Water-resistant and high-temperature-resistant flexible phase change material as well as preparation method and application thereof

By crosslinking phase change polymer materials with micron-level aerogel particles, flexible phase change materials that are resistant to water and high temperatures are prepared, which solves the problems of liquid phase leakage and shape stability in the prior art, and realizes high heat storage and multiple Functional performance, suitable for a variety of application scenarios.

CN118995141APending Publication Date: 2024-11-22SUZHOU INST OF NANO TECH & NANO BIONICS CHINESE ACEDEMY OF SCI
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411077982.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Problems such as liquid phase leakage in high-temperature environments limit their practical application, and composite materials are difficult to balance between shape stability and energy storage density, the preparation method is complex, and the circulation life is insufficient.

Method used

The reactive phase change polymer material is used to combine with micron-scale aerogel particles to prepare water and high temperature resistant flexible phase change materials through cross-linking reactions, and the large porosity and high specific surface area of ​​the aerogel are used to improve shape stability and Thermal hysteresis.

Benefits of technology

It realizes flexible, water-resistant and high-temperature phase change materials, with excellent mechanical, hydrophobic and moisture-permeable properties, and can provide high heat storage capacity in a relatively small volume, suitable for thermal insulation, hydrophobic and moisture-permeable gas materials and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118995141A_ABST
    Figure CN118995141A_ABST
Patent Text Reader

Abstract

The invention discloses a water-resistant and high-temperature-resistant flexible phase change material as well as a preparation method and application thereof. The preparation method comprises the following steps: providing a phase-change high polymer material with reaction activity as a main substrate component, and mixing micron-sized aerogel particles with a solution containing the phase-change high polymer material with reaction activity to obtain a phase-change high polymer material / aerogel particle dispersion liquid with reaction activity; enabling the phase-change high polymer material / aerogel particle dispersion liquid with reaction activity to be subjected to cross-linking reaction to prepare the water-resistant and high-temperature-resistant flexible phase-change material. The water-resistant and high-temperature-resistant flexible phase change material provided by the invention is a flexible self-supporting film, has the melting enthalpy of 113-147J / g, the density of 0.01-0.10 g / cm < 3 > and the phase transition temperature of 60-66 DEG C, realizes the special properties of slow heating and quick cooling, and is expected to be used in the fields of light heat insulation, heat preservation, energy conservation and emission reduction, human body heat management and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a flexible phase change material, in particular to a water-resistant and high-temperature-resistant flexible phase change material and a preparation method and application thereof, belonging to the technical field of nanomaterials and solid-solid phase change materials. Background Art

[0002] In daily life, thermal management is essential for human health. Prolonged exposure to high temperature may cause thermal discomfort to the human body and even cause serious skin damage. Therefore, designing a thermal protection material that heats up slowly and cools down quickly is crucial for human thermal management. Phase change materials, as an advanced thermal energy storage and management material, have a high thermal energy storage density and a relatively constant phase change temperature range. They can absorb or release a large amount of heat when the temperature changes without changing their own temperature. They have attracted much attention due to their strong heat storage capacity, adjustable phase change temperature and wide applicability. However, the original phase change materials generally have problems such as liquid phase leakage, which limits their practical application.

[0003] Infiltrating PCM into a supporting material to prepare a shape-stable composite PCM is a general solution. CN117700828A mentions that MXene-based aerogel is vacuum impregnated into a phase change material solution and dried to obtain a single-layer MXene-based aerogel composite phase change film; the steps are repeated to obtain a double-layer MXene-based aerogel composite phase change film; CN117964939A mentions the introduction of long-chain ether bonds in cellulose aerogels, and the use of their affinity with polyethylene glycol phase change materials to increase the coverage of cellulose aerogels on polyethylene glycol phase change materials, thereby obtaining an aerogel composite phase change insulation material; CN118027906A composites a molten mixture of aerogel and phase change materials by vacuum-assisted adsorption to obtain a photoresponsive aerogel phase change composite material. It is worth noting that balancing shape stability and energy storage density in shape-stable composite PCMs is still challenging because the introduced supporting material is an inactive material without energy storage capacity. In addition, its complex preparation method and cycle life also need to be further improved. Summary of the invention

[0004] The main purpose of the present invention is to provide a water-resistant and high-temperature-resistant flexible phase change material and a preparation method thereof, so as to overcome the deficiencies in the prior art.

[0005] Another object of the present invention is to provide an application of the water-resistant and high-temperature-resistant flexible phase change material.

[0006] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:

[0007] The embodiment of the present invention provides a method for preparing a water-resistant and high-temperature-resistant flexible phase change material, which comprises:

[0008] Providing a reactive phase change polymer material as a main substrate component;

[0009] Mixing micron-sized aerogel particles with a solution containing the reactive phase-change polymer material to obtain a reactive phase-change polymer material / aerogel particle dispersion;

[0010] The reactive phase-change polymer material / aerogel particle dispersion liquid is subjected to a cross-linking reaction to obtain a water-resistant and high-temperature-resistant flexible phase-change material.

[0011] In some embodiments, the preparation method comprises: performing an activation treatment on the phase change polymer material in a selected solvent system, wherein the activation treatment comprises any one of an esterification reaction, an etherification reaction, and an amination reaction.

[0012] The embodiment of the present invention also provides a water-resistant and high-temperature-resistant flexible phase change material prepared by the above method.

