Molten iron desulfurization slag treatment method and treatment system

The desulfurization slag of molten iron is treated through drum method and multi-stage magnetic separation screening technology, which solves the problems of long treatment cycle and low slag iron quality, and achieves efficient slag iron recovery and environmental protection.

CN118996024APending Publication Date: 2024-11-22SHANGHAI BAOSTEEL METALLURGICAL CONSTRUCTION CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310553012.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing iron desulfurization slag treatment process has the problems of long treatment cycle and low slag iron quality, resulting in limited resource utilization and environmental pollution.

Method used

The iron desulfurization slag is pretreated by the roller method, and the slag is separated into iron powder, slag block material and slag powder material through multi-stage magnetic separation and screening technology. The quality of slag iron is further improved through rod grinding and magnetic separation. .

Benefits of technology

The treatment cycle is shortened, the quality of slag iron recycling is improved, environmental pollution is avoided, and the high added value of slag iron is realized.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996024A_ABST
    Figure CN118996024A_ABST
Patent Text Reader

Abstract

The invention discloses a molten iron desulfurization slag treatment method and system in the technical field of steel slag treatment, and the method comprises the following steps: pretreating molten iron desulfurization slag by adopting a roller method to obtain a primary treatment material; performing magnetic separation on the primary treatment material to obtain a primary magnetic separation material and a primary slag material; screening the primary slag charge to obtain a primary screen material and a slag block material; carrying out magnetic separation on the primary undersize material to obtain a secondary magnetic separation material and a secondary slag material; performing screening and magnetic separation on the secondary slag charge for many times to obtain an iron powder material, a slag powder material and a slag particle material; performing rod milling on the primary magnetic separation material and the secondary magnetic separation material to obtain a rod milled material; and screening and magnetically separating the rod grinding material to obtain an iron powder material, a slag powder material, an iron block material and a slag block material. According to the method, slag and iron in the molten iron desulfurization slag are effectively separated, flying dust, waste water and air pollution are avoided, meanwhile, the treatment time of the molten iron desulfurization slag is shortened, and the quality of the slag iron is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel slag treatment, and in particular to a method and system for treating molten iron desulfurization slag. Background Art

[0002] Hot metal desulfurization slag refers to the molten iron produced by the blast furnace and a small amount of hot metal slag that undergoes hot metal pretreatment before steelmaking, and is produced by front slag skimming, rear slag skimming, mixing iron car slag discharge, steelmaking iron receiving station, electric furnace iron receiving station, etc. The hot metal desulfurization slag floats on the surface of the molten iron and is removed from the ladle by mechanical slag skimming.

[0003] At present, the treatment methods of hot metal desulfurization slag mainly include pit-type hot pouring process and slag pot soaking process. Among them, the pit-type hot pouring process is the most primitive hot metal desulfurization slag treatment process, which is to directly pour the high-temperature hot metal slag into the slag pit, and then dispose of it centrally after natural cooling, shovel transfer, stacking and cooling. Because the slag and molten iron are easily mixed to form a large slag lump, subsequent treatment is more difficult. This treatment process not only occupies a large area, but also has many turnover times, serious dust and pollution. The slag iron finally recovered has a low grade and high sulfur content, and its resource utilization is limited. In addition, when cooling water is sprayed on hot metal slag, only a layer of blackening is formed on the surface. A large amount of water can easily penetrate into the slag pile and cause water accumulation in the slag pit, which is easy to explode when the red slag is overturned; at the same time, when the steel slag is overturned, it splashes everywhere, which is very dangerous, and yellow smoke and black smoke dust rise up.

