Cleaning composition as well as preparation method and application thereof
By optimizing the aqueous cleaning agent containing amine oxides, water-retaining agents, and surfactants, the problem of corrosion of metal substrates by existing cleaning solutions has been solved, achieving efficient cleaning and improved yield.
Patent Information
- Application Number
- CN202411102130.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-22
AI Technical Summary
Existing cleaning solutions tend to corrode metal substrates when removing photoresist residues, leading to reduced wafer yield and difficulty in stable use over a wide temperature range.
A water-based cleaning agent composed of amine oxide, water-retaining agent and surfactant is used to improve cleaning effect and protect metal substrate from corrosion by optimizing the component ratio.
It achieves efficient cleaning of photoresist and etching residues, avoids particle accumulation and photoresist deposition, protects the metal substrate, is suitable for a wide temperature range, and improves the yield of semiconductor wafers.
Smart Images

Figure BDA0004989649040000021 
Figure BDA0004989649040000061 
Figure BDA0004989649040000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of semiconductor photoresist stripping, in particular to a cleaning composition and a preparation method and application thereof. Background Art
[0002] In the process of semiconductor component manufacturing, photoresist coating, exposure and development are essential process steps for component pattern manufacturing. At the end of patterning (i.e. after coating, exposure, development, ion implantation and etching of the photoresist layer) and before the next process, the photoresist residue and unexposed parts need to be completely removed.
[0003] Usually, multiple photolithography processes are required in the manufacture of semiconductor devices to obtain the required structural patterns. After etching, the photoresist needs to be peeled off from the surface of the wafer. However, in the previous process, the photoresist will undergo high-temperature baking, exposure, development, and etching, and will quickly cross-link and harden, forming a complex cross-linked network structure, and even undergo a certain degree of denaturation, making the photoresist more difficult to remove.
[0004] In the semiconductor manufacturing process, a two-step method (ashing and wet cleaning) is generally used to remove this layer of photoresist. The first step is to remove most of the photoresist by ashing; the second step is to use a cleaning solution and / or a cleaning process to clean the remaining photoresist, and the steps are generally to use a cleaning solution for cleaning, and then rinse and dry in sequence. That is, the photoresist on the semiconductor wafer is removed by immersing the semiconductor wafer in a cleaning agent or washing the semiconductor wafer with a cleaning agent. However, in the process of using a cleaning agent to remove residual polymer photoresist and inorganic substances, it is inevitable that damage will be caused to the metal substrate. In particular, in the process of using a chemical cleaning agent to remove photoresist and etching residues, metal corrosion (especially more active metals such as aluminum, titanium, tungsten, etc.) is a common and very serious problem, which often leads to a significant reduction in the wafer yield.
[0005] In the current wet cleaning process, the most commonly used cleaning liquids are alkaline cleaning liquids and fluorine-containing cleaning liquids. Among them, the alkali in the alkaline cleaning liquid is mostly alkali metal hydroxides, quaternary ammonium hydroxides, alcohol amines or hydroxylamines, etc. These components can dissolve photoresist and / or photoresist residues produced by etching, but the strong alkalinity can easily cause corrosion of the wafer pattern and substrate, and too little content cannot achieve the cleaning effect. In addition, hydroxylamine also has the problem of easy explosion and single source. Although the existing fluorine-containing cleaning liquid has been greatly improved, it still cannot well control the corrosion of metal and non-metallic substrates at the same time, and it is easy to cause changes in the channel feature size after cleaning, and it is easy to form particulate accumulation on the wafer surface after cleaning, or it may cause deposition or adhesion of photoresist on the wafer surface.
[0006] In view of this, the present invention is proposed. Summary of the invention
[0007] The object of the present invention is to provide a cleaning composition and a preparation method and application thereof. The cleaning composition can efficiently clean the photoresist and other etching residues after etching, and the cleaning composition is mild and has low corrosiveness, and will not damage the wafer pattern and the metal substrate that may be in contact with it, such as aluminum, titanium, tungsten and other metal substrates. The cleaning composition has a large operating window and can be used in a large temperature range, and has good application prospects in the field of semiconductor wafer cleaning.
