Fluorescence enhanced composite material based on inorganic molecular lock as well as preparation method and application of fluorescence enhanced composite material
Through the crosslinking method of inorganic ion oligomers and organic fluorescent molecules, the problem of color change and non-universality when modifying organic fluorescent molecules in the prior art is solved, and a fluorescence-enhanced composite material with high quantum yield and stability is achieved , suitable for organic fluorescent molecules of different sizes.
Patent Information
- Application Number
- CN202411092457.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-22
AI Technical Summary
When modifying organic fluorescent molecules, the introduced unsaturated functional groups or rigid structures will change the luminous color of the original molecules, and the design framework limiting the molecular interaction force cannot maintain the original fluorescent color, which lacks universality.
Inorganic ion oligomers are used as molecular locks, and the fluorescence enhancement composite material with calcium carbonate ions crosslinked with carboxyl-containing organic fluorescent molecules to limit molecular vibration and rotation, improve fluorescence performance, and maintain the original emission wavelength of fluorescence enhancement composite material.
It achieves high quantum yield and stability, is suitable for organic fluorescent molecules of different sizes, is universal, and shows excellent fluorescence performance in both solution and solid state.
Smart Images

Figure CN118995197A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fluorescence enhancement, and in particular to a fluorescence enhancement composite material based on inorganic molecular locks, and a preparation method and application thereof. Background Art
[0002] In the field of organic fluorescence, there are two well-known effects, namely aggregation-induced quenching (ACQ) and aggregation-induced emission (AIE). The specific principle is that the intermolecular forces and the rotation and vibration within the molecule affect the path of the excited state returning to the ground state, which often brings many limitations on the practical application of organic fluorescent molecules. For example, the luminescence of molecules with ACQ effect in poor solvents or aggregated states will be very weak, and the emission of molecules with AIE effect in good solvents or dispersion stages will be very weak. This limits the practical application of fluorescent molecules.
[0003] In the existing technology, organic molecules can be modified through organic synthesis, and functional groups can be added to change the configuration of the molecules to eliminate the ACQ / AIE effect; it is also possible to confine small organic molecules in a rigid cage by designing a rigid framework, thereby inhibiting the movement within the molecules and the interaction between molecules.
[0004] Patent document CN110540650B discloses an aggregation-induced luminescent polyphosphate and a synthesis method thereof, wherein the aggregation-induced luminescent polyphosphate is obtained by ester exchange polycondensation reaction using phosphate and alcohol as raw materials. However, due to structural limitations, its luminescence mechanism is usually that the P heteroatoms contained therein form a spatial conjugated structure with each other after polymerization.
[0005] Patent document CN108912337B discloses a rare earth metal organic framework material with high quantum yield and its preparation method, which is constructed by using deprotonated 2,4,6-tris(4-carboxyphenyl)-1,3,5-triazine as ligand and rare earth metal ions as luminescent centers through π-π interactions between ligands or CH-π interactions between ligands and solvents. The invention controls the distance between the aromatic ring centers corresponding to the π-π interactions between ligands, enhances the interaction force between ligand molecules, increases the rigidity of the material skeleton, reduces the self-loss of energy on the skeleton, and enhances the energy transfer from ligands to rare earth metals, thereby improving the quantum yield.
[0006] However, the biggest problem with the current method of modifying organic molecules using organic synthesis is that the introduction of unsaturated functional groups such as double bonds or benzene rings and other rigid structures often leads to the expansion or change of the conjugated system, which will change the luminescent color of the original organic molecules, which is undesirable in practical applications. And by designing a framework of corresponding size, such as using organic metal frameworks or eutectics to limit the intramolecular or intermolecular interaction forces, it is often impossible to maintain the luminescent color of the original organic molecules. At the same time, because this framework needs to have good crystallinity and requires organic molecules of a specific size to perfectly fit in it to achieve the desired effect, it is not universal.