[0004] The process route of the hot metal slag soaking production process is slag receiving → transportation → tank unloading → empty tank replacement → slag padding → slag receiving; the process of red slag tank watering → cold slag tank turning over → empty tank. The specific method of hot metal slag soaking is: ① Put the slag tank in the specified position, leaving 50cm space between the slag tanks; ② The slag volume can be controlled at about 40 to 60cm below the tank mouth according to the expansion of slag tanks of different capacities and hot metal slag, and check that the slag temperature is normal; ③ Perform watering operations in the following order: watering for 20 minutes → interval for 20 minutes → watering for 20 minutes → interval for 20 minutes → watering for 20 minutes → interval for 20 minutes → stop watering after 20 minutes and air cool for 12 hours. During the operation, the amount of water should be controlled to avoid water accumulation on the surface of the hot metal slag and control the water level to overflow; ④ After confirming that the slag tank has cooled, adjust the amount of watering and the time of watering in time according to the dryness and wetness of the slag; ⑤ The slag tank truck transports the slag tank to a fixed position to turn the tank over; ⑥ Confirm that there is no red slag and no dust. This process is a great improvement over the pit-type hot pouring process, but the molten iron desulfurization slag contains components such as C and S, and toxic gases such as CO and H2S and dust-containing waste steam are produced during the soaking process, polluting the atmosphere. There is also the possibility of sewage flowing across the surface and generating wastewater. The treatment cycle is long, and many slag pots are occupied, covering a large area. The slag pots are subjected to alternating hot and cold changes, resulting in large cracking and deformation losses, and high costs. At the same time, the recovered slag iron is of low grade and high sulfur content, and its resource utilization is limited.

[0005] Therefore, how to shorten the processing cycle of molten iron desulfurization slag and improve the quality of slag iron recovery has become a technical problem that needs to be urgently solved by technical personnel in this field. Summary of the invention

[0006] In view of this, the object of the present invention is to provide a method and system for treating molten iron desulfurization slag, so as to solve the technical problems of long treatment cycle and low slag quality in the existing molten iron desulfurization slag treatment process.

[0007] The technical solution adopted by the present invention is: a method for treating molten iron desulfurization slag, comprising the following steps:

[0008] S1: pre-treating the molten iron desulfurization slag by a drum method to obtain a primary treated material;

[0009] S2: During the transportation process, the primary processed material is subjected to magnetic separation to obtain a primary magnetically separated material and a primary slag material;

[0010] S3: Screening the primary slag material to obtain primary undersize material and slag block material;

[0011] S4: During the conveying process, the primary undersize material is subjected to magnetic separation to obtain secondary magnetic separation material and secondary slag material;

[0012] S5: Screening the secondary slag material to obtain secondary undersize material and slag granules;

[0013] S6: During the conveying process, the secondary screened material is subjected to magnetic separation to obtain iron powder and tertiary slag;

[0014] S7: Screening the three slag materials to obtain slag powder and slag granules;

[0015] S8: performing rod grinding on the primary magnetic separation material and the secondary magnetic separation material to obtain rod grinding material;

[0016] S9: Screening the rod mill material to obtain rod mill screen upper material and rod mill screen lower material;

[0017] S10: performing magnetic separation on the rod mill screen material to obtain iron powder and slag powder, and performing magnetic separation on the rod mill screen material to obtain iron block material and slag block material.

[0018] Preferably, in S2, the primary processed material is conveyed by a first magnetic separation belt conveyor, and the primary processed material being conveyed is magnetically separated successively by a first suspended magnetic separator and a first magnetic separation belt conveyor.

[0019] Preferably, the primary slag material is screened by a first vibrating screen with a screening particle size of 16 mm to obtain primary undersize material of 0 to 16 mm and slag block material of 16 to 300 mm.

[0020] Preferably, in S5, the secondary slag material is screened by a second vibrating screen with a screening particle size of 8 mm to obtain secondary undersize material of 0 to 8 mm and slag particles of 8 to 16 mm.

[0021] Preferably, in S7, the tertiary slag is screened by a third vibrating screen with a screening particle size of 5 mm to obtain slag powder of 0 to 5 mm and slag granules of 5 to 8 mm.

[0022] Preferably, in S9, the rod mill material is screened by a fourth vibrating screen with a screening particle size of 8 mm to obtain a rod mill screen undersize of 0 to 8 mm and a rod mill screen oversize of 8 to 200 mm.