[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0009] In a first aspect, the present invention provides a cleaning composition, wherein the cleaning composition comprises the following components by weight percentage:
[0010]
[0011] In the present invention, the cleaning composition is an aqueous cleaning agent composed of a certain proportion of amine oxide, a water retaining agent and a surfactant. Under the mutual cooperation and synergistic effect of each component, the cleaning effect of the cleaning agent on the photoresist after etching and any other etching residues is further improved. Even for the cross-linked and hardened mesh structure photoresist after etching, it still has good cleaning ability, and to a great extent avoids the problem of easy accumulation of particles on the surface of the semiconductor wafer after cleaning and the deposition or adhesion of the photoresist on the surface of the wafer. In addition, the cleaning composition is mild in nature and low in corrosiveness, and will not cause damage to the wafer pattern and the metal substrate that may be in contact, such as aluminum, titanium, tungsten and other metal substrates. The substrate does not corrode, and the operating window is large, and it can be used in a large temperature range, and has good application prospects in the field of semiconductor wafer cleaning.
[0012] Preferably, the cleaning composition comprises the following components by mass percentage:
[0013] Amine oxide 30.00~60.00%
[0014] Water-retaining agent 1.00~10.00%
[0015] Corrosion inhibitor 1.00~10.00%
[0016] Surfactant 0.05~8.00%
[0017] The balance is water.
[0018] In the present invention, by further optimizing the ratio among amine oxide, water retaining agent and surfactant, the cleaning effect and cleaning efficiency of the cleaning composition for photoresist are further improved, thereby ensuring the stability of the cleaning composition during a long cleaning process, and further enhancing the protective ability of the cleaning composition for a variety of metal substrate materials, thereby improving the yield of semiconductor wafers.
[0019] Preferably, the amine oxide is selected from N,N-dimethylethylamine-N-oxide and / or trimethylamine oxide.
[0020] In the present invention, the main component of the cleaning agent is preferably added with N,N-dimethylethylamine-N-oxide and / or trimethylamine oxide. The hydroxyl group and the amino group in the structure of these two amine oxides are directly connected, which can fully react with the photoresist residues to break them into small molecules, thereby falling off from the wafer surface and entering the solution.
[0021] Preferably, the water retaining agent is selected from any one of D-glucosamine, tripolyphosphate or triphosphate ester, or a combination of at least two thereof.
[0022] In the present invention, by further optimizing the water retaining agent, the water loss of the cleaning liquid under long-term high-temperature heating conditions is greatly reduced, the stability of the cleaning composition during the long-term cleaning process is ensured, and the damage to the metal substrate caused by the gradual increase in the concentration of water loss is avoided, thereby further enhancing the protection ability of the cleaning composition for various metal substrate materials.
[0023] Preferably, the corrosion inhibitor is selected from any one or a combination of at least two of salicylic acid, methoxysalicylic acid, 5-methylsalicylic acid methyl ester, ethyl salicylate, 4-amino-3-hydroxybenzoic acid, 4-hydroxyphthalic acid, 5-hydroxyisophthalic acid or p-hydroxyphenylethanol, preferably any one or a combination of at least two of ethyl salicylate, 4-amino-3-hydroxybenzoic acid, 5-hydroxyisophthalic acid or p-hydroxyphenylethanol.
[0024] In the present invention, by further optimizing the corrosion inhibitor, the carboxyl group or carbonyl group in the corrosion inhibitor structure is complexed with the metal, and the benzene ring is hydrophobic to form a metal protective layer, ensuring that the cleaning liquid in the degumming process will not corrode the metal it contacts.
[0025] Preferably, the surfactant is selected from any one or a combination of at least two of n-butanol, n-pentanol, n-hexanol, 3-methoxy-1-propanol, 2-amino-3-methyl-1-butanol or 4-methoxy-1-butanol.