[0013] The embodiments of the present invention also provide the use of the aforementioned water-resistant and high-temperature-resistant flexible phase change material in the preparation of thermal insulation materials, hydrophobic, moisture-permeable and breathable materials, filtration membrane materials or flexible functional composite material substrates.

[0014] Compared with the prior art, the advantages of the present invention are at least:

[0015] 1) The water-resistant and high-temperature-resistant flexible phase-change material provided by the present invention has excellent mechanical properties, flexibility, hydrophobic properties, and excellent moisture permeability and air permeability; at the same time, the flexible phase-change material can be cut, folded, curled, and twisted;

[0016] 2) The water-resistant and high-temperature-resistant flexible phase change material provided by the present invention has a high thermal enthalpy, that is, it provides a considerable heat storage capacity in a relatively small volume, which can reduce the damage to human skin caused by drastic changes in external temperature;

[0017] 3) The preparation method of the water-resistant and high-temperature-resistant flexible phase change material provided by the present invention is simple, the raw material source is wide, the price is low, and it is easy to carry out continuous and large-scale production; it can be used to prepare thermal insulation materials, hydrophobic moisture-permeable and breathable materials, filter membrane materials or flexible functional composite material substrates, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0019] Figure 1 This is a scanning electron microscope image of the water-resistant and high-temperature-resistant flexible phase change material obtained in Example 1 of the present invention;

[0020] Figure 2 This is an optical photograph of the appearance of the water-resistant and high-temperature-resistant flexible phase change material obtained in Example 1 of the present invention;

[0021] Figure 3 This is a stress-strain curve diagram of the water-resistant and high-temperature-resistant flexible phase change material obtained in Example 1 of the present invention under a tensile mode;

[0022] Figure 4 This is a photograph of the hydrophobic angle of the water-resistant and high-temperature-resistant flexible phase change material obtained in Example 1 of the present invention;

[0023] Figure 5 This is a differential scanning calorimetry diagram of the water-resistant and high-temperature-resistant flexible phase change material obtained in Example 1 of the present invention;

[0024] Figure 6 This is a diagram showing the thermal management effect of the water-resistant and high-temperature-resistant flexible phase change material obtained in Example 1 of the present invention under a high-temperature environment;

[0025] Figure 7 This is a stress-strain curve diagram of the water-resistant and high-temperature-resistant flexible phase change material obtained in Example 2 of the present invention under a tensile mode;

[0026] Figure 8 This is a photograph of the hydrophobic angle of the water-resistant and high-temperature-resistant flexible phase change material obtained in Example 2 of the present invention;

[0027] Fig. 9 This is a differential scanning calorimetry diagram of the water-resistant and high-temperature-resistant flexible phase change material obtained in Example 2 of the present invention;

[0028] Fig.10 This is a diagram showing the thermal management effect of the water-resistant and high-temperature-resistant flexible phase change material obtained in Example 2 of the present invention under a high-temperature environment;

[0029] Fig.11 This is a stress-strain curve diagram of the water-resistant and high-temperature-resistant flexible phase change material obtained in Example 3 of the present invention under a tensile mode;

[0030] Fig.12 This is a photograph of the hydrophobic angle of the water-resistant and high-temperature-resistant flexible phase change material obtained in Example 3 of the present invention;

[0031] Fig.13 This is a differential scanning calorimetry diagram of the water-resistant and high-temperature-resistant flexible phase change material obtained in Example 3 of the present invention;

[0032] Fig.14This is a diagram showing the thermal management effect of the water-resistant and high-temperature-resistant flexible phase change material obtained in Example 3 of the present invention in a high-temperature environment of 80°C;

[0033] Fig.15 This is a picture of the pure PEG phase change material obtained in Control Example 1 dissolved in water in a hot environment at 80°C;

[0034] Fig.16 This is a picture of the leakage problem of the pure PEG phase change material obtained in Control Example 2 in a hot environment of 80°C. DETAILED DESCRIPTION

[0035] Cross-linked polyethylene glycol diacrylate gel has the advantages of high thermal stability, high thermal enthalpy, and high mechanical strength. Micron-sized aerogel particles, due to their large porosity and high specific surface area, can be used as functional materials to further improve the shape stability of phase change materials. In addition, aerogel particles can reduce the thermal conductivity of phase change materials, and effectively slow down the rise in surface temperature of composite phase change materials through the synergistic effect of thermal insulation of aerogel particles and latent heat absorption of phase change materials. Therefore, designing an effective strategy to prepare polyethylene glycol diacrylate / aerogel particle composites can not only broaden the structural and functional options of phase change materials, but also help promote the high-value utilization of phase change materials. At present, research on polyethylene glycol diacrylate / aerogel particles is relatively limited, and no precedents have been reported for successful preparation and application in the field of thermal insulation.

[0036] In view of the defects of the prior art, the inventors of this case have proposed the technical solution of the present invention after long-term research and extensive practice. The main steps are to first prepare a reactive phase change polymer material as the main base component; secondly, add micron-sized aerogel particles to the reactive phase change polymer material to give the phase change material excellent flexibility and thermal hysteresis; finally, a cross-linking reaction is carried out to obtain a water-resistant and high-temperature resistant flexible phase change material.

[0037] The technical solution, its implementation process and principle are further explained as follows. However, it should be understood that within the scope of the present invention, the above-mentioned technical features of the present invention and the technical features specifically described in the following (embodiments) can be combined with each other to form a new or preferred technical solution. Due to space limitations, they will not be described one by one here.