[0023] Preferably, in S10, the rod mill screen material is magnetically separated by a dry magnetic separator to obtain 0-8 mm iron powder and 0-8 mm slag powder, and the rod mill screen material is magnetically separated by a second hanging magnetic separator to obtain 8-200 mm slag iron block material and 8-200 mm slag block material.

[0024] The second object of the present invention is to provide a molten iron desulfurization slag treatment system, including a slag-iron separation module, a slag material treatment module and a magnetic separation material treatment module.

[0025] The slag-iron separation module includes a pretreatment device, a feeder, a first magnetic separation belt conveyor and a first suspended magnetic separator. The pretreatment device can perform a drum method treatment on the molten iron desulfurization slag and obtain a primary treated material; the feeder is arranged at the feeding end of the first magnetic separation belt conveyor, and the feeder is used to supply the primary treated material to the first magnetic separation belt conveyor; the first suspended magnetic separator is arranged above the first magnetic separation belt conveyor, and can magnetically separate the first magnetic separation material from the surface of the primary treated material; the head wheel of the first magnetic separation belt conveyor is a permanent magnet roller, and can magnetically separate the first magnetic separation material from the inside of the primary treated material.

[0026] The slag processing module includes a first vibrating screen, a second magnetic separation belt conveyor, a second vibrating screen, a third magnetic separation belt conveyor and a third vibrating screen; the first vibrating screen can screen the primary slag output by the first magnetic separation belt conveyor into primary undersize material and slag block material; the second magnetic separation belt conveyor is arranged between the first vibrating screen and the second vibrating screen, and is used to transport the primary undersize material screened by the first vibrating screen to the second vibrating screen, and magnetically separate the second magnetic separation material from the primary undersize material during the conveying process; the second vibrating screen can screen the secondary slag output by the second magnetic separation belt conveyor into secondary undersize material and slag granular material; the third magnetic separation belt conveyor is arranged between the second vibrating screen and the third vibrating screen, and is used to transport the secondary undersize material screened by the second vibrating screen to the third vibrating screen, and magnetically separate the iron powder material from the secondary undersize material during the conveying process; the third vibrating screen can screen the tertiary slag output by the third magnetic separation belt conveyor into slag powder material and slag granular material.

[0027] The magnetic material processing module includes a rod mill, a fourth vibrating screen, a dry magnetic separator and a second suspended magnetic separator; the rod mill can rod grind the primary magnetic separation material and the secondary magnetic separation material; the fourth vibrating screen can screen the rod mill material output by the rod mill into rod mill screen upper material and rod mill screen lower material; the dry magnetic separator can magnetically separate iron powder from the rod mill screen lower material; the second suspended magnetic separator can magnetically separate iron block material from the rod mill screen upper material.

[0028] Beneficial effects of the present invention:

[0029] The present invention firstly pre-treats the molten iron desulfurization slag by a drum method, so that the molten iron desulfurization slag becomes a primary treatment material with a particle size within 300 mm, and then separates the magnetic separation material and the slag material by two magnetic separation methods, and then screens the slag material into iron powder material, slag block material and slag powder material by multi-stage screening and magnetic separation of the slag material, and screens the magnetic separation material into iron powder material, iron block material, slag powder material and slag block material by rod grinding, screening and magnetic attraction of the magnetic separation material, which not only improves the slag iron recovery quality, shortens the treatment cycle, but also avoids environmental pollution. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a schematic structural diagram of the molten iron desulfurization slag treatment system of the present invention.