[0026] In the present invention, by further optimizing the surfactant for the water retaining agent, the hydroxyl group in the surfactant structure forms a hydrogen bond with the water in the solution, and the other end is hydrophobic, thereby reducing the surface tension of the cleaning solution, so that the cleaning solution can quickly penetrate into the through hole of the wafer, which is beneficial to remove the post-etching residue in the through hole.
[0027] In a second aspect, the present invention provides a method for preparing the cleaning composition according to the first aspect, the preparation method comprising the following steps:
[0028] Amine oxide, a water retaining agent, a corrosion inhibitor, a surfactant and water are mixed and stirred to dissolve to obtain the cleaning composition.
[0029] Preferably, the temperature of the stirring and dissolving is 20-40°C.
[0030] Preferably, the rotation speed of the stirring and dissolving is 100 to 500 rpm.
[0031] Preferably, the stirring and dissolving time is 10 to 60 minutes.
[0032] In a third aspect, the present invention provides a use of the cleaning composition as described in the first aspect in cleaning semiconductor components after etching.
[0033] In a fourth aspect, the present invention provides a method for cleaning a semiconductor component after etching, the cleaning method comprising the following steps:
[0034] The etched semiconductor components are immersed in the cleaning composition, then washed with water and dried to obtain the cleaned semiconductor components.
[0035] Preferably, the soaking temperature is 40-80° C., and the soaking time is 10-60 min.
[0036] Preferably, the material of the semiconductor component includes any one of aluminum, titanium or tungsten.
[0037] Compared with the prior art, the present invention has the following beneficial effects:
[0038] The cleaning composition of the present invention can efficiently clean the photoresist and other etching residues after etching, and the cleaning composition is mild and low in corrosiveness, and will not cause damage to the chip pattern and the metal substrate that may be in contact with it, such as aluminum, titanium, tungsten and other metal substrates. The cleaning composition has a large operating window and can be used in a large temperature range. It has good application prospects in the field of semiconductor chip cleaning. DETAILED DESCRIPTION
[0039] Unless otherwise defined herein, scientific and technical terms used in conjunction with the present invention shall have the meanings commonly understood by those of ordinary skill in the art. The meaning and scope of the terms should be clear, however, in the case of any potential ambiguity, the definitions provided herein take precedence over any dictionary or external definitions. In this application, unless otherwise stated, the use of "or" means "and / or". In addition, the use of the term "including" and other forms is non-limiting.
[0040] It should be noted that specific details are described in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in a variety of other ways different from those described herein, and those skilled in the art can make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0041] The following will clearly and completely describe the implementation methods of the present invention in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] In a first aspect, the present invention provides a cleaning composition, wherein the cleaning composition comprises the following components by weight percentage:
[0043]
[0044] In the present invention, the cleaning composition is an aqueous cleaning agent composed of a certain proportion of amine oxide, a water retaining agent and a surfactant. Under the mutual cooperation and synergistic effect of each component, the cleaning effect of the cleaning agent on the photoresist after etching and any other etching residues is further improved. Even for the cross-linked and hardened mesh structure photoresist after etching, it still has good cleaning ability, and to a great extent avoids the problem of easy accumulation of particles on the surface of the semiconductor wafer after cleaning and the deposition or adhesion of the photoresist on the surface of the wafer. In addition, the cleaning composition is mild in nature and low in corrosiveness, and will not cause damage to the wafer pattern and the metal substrate that may be in contact, such as aluminum, titanium, tungsten and other metal substrates. The substrate does not corrode, and the operating window is large, and it can be used in a large temperature range, and has good application prospects in the field of semiconductor wafer cleaning.
[0045] As an optional embodiment of the present invention, taking the total mass of the cleaning composition as 100%, the content of the amine oxide is 25.00-65.00%, for example, it can be 25.00%, 26.00%, 28.00%, 30.00%, 32.00%, 34.00%, 36.00%, 38.00%, 40.00%, 42.00%, 44.00%, 46.00%, 48.00%, 50.00%, 52.00%, 54.00%, 56.00%, 58.00%, 60.00%, 62.00%, 64.00%, 65.00% and the like.