[0007] In summary, it is of great significance to develop a universal fluorescence-enhanced composite material that does not change the original emission wavelength of organic molecules and has a good effect. Summary of the invention
[0008] In order to solve the above problems in the prior art, the present invention provides a fluorescence-enhanced composite material based on inorganic molecular locks, which can have a very high quantum yield in both solution and solid state and exhibits excellent stability.
[0009] Inorganic ion oligomers have attracted scientists to study the construction of nanocomposite materials due to their molecular size. Inorganic ion oligomers can remain stable at the molecular level without being affected by classical nucleation and crystallization, and they have a rigid structure similar to unsaturated rigid groups. Therefore, the inventors designed to use inorganic ion oligomers as a molecular lock to modify the organic fluorescent molecules in situ to form a lock structure, thereby limiting the vibration and rotation of the molecules and improving their fluorescence properties.
[0010] A fluorescence enhancement composite material based on inorganic molecular locks comprises a calcium carbonate ion oligomer and a carboxyl-containing organic fluorescent molecule, wherein the calcium carbonate ion oligomer is cross-linked with the carboxyl groups in the carboxyl-containing organic fluorescent molecule via calcium ions.
[0011] The fluorescent enhancement material obtained based on the above design exhibits an ultra-high fluorescence quantum yield, and on this basis retains the emission wavelength of the original organic fluorescent molecules, and exhibits excellent stability under changes in solvent and temperature. At the same time, this inorganic molecular lock is suitable for organic fluorescent molecules of different sizes and has a certain universality.
[0012] Preferably, the molar ratio of calcium ions in the calcium carbonate ion oligomer to carboxyl groups in the carboxyl-containing organic fluorescent molecule is 2 to 5: 1. The present invention controls the molar ratio of calcium ions in the calcium carbonate ion oligomer to carboxyl groups in the carboxyl-containing organic fluorescent molecule within the above range, which can ensure that the organic fluorescent molecule fully reacts with the calcium carbonate oligomer and that the content of the organic fluorescent molecule is sufficient.
[0013] Preferably, the carboxyl-containing organic fluorescent molecule is a polycarboxyl organic fluorescent molecule, including any one of tetrakis-(carboxyphenyl)ethylene (H4TCPE), tetrakis[4-(4'-carboxyphenyl)phenyl]ethylene (H4ETTC), 4,4'4"-triphenylamine tricarboxylate (H3TPA) or perylene-3,4,9,10-tetracarboxylic acid (H4Perylene).
[0014] H4TCPE and H4ETTC are classic AIE organic fluorescent molecules that can greatly improve their fluorescence properties by restricting their intramolecular motion; H3TPA is an organic molecule with a propeller structure that can also improve its fluorescence properties by restricting its intramolecular motion; and H4Perylene is a classic planar ACQ molecule that can improve its fluorescence properties by restricting its intermolecular interaction forces.
[0015] The present invention also provides a method for preparing the fluorescence enhanced composite material, comprising the following steps:
[0016] The calcium carbonate ion oligomer and the organic fluorescent molecule containing a carboxyl group are added to an organic solvent for dispersion, and then an acid-base reaction is carried out to obtain the fluorescence enhanced composite material.
[0017] The present invention uses inorganic ion oligomers as inorganic ion locks, utilizes the characteristics and rigidity of non-shared electrons of ionic bonds, and obtains a composite fluorescent material locked by inorganic molecules through a simple acid-base reaction between calcium carbonate and organic molecules containing carboxyl groups. The technical difficulty of functionalizing organic matter with inorganic matter is solved through the reaction of inorganic ion oligomers and organic fluorescent molecules at the molecular level, promotes a more uniform and sufficient reaction of organic-inorganic composites, and obtains a fluorescence enhanced composite material with ultra-high fluorescence quantum yield and stability.
[0018] Preferably, the molar ratio of calcium ions in the calcium carbonate ion oligomer to carboxyl groups in the carboxyl-containing organic fluorescent molecules is 2 to 5:1.