[0031] Description of reference numerals in the figures:

[0032] 100. Slag and iron separation module;

[0033] 101, slag receiving point; 102, pretreatment device; 103, feeder; 104, first magnetic separation belt conveyor; 105, first suspension magnetic separator; 106, first magnetic separation tank;

[0034] 200. Slag processing module;

[0035] 201, first vibrating screen; 202, first trough; 203, second magnetic separation belt conveyor; 204, second magnetic separation trough; 205, second vibrating screen; 206, second trough; 207, third magnetic separation belt conveyor; 208, first iron powder trough; 209, third vibrating screen; 210, third trough; 211, fourth trough;

[0036] 300. Magnetic material separation processing module;

[0037] 301, rod mill; 302, fourth vibrating screen; 303, first belt conveyor; 304, dry magnetic separator; 305, second iron powder trough; 306, slag powder trough; 307, second belt conveyor; 308, second suspended magnetic separator; 309, rod mill iron block trough; 310, rod mill slag block trough. DETAILED DESCRIPTION

[0038] The specific embodiments of the present invention are further described in detail below in conjunction with the accompanying drawings. These embodiments are only used to illustrate the present invention, but not to limit the present invention.

[0039] In the description of the present invention, it should be noted that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.

[0040] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0041] Furthermore, in the description of the present invention, unless otherwise specified, “plurality” means two or more.

[0042] Examples, such as Figure 1As shown, a method for treating molten iron desulfurization slag is provided. By treating the molten iron desulfurization slag by this method, not only the slag iron recovery quality can be improved, but also waste materials and environmental pollution are not generated. The method comprises the following steps:

[0043] S1: Pre-treat the molten iron desulfurization slag by the drum method to obtain the primary treated material.

[0044] S2: During the transportation process, the primary processed material is magnetically separated to obtain primary magnetically separated material and primary slag material.

[0045] S3: Screening the primary slag material to obtain primary undersize material and slag block material.

[0046] S4: During the transportation process, the primary screened material is magnetically separated to obtain secondary magnetically separated material and secondary slag material.

[0047] S5: Screening the secondary slag material to obtain secondary undersize material and slag pellets.

[0048] S6: During the transportation process, the secondary screened material is magnetically separated to obtain iron powder and tertiary slag.

[0049] S7: Screening the tertiary slag to obtain slag powder and slag granules.

[0050] S8: Rod milling the primary magnetic separation material and the secondary magnetic separation material to obtain rod mill material.

[0051] S9: Screening the rod mill material to obtain rod mill screen upper material and rod mill screen lower material.

[0052] S10: magnetically separating the material under the rod mill screen to obtain iron powder and slag powder, and magnetically separating the material on the rod mill screen to obtain iron block and slag block.

[0053] The present application first pre-treats the molten iron desulfurization slag through the drum method, so that the molten iron desulfurization slag becomes a primary treatment material with a particle size of less than 300 mm, and then divides the primary treatment material into magnetic separation material and slag material through two magnetic separation methods, and then through multi-stage screening and magnetic separation of the slag material, the slag material can be screened into iron powder material, slag block material and slag powder material, and through rod grinding, screening and magnetic attraction of the magnetic separation material, the magnetic separation material can be screened into iron powder material, iron block material, slag powder material and slag block material, which not only shortens the processing cycle and improves the quality of slag iron recovery, but also avoids environmental pollution.

[0054] Preferably, in step S2, the primary treated material is conveyed by the first magnetic separation belt conveyor 104, and the surface of the primary treated material in transportation is firstly subjected to magnetic separation by the first suspended magnetic separator 105, and then the internal magnetic separation of the primary treated material in transportation is performed by the permanent magnet roller of the first magnetic separation belt conveyor 104, so as to obtain the primary magnetic separation material.

[0055] Preferably, in step S3, the primary slag material is screened by a first vibrating screen 201 with a screening particle size of 16 mm to obtain primary undersize material of 0 to 16 mm and slag block material of 16 to 300 mm.

[0056] Preferably, in step S5, the secondary slag material is screened by a second vibrating screen 205 with a screening particle size of 8 mm to obtain secondary undersize material of 0 to 8 mm and slag particles of 8 to 16 mm.

[0057] Preferably, in step S7, the tertiary slag is screened by a third vibrating screen 209 with a screening particle size of 5 mm to obtain slag powder of 0 to 5 mm and slag granules of 5 to 8 mm.