[0046] As an optional embodiment of the present invention, taking the total mass of the cleaning composition as 100%, the content of the water retaining agent is 0.10-15.00%, for example, it can be 0.10%, 0.20%, 0.50%, 0.80%, 1.00%, 1.50%, 2.00%, 2.50%, 3.00%, 3.50%, 4.00%, 4.50%, 5.00%, 6.00%, 7.00%, 8.00%, 9.00%, 10.00%, 11.00%, 12.00%, 13.00%, 14.00%, 15.00% and the like.
[0047] As an optional embodiment of the present invention, taking the total mass of the cleaning composition as 100%, the content of the corrosion inhibitor is 0.10-15.00%, for example, it can be 0.10%, 0.20%, 0.50%, 0.80%, 1.00%, 1.50%, 2.00%, 2.50%, 3.00%, 3.50%, 4.00%, 4.50%, 5.00%, 6.00%, 7.00%, 8.00%, 9.00%, 10.00%, 11.00%, 12.00%, 13.00%, 14.00%, 15.00% and the like.
[0048] As an optional embodiment of the present invention, taking the total mass of the cleaning composition as 100%, the content of the surfactant is 0.01-10.00%, for example, it can be 0.01%, 0.02%, 0.04%, 0.06%, 0.08%, 0.10%, 0.20%, 0.50%, 0.80%, 1.00%, 1.50%, 2.00%, 2.50%, 3.00%, 3.50%, 4.00%, 4.50%, 5.00%, 6.00%, 7.00%, 8.00%, 9.00%, 10.00% and the like.
[0049] As a preferred embodiment of the present invention, the cleaning composition comprises the following components by mass percentage:
[0050]
[0051] In the present invention, by further optimizing the ratio among amine oxide, water retaining agent and surfactant, the cleaning effect and cleaning efficiency of the cleaning composition for photoresist are further improved, thereby ensuring the stability of the cleaning composition during a long cleaning process, and further enhancing the protective ability of the cleaning composition for a variety of metal substrate materials, thereby improving the yield of semiconductor wafers.
[0052] As an optional embodiment of the present invention, the amine oxide is selected from N,N-dimethylethylamine-N-oxide and / or trimethylamine oxide.
[0053] In the present invention, the main component of the cleaning agent is preferably added with N,N-dimethylethylamine-N-oxide and / or trimethylamine oxide. The hydroxyl group and the amino group in the structure of these two amine oxides are directly connected, which can fully react with the photoresist residues to break them into small molecules, thereby falling off from the wafer surface and entering the solution.
[0054] As an optional embodiment of the present invention, the water retaining agent is selected from any one of D-glucosamine, tripolyphosphate or triphosphate ester, or a combination of at least two thereof.
[0055] In the present invention, by further optimizing the water retaining agent, the water loss of the cleaning solution under long-term high-temperature heating conditions is greatly reduced, the stability of the cleaning composition during the long-term cleaning process is ensured, and the damage to the metal substrate caused by the gradual increase in the concentration of water loss is avoided, and the protection ability of the cleaning composition for various metal substrate materials is further enhanced, and the yield of semiconductor wafers is more effectively improved. In addition, if the water retaining agent is lacking, the volatilization speed of water will be too fast, which will also lead to poor cleaning effect.
[0056] As an optional embodiment of the present invention, the corrosion inhibitor is selected from any one or a combination of at least two of salicylic acid, methoxysalicylic acid, 5-methylsalicylic acid methyl ester, ethyl salicylate, 4-amino-3-hydroxybenzoic acid, 4-hydroxyphthalic acid, 5-hydroxyisophthalic acid or p-hydroxyphenylethanol.
[0057] In the present invention, by further optimizing the corrosion inhibitor, the carboxyl group or carbonyl group in the corrosion inhibitor structure is complexed with the metal, and the benzene ring is hydrophobic to form a metal protective layer, ensuring that the cleaning liquid in the degumming process will not corrode the metal it contacts.