[0019] Preferably, the organic solvent includes ethanol, tetrahydrofuran and the like.
[0020] Preferably, the acid-base reaction time is 3 to 48 hours.
[0021] Preferably, the carboxyl-containing organic fluorescent molecule is a polycarboxyl organic fluorescent molecule, including any one of tetrakis-(carboxyphenyl)ethylene (H4TCPE), tetrakis[4-(4'-carboxyphenyl)phenyl]ethylene (H4ETTC), 4,4'4"-triphenylamine tricarboxylate (H3TPA) or perylene-3,4,9,10-tetracarboxylic acid (H4Perylene).
[0022] Further preferably, according to the characteristics of the organic fluorescent molecules containing carboxyl groups, the present invention first dissolves them in a suitable good solvent, and then adds calcium carbonate ion oligomers, wherein H4TCPE, H3TPA and H4Perylene are preferably dissolved in ethanol, and H4ETTC is preferably dissolved in tetrahydrofuran.
[0023] Preferably, in order to allow the carboxyl-containing organic fluorescent molecule to fully react in the solution, when the carboxyl-containing organic fluorescent molecule is H4TCPE, H4ETTC and H3TPA, the acid-base reaction time is 6 to 12 hours; when the carboxyl-containing organic fluorescent molecule is H4Perylene, the acid-base reaction time is 24 to 48 hours.
[0024] Preferably, the preparation method of the calcium carbonate ion oligomer is: triethylamine as a capping agent, a calcium salt as a cation source, and carbon dioxide as an anion source are introduced into an organic solvent, and reacted at room temperature to obtain the calcium carbonate ion oligomer.
[0025] Preferably, the molar ratio of triethylamine to calcium ions in the calcium salt is 20 to 100:1. The organic solvent includes ethanol, propanol or butanol, preferably ethanol solvent. When preparing the calcium carbonate ion oligomer, a slightly excessive amount of anion source is added to completely bind the Ca in the solution.
[0026] The present invention can prepare low-concentration and high-concentration calcium carbonate ion oligomer solutions by controlling the amount of organic solvent added. A fluorescence-enhanced composite material in a solution state is prepared based on a calcium carbonate ion oligomer solution at a low concentration. A high-concentration fluorescence-enhanced composite material is prepared based on a calcium carbonate ion oligomer solution at a high concentration, and then the high-concentration fluorescence-enhanced composite material is centrifuged, washed, and vacuum-dried to prepare a fluorescence-enhanced composite material in a solid state. The fluorescence-enhanced composite material of the present invention can achieve fluorescence enhancement in both solid and liquid states.
[0027] The present invention also provides the application of the fluorescence enhanced composite material in the field of anti-counterfeiting. The fluorescence composite material of the present invention has very high quantum yield and excellent stability, and has broad application prospects in the field of anti-counterfeiting.
[0028] Compared with the prior art, the present invention has at least the following beneficial effects:
[0029] (1) The present invention utilizes the characteristics and rigidity of inorganic ions locking non-shared electrons in their ionic bonds, and obtains a composite fluorescent material locked by inorganic molecules through a simple acid-base reaction between calcium carbonate ion oligomers and organic molecules containing carboxyl groups. The reaction of inorganic ion oligomers and organic fluorescent molecules at the molecular level solves the technical difficulties of functionalizing organic matter with inorganic substances, promotes a more uniform and sufficient reaction of organic-inorganic composites, and achieves a great enhancement of material performance. The prepared fluorescence-enhanced composite material has excellent stability, high fluorescence quantum yield (up to 99.9%), and can still maintain its single-molecule performance of luminescence.