[0038] As one aspect of the technical solution of the present invention, a method for preparing a water-resistant and high-temperature-resistant flexible phase change material includes:

[0039] Providing a reactive phase change polymer material as a main substrate component;

[0040] Mixing micron-sized aerogel particles with a solution containing the reactive phase-change polymer material to obtain a reactive phase-change polymer material / aerogel particle dispersion;

[0041] The reactive phase-change polymer material / aerogel particle dispersion liquid is subjected to a cross-linking reaction to obtain a water-resistant and high-temperature-resistant flexible phase-change material.

[0042] The main preparation method of the present invention is: firstly, a reactive phase-change polymer material is prepared as the main base component; secondly, micron-sized aerogel particles are added to the reactive phase-change polymer material to give the phase-change material excellent flexibility and thermal hysteresis; finally, a cross-linking reaction is performed to obtain a flexible phase-change material that is resistant to water and high temperature. This method is different from the traditional porous aerogel as the base phase-change material as the filler. Instead, the aerogel is used as a functional group, and its large specific surface area, high hydrophobicity and excellent thermal management performance are utilized to achieve the flexibility, water resistance and temperature resistance of the phase-change material, thereby obtaining a flexible phase-change material that is resistant to water and high temperature, that is, a flexible self-supporting film.

[0043] In some specific embodiments, the preparation method includes: in a selected solvent system, activating the phase change polymer material at room temperature for 24 to 48 hours, wherein the activation treatment includes any one of esterification reaction, etherification reaction, and amination reaction, but is not limited thereto.

[0044] In some specific embodiments, the reactive phase-change polymer material has two or more functional groups at each end, such as acrylate functional groups, etc., so that it has a basis for cross-linking reaction.

[0045] In some specific embodiments, the phase change polymer material may include any one or a combination of two or more of polyethylene glycol, polypropylene glycol, polyurethane, polyvinyl acetate, etc., preferably polyethylene glycol (number average molecular weight of 10,000), but is not limited thereto.

[0046] In some specific embodiments, the number average molecular weight of the phase change polymer material is 400 to 100,000, preferably 6,000 to 10,000.

[0047] Furthermore, the phase change enthalpy of the phase change polymer material is 100 to 200 J g -1 .

[0048] In some embodiments, the preparation method comprises: performing activation treatments such as terminal hydroxyl vinylation, polyhydroxylation, polyaminoation, etc. on the polymer phase change material in a selected solvent system.

[0049] In some specific embodiments, the selected solvent system includes at least any one of organic substances such as dichloromethane, acetone, and dimethylacetamide, but is not limited thereto.

[0050] In some more preferred embodiments, the activation treatment includes vinylation of the terminal hydroxyl groups of polyethylene glycol; specifically, the vinylation of the terminal hydroxyl groups of polyethylene glycol includes: allowing polyethylene glycol to undergo an esterification reaction with acryloyl chloride in a selected solvent system to generate polyethylene glycol diacrylate.

[0051] Furthermore, the preparation method of the reactive phase change polymer material polyethylene glycol diacrylate specifically comprises:

[0052] 1) Take polyethylene glycol (PEG) with a molecular weight of 6000-10000 Daltons and prepare a polyethylene glycol solution with an organic solvent, wherein PEG: organic solvent = 1:3-1:10 (mass volume ratio, g / m1);

[0053] 2) Under argon protection, adding an appropriate amount of catalyst to the polyethylene glycol solution, the reaction time is 18h to 48h, preferably 48h, wherein the catalyst is triethylamine;

[0054] 3) Under argon protection, adding an acrylic acid compound and reacting for a certain time, wherein the ratio of PEG to acrylic acid compound is 1:2 to 1:4, preferably 1:4;

[0055] 4) Terminating the reaction and purifying to obtain polyethylene glycol diacrylate (PEGDA) with different molecular weights.

[0056] In some specific embodiments, the micron-sized aerogel particles have a high specific surface area, provide a strong capillary effect, and may include any one or a combination of two or more of superhydrophobic silica aerogel particles, hydrophilic silica aerogel particles, polymer-based aerogel particles, cellulose aerogel particles, etc., but are not limited thereto.

[0057] Furthermore, the micron-sized aerogel particles have a three-dimensional porous structure, a pore size of 1 to 1000 μm, and a porosity of 80 to 98.45%.

[0058] Furthermore, the micron-sized aerogel particles are preferably silicon oxide aerogel particles having excellent thermal insulation and thermal hysteresis.

[0059] In some specific embodiments, the mass fraction of micron-sized aerogel particles in the reactive phase-change polymer material / aerogel particle dispersion is 1 to 5 wt %, preferably 1 to 3 wt %.

[0060] In some specific embodiments, the mass fraction of the reactive phase-change polymer material in the reactive phase-change polymer material / aerogel particle dispersion is 50 to 90 wt %, preferably 60 to 70 wt %.

[0061] In some specific embodiments, the preparation method includes: adding the micron-sized aerogel particles to the solution containing the reactive phase-change polymer material by at least one of high-speed mechanical stirring and ultrasonic dispersion. That is, from another perspective, the method of adding the micron-sized aerogel particles to the solution containing the reactive phase-change polymer material includes any one of mechanical stirring, ultrasonic dispersion, etc., and finally obtaining a reactive phase-change polymer material / aerogel particle dispersion, which gives the phase-change material excellent flexibility and thermal hysteresis.