[0058] As an optional embodiment of the present invention, the surfactant is selected from any one of n-butanol, n-pentanol, n-hexanol, 3-methoxy-1-propanol, 2-amino-3-methyl-1-butanol or 4-methoxy-1-butanol, or a combination of at least two thereof.
[0059] In the present invention, by further optimizing the surfactant, the hydroxyl group in the surfactant structure forms hydrogen bonds with the water in the solution, and the other end is hydrophobic, thereby reducing the surface tension of the cleaning solution, so that the cleaning solution can quickly penetrate into the through holes of the wafer, which is beneficial to removing the post-etching residues in the through holes.
[0060] In a second aspect, the present invention provides a method for preparing the cleaning composition according to the first aspect, the preparation method comprising the following steps:
[0061] Amine oxide, a water retaining agent, a corrosion inhibitor, a surfactant and water are mixed and stirred to dissolve to obtain the cleaning composition.
[0062] As an optional embodiment of the present invention, the stirring and dissolving temperature is 20-40°C, for example, it can be 25°C, 26°C, 28°C, 30°C, 32°C, 35°C, 38°C, 40°C, etc.
[0063] As an optional embodiment of the present invention, the rotation speed of the stirring and dissolving is 100-500 rpm, for example, it can be 100 rpm, 150 rpm, 200 rpm, 250 rpm, 300 rpm, 350 rpm, 400 rpm, 450 rpm, 500 rpm, etc.
[0064] As an optional embodiment of the present invention, the stirring and dissolving time is 10 to 60 min, for example, it can be 10 min, 15 min, 20 min, 25 min, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min, etc.
[0065] In a third aspect, the present invention provides a use of the cleaning composition as described in the first aspect in cleaning semiconductor components after etching.
[0066] In a fourth aspect, the present invention provides a method for cleaning a semiconductor component after etching, the cleaning method comprising the following steps:
[0067] The etched semiconductor components are immersed in the cleaning composition, then washed with water and dried to obtain the cleaned semiconductor components.
[0068] As an optional embodiment of the present invention, the immersion temperature is 40-80°C, for example, it can be 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, etc.
[0069] As an optional embodiment of the present invention, the soaking time is 10 to 60 minutes, for example, it can be 10 minutes, 15 minutes, 20 minutes, 25 minutes, 30 minutes, 35 minutes, 40 minutes, 45 minutes, 50 minutes, 55 minutes, 60 minutes, etc.
[0070] As an optional implementation of the present invention, the material of the semiconductor component includes any one of aluminum, titanium or tungsten.
[0071] The features and performance of the present invention are further described in detail below in conjunction with specific embodiments.
[0072] Examples 1 to 13
[0073] Examples 1 to 13 provide cleaning compositions with different composition ratios, each of which includes the following components by mass percentage, as shown in Table 1 below:
[0074] Table 1
[0075]
[0076]
[0077] The preparation method of the cleaning composition comprises the following steps:
[0078] Amine oxide, a water retaining agent, a corrosion inhibitor, a surfactant and deionized water were mixed, and stirred at 25° C. and 300 rpm for 30 minutes to dissolve, thereby obtaining the above cleaning composition.
[0079] Comparative Examples 1 to 8
[0080] Comparative Examples 1 to 8 provide cleaning compositions with different composition ratios, each of which includes the following components by mass percentage, as shown in Table 2 below:
[0081]
[0082] The preparation method of the cleaning composition comprises the following steps:
[0083] The raw materials of each comparative example and deionized water were mixed according to the proportions, and stirred at 25° C. and 300 rpm for 30 minutes to dissolve, thereby obtaining the above cleaning composition.
[0084] Comparative Example 9
[0085] This comparative example provides a fluoride-containing cleaning composition, which comprises, by mass percentage, 5% hydrofluoric acid, 15% ethylene glycol dimethyl ether, 8% cyclopentane sulfone, 5% 2-pyrrolidone, 0.5% propylene glycol polyether, 0.5% dihydroxyethyl imidazoline and 66% water.