[0030] (2) Due to the polymerization and cross-linking of calcium carbonate ion oligomers, the fluorescence enhanced composite material of the present invention can be made into a centimeter-level block, which expands its application scenarios. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 are photographs of solid-state fluorescent materials in the embodiments and comparative examples and their quantum yields, wherein Native represents the carboxyl-containing organic fluorescent molecules used in Examples 1-4; Nps represents the fluorescent composite materials prepared in Comparative Examples 1-4, and Locked represents the fluorescent composite materials prepared in Examples 1-4.
[0032] Figure 2 The fluorescence spectra of the solid-state fluorescent composite materials prepared in Examples 1-4.
[0033] Figure 3 The fluorescence spectra of the liquid fluorescent composite materials prepared in Examples 1-4.
[0034] Figure 4 These are fluorescence photographs of the carboxyl-containing organic fluorescent molecules and fluorescent composite materials in solution under ultraviolet light in Examples 1-4.
[0035] Figure 5 This is a block sample picture of the solid-state fluorescent composite material prepared in Example 1 and Example 2.
[0036] Figure 6 These are photos of the solid-state fluorescent composite material prepared in Example 1 processed at different temperatures.
[0037] Figure 7 This is a picture of the organic fluorescent molecules and fluorescent composite materials of Example 2 after being soaked in ethanol solvent and dried. DETAILED DESCRIPTION
[0038] The present invention will be further described below in conjunction with the examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention.
[0039] The preparation method of low-concentration calcium carbonate inorganic ion oligomers is as follows: 0.0117 g of calcium chloride dihydrate is dissolved in 100 mL of ethanol; 0.9 mL of triethylamine is added to the above solution; carbon dioxide is introduced at a flow rate of 100 mL / min for 2 minutes to obtain a low-concentration calcium carbonate ion oligomer solution.
[0040] The preparation method of a high-concentration calcium carbonate ion oligomer solution is as follows: 0.234 g of calcium chloride dihydrate is dissolved in 100 mL of ethanol; 90 mL of triethylamine is added to the above solution; carbon dioxide is introduced at a flow rate of 100 mL / min for 15 minutes to obtain a high-concentration calcium carbonate ion oligomer solution.
[0041] Example 1
[0042] 0.0051 g of H4TCPE organic molecules were weighed and dispersed in 20 mL of ethanol solution, and ultrasonically dispersed for 30 min to obtain a transparent solution, which showed very weak fluorescence under ultraviolet light. Subsequently, 100 mL of the above-mentioned low-concentration calcium carbonate ion oligomer solution was slowly added dropwise to the ethanol solution of organic molecules, and reacted at room temperature for 3 h to finally obtain a fluorescence enhanced composite material (H4TCPE-Locked) in a solution state.
[0043] Weigh 0.1g H4TCPE organic molecules and disperse them in 20mL ethanol solution, ultrasonically disperse for 30min to obtain a transparent solution, which shows very weak fluorescence under ultraviolet light. Subsequently, 100mL of the above-mentioned high-concentration calcium carbonate ion oligomer solution is slowly added dropwise to the ethanol solution of organic molecules, reacted at room temperature for 6h, and then the reacted solution is centrifuged and washed twice with ethanol, and the centrifugation parameters are: 20000rpm, 5min. Subsequently, the gel obtained by centrifugation is dried at room temperature in a vacuum dryer for 24h to obtain a block of composite fluorescent material, and the block is ground into powder with a mortar to finally obtain a fluorescence enhanced composite material (H4TCPE-Locked) in a solid state.
[0044] The structure of H4TCPE in this embodiment is as follows:
[0045]
[0046] Example 2
[0047] 0.0081g H4ETTC organic molecules were weighed and dispersed in 20mL tetrahydrofuran solution, and ultrasonically dispersed for 30min to obtain a transparent solution, which showed very weak fluorescence under ultraviolet light. Subsequently, 100mL of the above-mentioned low-concentration calcium carbonate ion oligomer solution was slowly added dropwise to the tetrahydrofuran solution of organic molecules, and reacted at room temperature for 3h to finally obtain a fluorescence enhanced composite material (H4ETTC-Locked) in a solution state.