[0062] In some specific embodiments, the cross-linking reaction includes covalent cross-linking, physical cross-linking, and a mixed cross-linking of the two.

[0063] Furthermore, the cross-linking reaction includes: using a photoinitiator, adopting a photochemical reaction to trigger the cross-linking reaction, and using ultraviolet light to initiate a free radical polymerization reaction.

[0064] In some preferred embodiments, the phase change polymer material / aerogel particle composite gel is fully swollen and dried to obtain a water-resistant and high-temperature-resistant flexible phase change material.

[0065] Furthermore, the cross-linking reaction includes: under ultraviolet light conditions, causing the reactive phase change polymer material / aerogel particle dispersion to undergo a cross-linking reaction to obtain a phase change polymer material / aerogel particle composite gel, and then fully swelling and drying the composite gel to obtain a water-resistant and high-temperature resistant flexible phase change material.

[0066] In some more preferred specific embodiments, the cross-linking method of the polyethylene glycol diacrylate comprises: placing the polyethylene glycol diacrylate / aerogel particle dispersion in quartz glass, and cross-linking under ultraviolet light to form a polyethylene glycol diacrylate / aerogel particle composite gel.

[0067] Furthermore, the mass fraction of polyethylene glycol diacrylate in the polyethylene glycol diacrylate / aerogel particle dispersion is 50 to 90 wt %, preferably 60 to 70 wt %.

[0068] Further, the photoinitiator includes Irgacure 2959, but is not limited thereto.

[0069] Furthermore, the wavelength of the ultraviolet light is 300-400 nm, and the light intensity is 4-5 mW / cm2 .

[0070] Furthermore, the cross-linking reaction time is 8 min to 30 min, preferably 10 min.

[0071] In some specific embodiments, the preparation method includes: placing the phase change polymer material / aerogel particle composite gel in water (such as deionized water) for full swelling.

[0072] Furthermore, the swelling temperature is room temperature, and the swelling time is 12 to 48 hours, preferably 24 hours.

[0073] Furthermore, the frequency of replacement in water (such as deionized water) is 4 to 6 hours per time, and the number of times is 2 to 8 times.

[0074] In some specific embodiments, the drying treatment includes any one of room temperature drying, freeze drying and supercritical drying, or a combination of two or more thereof, preferably freeze drying.

[0075] Furthermore, the drying process takes 24 to 72 hours.

[0076] Among them, in some more specific embodiments, the preparation method of the water-resistant and high-temperature-resistant flexible phase change material comprises the following steps:

[0077] A reactive phase-change polymer material is prepared as the main base component;

[0078] Adding micron-sized aerogel particles to a solution containing the reactive phase-change polymer material to obtain a reactive phase-change polymer material / aerogel particle dispersion, which imparts excellent flexibility and thermal hysteresis to the phase-change material;

[0079] The reactive phase-change polymer material / aerogel particle dispersion is subjected to a cross-linking reaction to prepare a composite gel, which is then fully swollen and dried to obtain a water-resistant and high-temperature-resistant flexible phase-change material.

[0080] In summary, the preparation method of the water-resistant and high-temperature-resistant flexible phase change material provided by the present invention is simple, the raw material sources are wide, the price is low, and it is easy to carry out continuous and large-scale production.

[0081] As another aspect of the technical solution of the present invention, it also relates to a water-resistant and high-temperature-resistant flexible phase change material prepared by the aforementioned preparation method, which includes: a flexible matrix material, and micron-sized aerogel particles uniformly distributed in the flexible matrix material.

[0082] In some embodiments, the water-resistant and high-temperature-resistant flexible phase-change material is a flexible phase-change film with a self-supporting structure.

[0083] Furthermore, the micron-sized aerogel particles are highly hydrophobic aerogel particles. Preferably, when the micron-sized aerogel particles are silica aerogel particles, the silica aerogel particles form a gradient distribution state in the flexible matrix material with the upper surface being enriched and the lower surface being sparse.

[0084] In some embodiments, the water-resistant and high-temperature-resistant flexible phase change material has multiple functions such as light weight, solid-solid phase transition, porosity, and adjustable latent heat, and achieves special properties of slow heating and fast cooling.

[0085] In some implementation cases, the density of the water-resistant and high-temperature-resistant flexible phase change material is 0.01 to 0.10 g / cm 3 , preferably 0.072 to 0.10 g / cm 3 , hydrophobic angle is 97-131°, thermal conductivity is 0.0340-0.0629 W / m·K, and melting enthalpy is 113-147 J g -1 The phase transition temperature is 60-66°C, achieving the special properties of slow heating and fast cooling, and is expected to be used in lightweight insulation, thermal insulation, energy conservation and emission reduction, and human thermal management.

[0086] In summary, the water-resistant and high-temperature-resistant flexible phase change material provided by the present invention has excellent mechanical, flexibility, hydrophobic properties and excellent moisture permeability and air permeability; at the same time, the flexible phase change material can be cut, folded, curled, and twisted.

[0087] The water-resistant and high-temperature-resistant flexible phase-change material provided by the present invention has a high thermal enthalpy, that is, it provides a considerable heat storage capacity in a relatively small volume, and can reduce the damage to human skin caused by drastic changes in external temperature.