[0086] Comparative Example 10
[0087] This comparative example provides a fluoride-containing cleaning composition, which comprises, by mass percentage, 0.1% ammonium fluoride, 74.85% methyl ethyl sulfoxide, 10% hydrogen peroxide, 0.05% pentamethyldiethylenetriamine and 15% water.
[0088] Test Case
[0089] Test samples: cleaning compositions provided in Examples 1 to 13, cleaning compositions provided in Comparative Examples 1 to 10:
[0090] Test method:
[0091] Etch rate of aluminum :Put the cleaning solution in the reactor and heat it to the experimental temperature. Then place the copper wafer cut into 3cm*3cm pieces in it and soak it at a constant temperature for 30 minutes, wash it with water, and blow it dry with nitrogen. Then use a four-point probe to measure the change in resistance value before and after etching to calculate the etching rate.
[0092] Etching rate of titanium :Put the cleaning solution in the reactor and heat it to the experimental temperature. Then place the silver wafer cut into 3cm*3cm pieces in the reactor and soak it at a constant temperature for 30 minutes, wash it with water, and blow it dry with nitrogen. Then use a four-point probe to measure the change in resistance value before and after etching to calculate the etching rate.
[0093] Etch rate of tungsten :Put the cleaning solution in the reactor and heat it to the experimental temperature. Then place the titanium wafer cut into 3cm*3cm pieces in it and soak it at a constant temperature for 30 minutes, wash it with water, and blow it dry with nitrogen. Then use a four-point probe to measure the change in resistance value before and after etching to calculate the etching rate.
[0094] Cleaning effect test: Place the cleaning solution in a reactor and heat it to the experimental temperature. Cut the exposed and developed wafer into 2cm*2cm square pieces, soak the square pieces in the solution at a constant temperature for 30 minutes, wash with water, and blow dry with nitrogen. Then observe the removal of residues on the surface of the cleaned wafer square pieces using an optical microscope and SEM.
[0095] Among them, A-complete removal; B-residue ≤ 10%; C-10%<residue ≤ 30%; D-residue> 30%.
[0096] Among them, “-” means that only the cleaning effect is compared, and the etching rate is not measured.
[0097] The specific test results are shown in Table 3:
[0098] Table 3
[0099]
[0100]
[0101] As shown in Table 3, after different metal substrates were immersed in the cleaning composition of the present invention for 30 minutes at 40-80°C, it was found that the etching rate of aluminum was The etching rate for titanium is The etching rate for tungsten is Next, after using the cleaning composition of the present invention to clean the wafer after exposure and development, it was found that the photoresist residues can be completely removed.
[0102] As shown by the data of Comparative Example 1, due to the lack of amine oxide, there is no effective component in the composition that can fully react with the photoresist residue to break it into small molecular substances. Therefore, it is difficult to clean the wafer after exposure and development, and the photoresist residue after cleaning is large.
[0103] As shown in the data of Comparative Example 2, the lack of a water retaining agent will cause the water to evaporate too quickly, which will also lead to a poor cleaning effect. Moreover, as the water is lost, the concentration of the substance gradually increases, causing certain etching damage to the metal substrate.
[0104] As shown in the data of Comparative Example 3, the lack of surfactant reduces the etching residue in Comparative Example 1, but the etching residue in the through hole is still relatively large.
[0105] As shown in the data of Comparative Example 4, the lack of corrosion inhibitor leads to a significant increase in the etching rate of the cleaning composition for aluminum, titanium and tungsten.
[0106] As shown in the data of Comparative Example 5, the use of the alcoholamine compound diglycolamine instead of the amine oxide of the present application results in poor cleaning effect of the composition.
[0107] As shown in the data of Comparative Example 6, using the alcohol-based water-retaining agent glycerol instead of the water-retaining agent of the present application will also lead to a decrease in the cleaning effect of the composition.
[0108] As shown by the data of Comparative Example 7, using polyethylene glycol instead of the surfactant of the present application will also lead to a decrease in the cleaning effect of the composition.