[0048] Weigh 0.162g H4ETTC organic molecules and disperse them in 20mL tetrahydrofuran solution, ultrasonically disperse for 30min to obtain a transparent solution, which shows very weak fluorescence under ultraviolet light. Subsequently, 100mL of the above-mentioned high-concentration calcium carbonate ion oligomer solution is slowly added dropwise to the tetrahydrofuran solution of organic molecules, react at room temperature for 6h, and then the reacted solution is centrifuged and washed twice with ethanol, and the centrifugation parameters are: 20000rpm, 5min. Subsequently, the gel obtained by centrifugation is dried at room temperature in a vacuum dryer for 24h to obtain a block of composite fluorescent material, and the block is ground into powder with a mortar to finally obtain a fluorescence enhanced composite material (H4ETTC-Locked) in a solid state.
[0049] The structure of H4ETTC in this embodiment is as follows:
[0050]
[0051] Example 3
[0052] 0.0038g H3TPA organic molecules were weighed and dispersed in 20mL ethanol solution, and ultrasonically dispersed for 30min to obtain a transparent solution, which showed very weak fluorescence under ultraviolet light. Subsequently, 100mL of the above-mentioned low-concentration calcium carbonate ion oligomer solution was slowly added dropwise to the ethanol solution of organic molecules, and reacted at room temperature for 3h to finally obtain a fluorescence enhanced composite material (H3TPA-Locked) in a solution state.
[0053] Weigh 0.076g H3TPA organic molecules and disperse them in 20mL ethanol solution, ultrasonically disperse for 30min to obtain a transparent solution. Subsequently, 100mL of the above-mentioned high concentration of calcium carbonate ion oligomer solution was slowly added dropwise to the ethanol solution of organic molecules, reacted at room temperature for 6h, and then the reacted solution was centrifuged and washed twice with ethanol, and the centrifugation parameters were: 20000rpm, 5min. Subsequently, the gel obtained by centrifugation was dried at room temperature in a vacuum dryer for 24h to obtain a block of composite fluorescent material, and the block was ground into powder with a mortar to finally obtain a fluorescence enhanced composite material (H3TPA-Locked) in a solid state.
[0054] The structure of H3TPA in this embodiment is as follows:
[0055]
[0056] Example 4
[0057] 0.0043g H4Perylene organic molecules were weighed and dispersed in 20mL ethanol solution, and ultrasonic dispersion was performed for 30min to obtain a transparent solution. Subsequently, 100mL of the above-mentioned low-concentration calcium carbonate ion oligomer solution was slowly added dropwise to the ethanol solution of organic molecules, and the reaction was carried out at room temperature for 12h to finally obtain a fluorescence enhanced composite material (H4Perylene-Locked) in a solution state.
[0058] Weigh 0.086g H4Perylene organic molecules and disperse them in 20mL ethanol solution, ultrasonically disperse for 30min to obtain a transparent solution. Subsequently, 100mL of the above-mentioned high concentration of calcium carbonate ion oligomer solution is slowly added dropwise to the ethanol solution of organic molecules, react at room temperature for 36h, and then the reacted solution is centrifuged and washed twice with ethanol, and the centrifugal parameters are: 20000rpm, 5min. Subsequently, the gel obtained by centrifugation is dried at room temperature in a vacuum dryer for 24h to obtain a composite fluorescent material of the block, and the block is ground into powder with a mortar to finally obtain a fluorescence enhanced composite material (H4Perylene-Locked) in a solid state.
[0059] The structure of H4Perylene in this embodiment is as follows:
[0060]
[0061] Comparative Example 1
[0062] 0.38 g of calcium chloride dehydrate and 0.36 g of sodium carbonate were dissolved in water, respectively, and then cooled in a refrigerator at 4°C for 30 minutes. Then, the calcium chloride solution was slowly added to the sodium carbonate in ice water with stirring. When the solution was slightly turbid, the precipitate was quickly separated by vacuum filtration through a 0.45 μm membrane filter, then washed twice with fresh acetone, and finally dispersed in 100 mL of ethanol to form a calcium carbonate nanoparticle dispersion.