[0088] Another aspect of an embodiment of the present invention further provides an application of the aforementioned water-resistant and high-temperature resistant flexible phase change material. Specifically, the water-resistant and high-temperature resistant flexible phase change material can be used in the preparation of thermal insulation materials, hydrophobic, moisture-permeable and breathable materials, filtration membrane materials or flexible functional composite material substrates.

[0089] The technical scheme of the present invention is further described in detail below in conjunction with several preferred embodiments and the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. It should be pointed out that the embodiments described below are intended to facilitate the understanding of the present invention, and do not have any limiting effect on it. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present invention. The experimental methods for which specific conditions are not specified in the following embodiments are usually carried out under conventional conditions or under the conditions recommended by the manufacturer.

[0090] Example 1

[0091] Step 1: Take 10g of polyethylene glycol (PEG10000) and dissolve it in 50ml of dichloromethane at room temperature, and stir it evenly at room temperature. Under argon protection, add appropriate amounts of triethylamine and acryloyl chloride, and continue stirring to react for 48 hours, wherein the molar ratio of polyethylene glycol, triethylamine, and acryloyl chloride is 1:2:4. After the reaction is completed, add 8 molar equivalents of 2M potassium bicarbonate and stir for 60 minutes to remove HCl in the reaction solution. Transfer the above reaction solution to a separatory funnel, let it stand for 4 hours after sufficient shaking, take the bottom reaction solution, add 2 to 10 times the volume of anhydrous ether until a white powder sample is precipitated, filter and collect the sample and place it in a 25°C vacuum drying oven to dry for 24 hours to obtain polyethylene glycol diacrylate (PEGDA10000).

[0092] Step 2: Dissolve PEGDA10000 in 0.6g / L 12959 aqueous solution to prepare a PEGDA solution with a mass fraction of 70wt%. Add superhydrophobic silica aerogel particles and stir at high speed at room temperature until the silica aerogel is evenly dispersed to prepare a precursor solution. The mass ratio of silica aerogel to polymer phase change material is 3:70.

[0093] Step 3: Transfer the precursor solution to a quartz mold and then irradiate with ultraviolet light (365nm, 4-5mW / m 2 ) for 10 minutes to achieve chemical crosslinking of the obtained composite hydrogel. The gel obtained after photopolymerization was immersed in deionized water for 24 hours until the residual monomers in the gel were completely removed, and freeze-dried for 48 hours to obtain a water-resistant and high-temperature-resistant flexible phase change material.

[0094] Figure 1 This is an optical photograph of the appearance of the water-resistant and high-temperature-resistant flexible phase-change material obtained in this embodiment. Figure 2 This is a scanning electron microscope image of the water-resistant and high-temperature-resistant flexible phase change material obtained in this case. Figure 3 The stress-strain curve of the water-resistant and high-temperature-resistant flexible phase change material obtained in this embodiment under the tensile mode. Figure 4 This is a photograph of the hydrophobic angle of the water-resistant and high-temperature-resistant flexible phase change material obtained in this example. Figure 5 This is a differential scanning calorimetry diagram of the water-resistant and high-temperature-resistant flexible phase change material obtained in this example. Figure 6 This is an infrared image of the thermal insulation effect of the water-resistant and high-temperature-resistant flexible phase change material obtained in this embodiment under a high-temperature environment.

[0095] Example 2

[0096] Step 1: Take 10g of polyethylene glycol (PEG10000) and dissolve it in 50ml of dichloromethane at room temperature, and stir it evenly at room temperature. Under argon protection, add appropriate amounts of triethylamine and acryloyl chloride, and continue stirring to react for 48 hours, wherein the molar ratio of polyethylene glycol, triethylamine, and acryloyl chloride is 1:2:4. After the reaction is completed, add 8 molar equivalents of 2M potassium bicarbonate and stir for 60 minutes to remove HCl in the reaction solution. Transfer the above reaction solution to a separatory funnel, let it stand for 4 hours after sufficient shaking, take the bottom reaction solution, add 2 to 10 times the volume of anhydrous ether until a white powder sample is precipitated, filter and collect the sample and place it in a 25°C vacuum drying oven to dry for 24 hours to obtain polyethylene glycol diacrylate (PEGDA10000).

[0097] Step 2: Dissolve PEGDA10000 in 0.6g / L 12959 aqueous solution to prepare a PEGDA solution with a mass fraction of 70wt%. Add superhydrophobic silica aerogel particles and stir at high speed at room temperature until the silica aerogel is evenly dispersed to prepare a precursor solution, and the mass ratio of silica aerogel to polymer phase change material is 1:50.

[0098] Step 3: Transfer the precursor solution to a quartz mold and then irradiate with ultraviolet light (365nm, 4-5mW / m 2 ) for 10 minutes to achieve chemical crosslinking of the obtained composite hydrogel. The gel obtained after photopolymerization was immersed in deionized water for 24 hours until the residual monomers in the gel were completely removed, and freeze-dried for 48 hours to obtain a water-resistant and high-temperature-resistant flexible phase change material.

[0099] The water-resistant and high-temperature-resistant flexible phase-change material prepared in this embodiment is a white film with a thickness of about 0.4 mm, which can be folded and bent to any position without breaking and has good flexibility.