[0109] As shown in the data of Comparative Example 8, the use of corrosion inhibitors other than those of the present application resulted in a significant increase in the etching rate of the cleaning composition for aluminum, titanium, and tungsten.
[0110] As shown in the data of Comparative Example 9, when a cleaning system containing hydrofluoric acid is selected, the metal etching rate is significantly increased. This is because the high hydrofluoric acid content easily corrodes the substrate, and the cleaning effect of the cleaning system is poor. After cleaning, it is found that a certain amount of particulate matter will still form on the surface of the semiconductor wafer, and the photoresist is more likely to stick to the substrate and cannot be completely detached.
[0111] As shown in the data of Comparative Example 10, a cleaning system containing ammonium fluoride was selected, and its content was reduced relative to that of hydrofluoric acid to reduce the etching of metals by high-content fluorides. However, it is not difficult to find that the cleaning effect of the cleaning composition of this formula is also reduced relative to that of Comparative Example 9. In addition, the fluorine-containing cleaning solution will cause corrosion to non-metallic film layers.
[0112] In summary, the cleaning composition of the present invention can efficiently clean the photoresist and other etching residues after etching, and the cleaning composition is mild in nature and low in corrosiveness, and will not damage the wafer pattern and the metal substrate that may be in contact. In addition, Example 1 shows that the post-etching cleaning composition of the present invention has a large operating window and can be used in a large temperature range, and has good application prospects in the field of semiconductor wafer cleaning.
[0113] Finally, it should be noted that the above embodiments are only used to illustrate the implementation methods of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the implementation methods described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A cleaning composition, characterized in that The cleaning composition comprises the following components by weight percentage:
2. The cleaning composition according to claim 1, characterized in that The cleaning composition comprises the following components by weight percentage:
3. The cleaning composition according to claim 1 or 2, characterized in that The amine oxide is selected from N,N-dimethylethylamine-N-oxide and / or trimethylamine oxide.
4. The cleaning composition according to claim 1 or 2, characterized in that The water retaining agent is selected from any one of D-glucosamine, tripolyphosphate or triphosphate ester or a combination of at least two thereof.
5. The cleaning composition according to claim 1 or 2, characterized in that The corrosion inhibitor is selected from any one or a combination of at least two of salicylic acid, methoxysalicylic acid, 5-methylsalicylic acid methyl ester, ethyl salicylate, 4-amino-3-hydroxybenzoic acid, 4-hydroxyphthalic acid, 5-hydroxyisophthalic acid or p-hydroxyphenylethanol, preferably any one or a combination of at least two of ethyl salicylate, 4-amino-3-hydroxybenzoic acid, 5-hydroxyisophthalic acid or p-hydroxyphenylethanol.
6. The cleaning composition according to claim 1 or 2, characterized in that The surfactant is selected from any one or a combination of at least two of n-butanol, n-pentanol, n-hexanol, 3-methoxy-1-propanol, 2-amino-3-methyl-1-butanol or 4-methoxy-1-butanol.
7. A method for preparing a cleaning composition according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: Amine oxide, a water retaining agent, a corrosion inhibitor, a surfactant and water are mixed and stirred to dissolve to obtain the cleaning composition.
8. The method for preparing the cleaning composition according to claim 7, characterized in that: The stirring and dissolving temperature is 20 to 40°C; And / or, the rotation speed of the stirring and dissolving is 100 to 500 rpm; And / or, the stirring and dissolving time is 10 to 60 minutes.
9. Use of the cleaning composition according to any one of claims 1 to 6 in cleaning semiconductor components after etching.
10. A method for cleaning semiconductor components after etching, characterized in that: The cleaning method comprises the following steps: The etched semiconductor components are immersed in the cleaning composition according to any one of claims 1 to 6, and then washed with water and dried to obtain cleaned semiconductor components; Preferably, the soaking temperature is 40 to 80° C., and the soaking time is 10 to 60 minutes; Preferably, the material of the semiconductor component includes any one of aluminum, titanium or tungsten.