[0063] Weigh 0.1g H4TCPE organic molecules and disperse them in 20mL ethanol solution, ultrasonically disperse for 30min to obtain a transparent solution, which shows very weak fluorescence under ultraviolet light. Subsequently, the calcium carbonate nanoparticle dispersion obtained above is added dropwise to the ethanol solution of the organic molecules, reacted at room temperature for 6h, and then the reacted solution is centrifuged and washed twice with ethanol, and the centrifugal parameters are: 20000rpm, 5min. Subsequently, the gel obtained by centrifugation is dried at room temperature for 24h in a vacuum dryer to obtain a composite fluorescent material of a block, and the block is ground into powder with a mortar, and finally a calcium carbonate nanoparticle fluorescence enhanced composite contrast material in a solid state is obtained, which is recorded as H4TCPE-ACCNps.
[0064] Comparative Example 2
[0065] 0.178 g of calcium chloride dehydrate and 0.17 g of sodium carbonate were dissolved in water, respectively, and then cooled in a refrigerator at 4°C for 30 minutes. Then, the calcium chloride solution was slowly added to the sodium carbonate in ice water with stirring. When the solution was slightly turbid, the precipitate was quickly separated by vacuum filtration through a 0.45 μm membrane filter, then washed twice with fresh acetone, and finally dispersed in 100 mL of ethanol to form a calcium carbonate nanoparticle dispersion.
[0066] Weigh 0.162g H4ETTC organic molecules and disperse them in 20mL ethanol solution, ultrasonically disperse for 30min to obtain a transparent solution, which shows very weak fluorescence under ultraviolet light. Subsequently, the calcium carbonate nanoparticle dispersion obtained above is added dropwise to the ethanol solution of the organic molecules above, reacted at room temperature for 6h, and then the reacted solution is centrifuged and washed twice with ethanol, and the centrifugation parameters are: 20000rpm, 5min. Subsequently, the gel obtained by centrifugation is dried at room temperature for 24h in a vacuum dryer to obtain a block of composite fluorescent material, and the block is ground into powder with a mortar, and finally a solid state calcium carbonate nanoparticle fluorescence enhanced composite contrast material is obtained, which is recorded as H4ETTC-ACCNps.
[0067] Comparative Example 3
[0068] 0.178 g of calcium chloride dehydrate and 0.17 g of sodium carbonate were dissolved in water, respectively, and then cooled in a refrigerator at 4°C for 30 minutes. Then, the calcium chloride solution was slowly added to the sodium carbonate in ice water with stirring. When the solution was slightly turbid, the precipitate was quickly separated by vacuum filtration through a 0.45 μm membrane filter, then washed twice with fresh acetone, and finally dispersed in 100 mL of ethanol to form a calcium carbonate nanoparticle dispersion.
[0069] Weigh 0.076g H3TPA organic molecules and disperse them in 20mL ethanol solution, ultrasonically disperse for 30min to obtain a transparent solution, which shows very weak fluorescence under ultraviolet light. Subsequently, the calcium carbonate nanoparticle dispersion obtained above is added dropwise to the ethanol solution of the organic molecules, reacted at room temperature for 6h, and then the reacted solution is centrifuged and washed twice with ethanol, and the centrifugation parameters are: 20000rpm, 5min. Subsequently, the gel obtained by centrifugation is dried at room temperature for 24h in a vacuum dryer to obtain a block of composite fluorescent material, and the block is ground into powder with a mortar, and finally a solid state calcium carbonate nanoparticle fluorescence enhanced composite contrast material is obtained, which is recorded as H3TPA-ACCNps.