[0100] Figure 7 The stress-strain curve of the water-resistant and high-temperature-resistant flexible phase change material obtained in an embodiment of the present invention under a tensile mode. Figure 8 This is a photograph of the hydrophobic angle of the water-resistant and high-temperature-resistant flexible phase change material obtained in an embodiment of the present invention. Fig. 9 This is a differential scanning calorimetry diagram of the water-resistant and high-temperature-resistant flexible phase change material obtained in an embodiment of the present invention. Fig.10 This is an infrared image of the thermal insulation effect of the water-resistant and high-temperature-resistant flexible phase change material obtained in an embodiment of the present invention under a high-temperature environment.

[0101] Example 3

[0102] Step 1: Take 10g of polyethylene glycol (PEG10000) and dissolve it in 50ml of dichloromethane at room temperature, and stir it evenly at room temperature. Under argon protection, add appropriate amounts of triethylamine and acryloyl chloride, and continue stirring to react for 48 hours, wherein the molar ratio of polyethylene glycol, triethylamine, and acryloyl chloride is 1:2:4. After the reaction is completed, add 8 molar equivalents of 2M potassium bicarbonate and stir for 60 minutes to remove HCl in the reaction solution. Transfer the above reaction solution to a separatory funnel, let it stand for 4 hours after sufficient shaking, take the bottom reaction solution, add 2 to 10 times the volume of anhydrous ether until a white powder sample is precipitated, filter and collect the sample and place it in a 25°C vacuum drying oven to dry for 24 hours to obtain polyethylene glycol diacrylate (PEGDA10000).

[0103] Step 2: Dissolve PEGDA10000 in 0.6g / L 12959 aqueous solution to prepare a PEGDA solution with a mass fraction of 70wt%. Add superhydrophobic silica aerogel particles and stir at high speed at room temperature until the silica aerogel is evenly dispersed to prepare a precursor solution. The mass ratio of silica aerogel to polymer phase change material is 5:90.

[0104] Step 3: Transfer the precursor solution to a quartz mold and then irradiate with ultraviolet light (365nm, 4-5mW / m 2 ) for 10 minutes to achieve chemical crosslinking of the obtained composite hydrogel. The gel obtained after photopolymerization was immersed in deionized water for 24 hours until the residual monomers in the gel were completely removed, and freeze-dried for 48 hours to obtain a water-resistant and high-temperature-resistant flexible phase change material.

[0105] Fig.11 The stress-strain curve of the water-resistant and high-temperature-resistant flexible phase change material obtained in an embodiment of the present invention under a tensile mode. Fig.12 This is a photograph of the hydrophobic angle of the water-resistant and high-temperature-resistant flexible phase change material obtained in an embodiment of the present invention. Fig.13 This is a differential scanning calorimetry diagram of the water-resistant and high-temperature-resistant flexible phase change material obtained in an embodiment of the present invention. Fig.14 This is an infrared image of the thermal insulation effect of the water-resistant and high-temperature-resistant flexible phase change material obtained in an embodiment of the present invention under a high-temperature environment.

[0106] Example 4

[0107] Step 1: Take 10g of polyethylene glycol (PEG10000) and dissolve it in 50ml of dichloromethane at room temperature, and stir it evenly at room temperature. Under argon protection, add appropriate amounts of triethylamine and acryloyl chloride, and continue stirring to react for 48 hours, wherein the molar ratio of polyethylene glycol, triethylamine, and acryloyl chloride is 1:2:4. After the reaction is completed, add 8 molar equivalents of 2M potassium bicarbonate and stir for 60 minutes to remove HCl in the reaction solution. Transfer the above reaction solution to a separatory funnel, let it stand for 4 hours after sufficient shaking, take the bottom reaction solution, add 2 to 10 times the volume of anhydrous ether until a white powder sample is precipitated, filter and collect the sample and place it in a 25°C vacuum drying oven to dry for 24 hours to obtain polyethylene glycol diacrylate (PEGDA10000).

[0108] Step 2: Dissolve PEGDA10000 in 0.6g / L 12959 aqueous solution to prepare a PEGDA solution with a mass fraction of 70wt%. Add hydrophilic silica aerogel particles and stir at high speed at room temperature until the hydrophilic silica aerogel is evenly dispersed to prepare a precursor solution. The mass ratio of hydrophilic silica aerogel to polymer phase change material is 3:70.

[0109] Step 3: Transfer the precursor solution to a quartz mold and then irradiate with ultraviolet light (365nm, 4-5mW / m 2 ) for 10 minutes to achieve chemical crosslinking of the obtained composite hydrogel. The gel obtained after photopolymerization was immersed in deionized water for 24 hours until the residual monomers in the gel were completely removed, and freeze-dried for 48 hours to obtain a water-resistant and high-temperature-resistant flexible phase change material.

[0110] Example 5

[0111] Step 1: Take 10g of polyethylene glycol (PEG10000) and dissolve it in 50ml of dichloromethane at room temperature, and stir it evenly at room temperature. Under argon protection, add appropriate amounts of triethylamine and acryloyl chloride, and continue stirring to react for 48 hours, wherein the molar ratio of polyethylene glycol, triethylamine, and acryloyl chloride is 1:2:4. After the reaction is completed, add 8 molar equivalents of 2M potassium bicarbonate and stir for 60 minutes to remove HCl in the reaction solution. Transfer the above reaction solution to a separatory funnel, let it stand for 4 hours after sufficient shaking, take the bottom reaction solution, add 2 to 10 times the volume of anhydrous ether until a white powder sample is precipitated, filter and collect the sample and place it in a 25°C vacuum drying oven to dry for 24 hours to obtain polyethylene glycol diacrylate (PEGDA10000).

