature of the Mannich reaction is 70-80° C., and the time of the Mannich reaction is 50-70 min.

5. The vibration-absorbing and fatigue-resistant epoxy structural adhesive for earthquake-affected areas according to claim 1, characterized in that: The method for preparing the modified epoxy resin comprises: After the polyol is subjected to a second drying, isocyanate and a second catalyst alcohol are added, and a second stirring and addition reaction is performed to obtain a polyurethane prepolymer; and The polyurethane prepolymer is added to the epoxy resin to carry out a grafting reaction to obtain the modified epoxy resin.

6. The vibration-absorbing and fatigue-resistant epoxy structural adhesive for earthquake-affected areas according to claim 5, characterized in that: The weight ratio of the polyol to the isocyanate is 1:0.9-1.3; And / or, the weight ratio of the polyurethane prepolymer to the epoxy resin is 1:15-20.

7. The vibration-absorbing and fatigue-resistant epoxy structural adhesive for earthquake-affected areas according to claim 5, characterized in that: The isocyanate includes dicyclohexylmethylene diisocyanate; and / or, the second catalyst comprises triethylenediamine; and / or, the polyol comprises polytetrahydrofuranol; And / or, the epoxy resin includes one of E44 and E51.

8. The vibration-absorbing and fatigue-resistant epoxy structural adhesive for earthquake-affected areas according to claim 5, characterized in that: The temperature of the addition reaction is 70-80°C, and the time of the addition reaction is 1.5-2.5h; And / or, the grafting reaction time is 1.5 to 2.5 hours.

9. The vibration-absorbing and fatigue-resistant epoxy structural adhesive for earthquake-affected areas according to claim 1, characterized in that: The method for preparing the modified nanoparticles comprises: dispersing the nanoparticles in an aqueous solution of ethanol to obtain a dispersion; adding a second coupling agent to the dispersion, performing a third stirring and suction filtration to obtain a precipitate; and The precipitate is subjected to a third drying to obtain modified nanoparticles; Wherein, the nanoparticles include gas-phase SiO2 nanoparticles; The second coupling agent includes KH550.

10. A method for preparing the vibration-absorbing and fatigue-resistant epoxy structural adhesive for earthquake zones as claimed in any one of claims 1 to 9, characterized in that: The following steps are involved: adding the modified nanoparticles, the first coupling agent and the reactive diluent to the modified epoxy resin, and performing a fourth stirring to obtain a mixture; and The mixture is mixed with the flexible chain curing agent to obtain the vibration-absorbing and fatigue-resistant epoxy structural adhesive for the seismic zone.

Citation Information

Cited By

  • Wind power blade structural adhesive for wind power grade CFRP reinforcing rib and preparation method of wind power blade structural adhesive

    CN122146213A