[0070] Comparative Example 4
[0071] 0.178 g of calcium chloride dehydrate and 0.17 g of sodium carbonate were dissolved in water, respectively, and then cooled in a refrigerator at 4°C for 30 minutes. Then, the calcium chloride solution was slowly added to the sodium carbonate in ice water with stirring. When the solution was slightly turbid, the precipitate was quickly separated by vacuum filtration through a 0.45 μm membrane filter, then washed twice with fresh acetone, and finally dispersed in 100 mL of ethanol to form a calcium carbonate nanoparticle dispersion.
[0072] Weigh 0.086g H4Perylene organic molecules and disperse them in 20mL ethanol solution, ultrasonically disperse for 30min to obtain a transparent solution, which shows very weak fluorescence under ultraviolet light. Subsequently, the calcium carbonate nanoparticle dispersion obtained above is added dropwise to the ethanol solution of the above organic molecules, reacted at room temperature for 36h, and then the reacted solution is centrifuged and washed twice with ethanol, and the centrifugal parameters are: 20000rpm, 5min. Subsequently, the gel obtained by centrifugation is dried at room temperature for 24h in a vacuum dryer to obtain a composite fluorescent material of a block, and the block is ground into powder with a mortar, and finally a calcium carbonate nanoparticle fluorescence enhanced composite contrast material in a solid state is obtained, which is recorded as H4Perylene-ACCNps.
[0073] Figure 1 The photographs of the solid fluorescent materials in the examples and comparative examples and their quantum yields, wherein Native represents the carboxyl-containing organic fluorescent molecular raw materials used in Examples 1-4; Nps represents the fluorescent composite materials prepared in Comparative Examples 1-4; and Locked represents the fluorescent composite materials prepared in Examples 1-4. Figure 1It can be seen that the fluorescence quantum yield of the fluorescent composite material prepared in the embodiment of the present invention is significantly higher than that of the pure carboxyl-containing organic fluorescent molecules and the fluorescent materials prepared in the comparative example. The fluorescence quantum yields of H4TCPE-Locked and H4ETTC-Locked in the solid state are as high as 83.8% and 99.9%, which are significantly improved compared with the quantum yields of pure organic matter H4TCPE (24.6%) and H4ETTC (42.0%) and the composite materials H4TCPE-ACCNps (30.1%) and H4ETTC-ACCNps (67.3%) enhanced by fluorescence with calcium carbonate nanoparticles.
[0074] Figure 2 It is a fluorescence spectrum diagram of solid organic fluorescent molecules and solid composite fluorescent materials obtained in Examples 1-4, wherein the gray part is the fluorescence spectrum diagram of organic fluorescent molecules containing carboxyl groups, and the colored part is the fluorescence spectrum diagram of composite fluorescent materials. Since the fluorescence of H4Perylene is so weak in the solid state that it can be ignored, its fluorescence spectrum is not displayed. It can be seen from the maximum emission peak that there is a significant difference between the fluorescence of solid organic molecules and the fluorescence of fluorescent composite materials, which shows that the effect of single-molecule fluorescence enhancement cannot be achieved simply by aggregating organic fluorescent molecules, and the locking effect of calcium carbonate oligomers can achieve fluorescence enhancement in the single-molecule state.
[0075] Figure 3 The fluorescence spectra of the organic fluorescent molecules in solution and the composite fluorescent materials in solution obtained in Examples 1-4 show that the fluorescence intensity is significantly enhanced after the addition of calcium carbonate oligomers.
[0076] Figure 4 These are fluorescence photographs of organic fluorescent molecules in solution and the composite fluorescent materials in solution obtained in Examples 1-4. It can be directly observed that after the addition of calcium carbonate oligomers, the fluorescence changes significantly from none to one.
[0077] Due to the advantage that calcium carbonate oligomers can be polymerized and cross-linked, the fluorescent composite material in the embodiment of the present invention can be prepared into a block of centimeter size. Figure 5 shown.