[0112] Step 2: Dissolve PEGDA10000 in 0.6g / L 12959 aqueous solution to prepare a PEGDA solution with a mass fraction of 70wt%. Add cellulose aerogel particles and stir at high speed at room temperature until the cellulose aerogel is evenly dispersed to prepare a precursor solution. The mass ratio of cellulose aerogel to polymer phase change material is 3:70.

[0113] Step 3: Transfer the precursor solution to a quartz mold and then irradiate with ultraviolet light (365 nm, 4 mW / m 2 ) for 30 minutes to achieve chemical crosslinking of the obtained composite hydrogel. The gel obtained after photopolymerization was immersed in deionized water for 12 hours until the residual monomers in the gel were completely removed, and freeze-dried for 72 hours to obtain a water-resistant and high-temperature-resistant flexible phase change material.

[0114] Example 6

[0115] Step 1: Take 10g of polypropylene glycol (PPG2000) and dissolve it in 50ml of dichloromethane at room temperature, and stir it evenly at room temperature. Under argon protection, add appropriate amounts of triethylamine and acryloyl chloride, and continue stirring to react for 18h, wherein the molar ratio of polyethylene glycol, triethylamine, and acryloyl chloride is 1:2:2. After the reaction is completed, add 8 molar equivalents of 2M potassium bicarbonate and stir for 60min to remove HCl in the reaction solution. Transfer the above reaction solution to a separatory funnel, let it stand for 4h after sufficient shaking, take the bottom reaction solution, add 2 to 10 times the volume of anhydrous ether until a white powder sample is precipitated, filter and collect the sample and place it in a vacuum drying oven at 25℃ to dry for 24h to obtain polypropylene glycol acrylate (PGA2000).

[0116] Step 2: Dissolve PGA2000 in 0.6g / L I2959 aqueous solution to prepare a PGA solution with a mass fraction of 70wt%. Add superhydrophobic silica aerogel particles and stir at high speed at room temperature until the silica aerogel is evenly dispersed to prepare a precursor solution. The mass ratio of silica aerogel to polymer phase change material is 3:70.

[0117] Step 3: Transfer the precursor solution to a quartz mold and then irradiate with ultraviolet light (365 nm, 5 mW / m 2 ) for 8 minutes to achieve chemical crosslinking of the obtained composite hydrogel. The gel obtained after photopolymerization was immersed in deionized water for 48 hours until the residual monomers in the gel were completely removed, and freeze-dried for 24 hours to obtain a water-resistant and high-temperature-resistant flexible phase change material.

[0118] Example 7

[0119] Thermoplastic polyurethane masterbatch is added to nitrogen-nitrogen dimethylacetamide and stirred at 50°C to prepare a polyurethane dispersion with a mass fraction of 10wt%. Superhydrophobic silica aerogel particles are added to an ethanol solution and stirred and ultrasonically dispersed at 20°C to prepare an aerogel dispersion with a mass fraction of 2wt%. The mass ratio of the thermoplastic elastomer to the nanopore module is 5:95, that is, the mass ratio of the superhydrophobic silica aerogel to the polymer phase change material is 1:80. The polyurethane dispersion and the aerogel dispersion are then mixed evenly, ultrasonically defoamed, and then transferred to a 10wt% ethanol aqueous solution for solvent-induced phase separation to form a thin film, which is dried at normal pressure to obtain a water-resistant and high-temperature resistant flexible phase change material.

[0120] Example 8

[0121] Thermoplastic polyurethane masterbatch is added to dimethyl sulfoxide and stirred at 80°C to prepare a thermoplastic polyurethane dispersion with a mass fraction of 10wt%. Superhydrophobic silica aerogel powder is added to acetone solution and stirred and ultrasonically dispersed at 25°C to prepare an aerogel dispersion with a mass fraction of 1wt%. The mass ratio of the nanopore module to the thermoplastic elastomer is 5:95, that is, the mass ratio of the superhydrophobic silica aerogel to the polymer phase change material is 1:80. The polyurethane dispersion and the aerogel dispersion are then mixed evenly, ultrasonically defoamed, and then transferred to deionized water for solvent-induced phase separation to form a thin film, which is then supercritically dried to obtain a water-resistant and high-temperature resistant flexible phase change material.

[0122] Comparative Example 1

[0123] This control example is basically the same as Example 2, except that in step 1, the terminal hydroxyl group of polyethylene glycol is not vinylized.

[0124] Due to the liquid-liquid phase transition of PEG, the material liquefies when heated and is easily soluble in water. It is difficult to carry aerogel particles with superior thermal properties and it is difficult to meet actual needs. Fig.15 This is a picture of the pure PEG phase change material obtained in this comparative example dissolving in water in a hot environment at 80°C.

[0125] Comparative Example 2

[0126] This comparative example is basically the same as Example 2, except that no super-hydrophobic silica aerogel particles are added in step 2.

[0127] Finally, a hydrophilic flexible phase change material was obtained, but its temperature resistance was poor and leakage occurred at 80°C. Fig.16 This is a picture of the leakage problem of the pure PEG phase change material obtained in this control example in a hot environment of 80°C.

[0128] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.

[0129] It should be understood that the above are only some embodiments of the present invention. It should be pointed out that for ordinary technicians in this field, other modifications and improvements can be made without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A method for preparing a water-resistant and high-temperature-resistant flexible phase change material, characterized in that: include: Providing a reactive phase change polymer material as a main substrate component; Mixing micron-sized aerogel particles with a solution containing the reactive phase-change polymer material to obtain a reactive phase-change polymer material / aerogel particle dispersion; The reactive phase-change polymer material / aerogel particle dispersion liquid is subjected to a cross-linking reaction to obtain a water-resistant and high-temperature-resistant flexible phase-change material.

2. The preparation method according to claim 1, characterized in that: include: In a selected solvent system, the phase change polymer material is activated at room temperature for 24 to 48 hours. Preferably, the activation treatment includes any one of esterification, etherification, and amination. Preferably, each end of the reactive phase-change polymer material has more than two functional groups, and the functional groups include acrylate functional groups.

3. The preparation method according to claim 2, characterized in that: The phase change polymer material comprises any one of polyethylene glycol, polypropylene glycol, polyurethane, and polyvinyl acetate, or a combination of two or more thereof, preferably polyethylene glycol; and / or the number average molecular weight of the phase change polymer material is 400 to 100,000, preferably 6,000 to 10,000; And / or, the phase change enthalpy of the phase change polymer material is 100 to 200 J g -1 ; Preferably, the activation treatment comprises vinylation of the terminal hydroxyl groups of polyethylene glycol; particularly preferably, the vinylation of the terminal hydroxyl groups of polyethylene glycol comprises: allowing polyethylene glycol to undergo an esterification reaction with acryloyl chloride in a selected solvent system to generate polyethylene glycol diacrylate; And / or, the selected solvent system includes at least any one of dichloromethane, acetone, and dimethylacetamide.

4. The preparation method according to claim 1, characterized in that: The micron-sized aerogel particles include any one or a combination of two or more of super-hydrophobic silica aerogel particles, polymer-based aerogel particles, and cellulose aerogel particles; And / or, the micron-sized aerogel particles have a three-dimensional porous structure, a pore size of 1 to 1000 μm, and a porosity of 80 to 98.45%; And / or, the mass fraction of micron-sized aerogel particles in the reactive phase change polymer material / aerogel particle dispersion is 1 to 5 wt%, preferably 1 to 3 wt%; And / or, the mass fraction of the reactive phase change polymer material in the reactive phase change polymer material / aerogel particle dispersion is 50 to 90 wt %, preferably 60 to 70 wt %.

5. The preparation method according to claim 1, characterized in that: include: At least one of mechanical stirring and ultrasonic dispersion is used to add the micron-sized aerogel particles into a solution containing the reactive phase-change polymer material.

6. The preparation method according to claim 1, characterized in that: The cross-linking reaction includes covalent cross-linking and / or physical cross-linking; preferably, the cross-linking reaction includes: using a photoinitiator to trigger the cross-linking reaction by a photochemical reaction, and using ultraviolet light to initiate a free radical polymerization reaction; particularly preferably, the cross-linking reaction includes: under ultraviolet light conditions, causing the reactive phase change polymer material / aerogel particle dispersion to undergo a cross-linking reaction to obtain a phase change polymer material / aerogel particle composite gel, which is then fully swollen and dried to obtain a water-resistant and high-temperature resistant flexible phase change material.

7. The preparation method according to claim 6, characterized in that: The photoinitiator includes Irgacure 2959; and / or the wavelength of the ultraviolet light is 300-400 nm, and the light intensity is 4-5 mW / cm 2 ; and / or, the cross-linking reaction time is 8min to 30min.

8. The preparation method according to claim 6, characterized in that: include: The phase change polymer material / aerogel particle composite gel is placed in water for full swelling; and / or, the swelling temperature is room temperature, and the swelling time is 12 to 48 hours; preferably, the frequency of replacement in water is 4 to 6 hours / time, and the number of times is 2 to 8 times; And / or, the drying process comprises any one or a combination of two or more of room temperature drying, freeze drying and supercritical drying, preferably freeze drying; And / or, the drying process is performed for 24 to 72 hours.

9. A water-resistant and high-temperature-resistant flexible phase-change material prepared by the preparation method according to any one of claims 1 to 8, comprising: A flexible matrix material, and micron-sized aerogel particles uniformly distributed in the flexible matrix material; Preferably, the water-resistant and high-temperature-resistant flexible phase-change material is a flexible phase-change film with a self-supporting structure; Preferably, the micron-sized aerogel particles are highly hydrophobic aerogel particles, preferably silica aerogel particles, and the silica aerogel particles form a gradient distribution state in the flexible matrix material with the upper surface being enriched and the lower surface being sparse; Preferably, the density of the water-resistant and high-temperature-resistant flexible phase change material is 0.01 to 0.10 g / cm 3 , preferably 0.072 to 0.10 g / cm 3 , hydrophobic angle is 97°~131°, thermal conductivity is 0.0340~0.0629W / m·K, melting enthalpy is 113~147J g -1 , the phase transition temperature is 60~66℃.

10. Use of the water-resistant and high-temperature-resistant flexible phase-change material according to claim 9 in the preparation of thermal insulation materials, hydrophobic, moisture-permeable and breathable materials, filtration membrane materials or flexible functional composite material substrates.

Citation Information

Patent Citations

  • Double-layer MXene-based aerogel composite phase change film as well as preparation method and application thereof

    CN117700828A

  • Preparation method and application of aerogel composite phase change thermal insulation material

    CN117964939A

  • Photoresponse aerogel phase change composite material and preparation method thereof

    CN118027906A