[0078] The photos of the solid-state fluorescent composite material (H4TCPE-Locked) prepared in Example 2 of the present invention treated at different temperatures are shown in FIG. Figure 6 As shown. Due to the full reaction of calcium carbonate ion oligomers and their advantages in thermal stability, at 150℃ and 200℃, the fluorescence of the organic fluorescent molecule H4TCPE is almost quenched, while the composite fluorescent material H4TCPE-Locked can still maintain its fluorescence performance.
[0079] Due to the stability of calcium carbonate ion oligomers to organic solvents, the fluorescent composite material can still maintain its good fluorescent properties after being soaked and dried in organic solvents, while the simple organic molecules are dissolved and dispersed after being soaked and dried in organic solvents, and their fluorescent properties are significantly reduced. The organic fluorescent molecules and fluorescent composite materials of Example 2 after being soaked and dried in ethanol solvents are shown in the figure below. Figure 7 shown.
Claims
1. A fluorescence enhanced composite material based on inorganic molecular locks, characterized in that: The invention comprises a calcium carbonate ion oligomer and an organic fluorescent molecule containing a carboxyl group. The calcium carbonate ion oligomer is cross-linked with the carboxyl group in the organic fluorescent molecule containing a carboxyl group through calcium ions.
2. The fluorescence enhanced composite material according to claim 1, characterized in that: The molar ratio of calcium ions in the calcium carbonate ion oligomer to carboxyl groups in the carboxyl-containing organic fluorescent molecules is 2-5:
1.
3. The preparation method according to claim 1 or 2, characterized in that: The carboxyl-containing organic fluorescent molecule is any one of tetrakis-(carboxyphenyl)ethylene, tetrakis[4-(4'-carboxyphenyl)phenyl]ethylene, 4,4'4"-tricarboxylic acid triphenylamine or perylene-3,4,9,10-tetracarboxylic acid.
4. The method for preparing the fluorescence enhanced composite material according to any one of claims 1 to 3, characterized in that: The following steps are involved: The calcium carbonate ion oligomer and the organic fluorescent molecule containing a carboxyl group are added to an organic solvent for dispersion, and an acid-base reaction is carried out to obtain the fluorescence enhanced composite material.
5. The preparation method according to claim 4, characterized in that: The carboxyl-containing organic fluorescent molecule is tetrakis-(carboxyphenyl)ethylene, 4,4'4"-triphenylamine tricarboxylate or perylene-3,4,9,10-tetracarboxylic acid, and the organic solvent is ethanol; or the carboxyl-containing organic fluorescent molecule is tetrakis[4-(4'-carboxyphenyl)phenyl]ethylene, and the organic solvent is tetrahydrofuran.
6. The preparation method according to claim 4 or 5, characterized in that: The acid-base reaction time is 3 to 48 hours.
7. The preparation method according to claim 6, characterized in that: When the carboxyl-containing organic fluorescent molecule is tetrakis-(carboxyphenyl)ethylene, tetrakis[4-(4'-carboxyphenyl)phenyl]ethylene or 4,4'4"-tricarboxylic acid triphenylamine, the acid-base reaction time is 6 to 12 hours; when the carboxyl-containing organic fluorescent molecule is perylene-3,4,9,10-tetracarboxylic acid, the acid-base reaction time is 24 to 48 hours.
8. The preparation method according to claim 4, characterized in that: The calcium carbonate ion oligomer is prepared by the following method: triethylamine as a capping agent, a calcium salt as a cation source, and carbon dioxide as an anion source are introduced into an organic solvent, and reacted at room temperature to obtain the calcium carbonate ion oligomer.
9. The preparation method according to claim 8, characterized in that: The molar ratio of the triethylamine to the calcium ion in the calcium salt is 20-100:
1.
10. Use of the fluorescence enhanced composite material according to any one of claims 1 to 3 in the field of anti-counterfeiting.
Citation Information
Cited By
Amine modified oligomer cross-linked epoxy resin material, preparation method and application
CN121673643A