[0058] Preferably, in step S9, the rod mill material is screened by a fourth vibrating screen 302 with a screening particle size of 8 mm to obtain a rod mill screen undersize of 0 to 8 mm and a rod mill screen oversize of 8 to 200 mm.

[0059] Preferably, in step S10, the rod mill screen material is magnetically separated by a dry magnetic separator 304 to obtain iron powder of 0 to 8 mm and slag powder of 0 to 8 mm, and the rod mill screen material is magnetically separated by a second suspended magnetic separator 308 to obtain slag iron blocks of 8 to 200 mm and slag blocks of 8 to 200 mm.

[0060] Specific embodiment 1, a method for treating molten iron desulfurization slag, the method comprising the following steps:

[0061] First, the slag is received at the slag receiving point of the molten iron desulfurization slag by a tank car, and the slag pot containing the high-temperature liquid molten iron desulfurization slag is transferred from the slag receiving point to the drum method steel slag processing point station, and the slag pot on the station is lifted by a crane to the receiving platform of the pretreatment device 102; then the molten iron desulfurization slag is subjected to drum method treatment by remotely operating the pretreatment device 102, and the particle size of the treated molten iron drum slag is less than 300 mm, which is output to the slag trough on the discharge side of the pretreatment device 102 as a standby for primary treatment material.

[0062] First, the primary processed material is loaded onto the feeder 103 of the secondary processing production line by a loader, and the feeder 103 is located above the loading end of the first magnetic separation belt conveyor 104; the primary processed material is then transported to the first vibrating screen 201 by the first magnetic separation belt conveyor 104. During the transportation process, a first suspended magnetic separator 105 is provided above the middle of the first magnetic separation belt conveyor 104, and the first suspended magnetic separator 105 can magnetically separate the magnetic material on the surface of the primary processed material. At the same time, the head roller (discharging end) of the first magnetic separation belt conveyor 104 is a permanent magnet roller, and the magnetic material inside the primary processed material can be magnetically separated by the permanent magnet roller. Then, during the transportation process, the primary magnetic material is magnetically separated from the primary processed material, and the primary slag material after magnetic separation is transported to the first vibrating screen 201.

[0063] The screening particle size of the first vibrating screen 201 is 16 mm. The primary slag material can be screened by the first vibrating screen 201 to obtain primary undersize material of 0-16 mm and slag block material of 16-300 mm. The slag block material of 16-300 mm is returned to production for use as tank padding material; the primary undersize material of 0-16 mm is conveyed to the second vibrating screen 205 by the second magnetic separation belt conveyor 203. The head roller (discharging end) of the second magnetic separation belt conveyor 203 is a permanent magnet roller, and secondary magnetic separation material can be magnetically separated from the primary undersize material by the permanent magnet roller. The secondary slag material after magnetic separation enters the second vibrating screen 205.

[0064] The screening particle size of the second vibrating screen 205 is 8 mm. The secondary slag can be screened by the second vibrating screen 205 to obtain 8-16 mm slag blocks that can be returned to society for utilization as asphalt aggregate; the secondary screened material of 0-8 mm is conveyed to the third vibrating screen 209 by the third magnetic separation belt conveyor 207; the head roller (discharging end) of the third magnetic separation belt conveyor 207 is a permanent magnet roller, which can be used to magnetically separate iron from the secondary screened material, and the iron powder of 0-8 mm is used as slag iron powder for reverse production, while the tertiary slag after magnetic separation enters the third vibrating screen 209.

[0065] The screening particle size of the third vibrating screen 209 is 5 mm. The tertiary slag can be screened by the third vibrating screen 209 to obtain 5-8 mm slag blocks that can be returned to society for utilization as asphalt aggregates; and 0-5 mm slag powder can be returned to society for utilization as fine powder raw materials.

[0066] The primary magnetic separation material and the secondary magnetic separation material below 300 mm are fed to the rod mill 301 by a loader and rod-milled to below 200 mm. The rod mill material processed by the rod mill 301 enters the fourth vibrating screen 302 with a screening particle size of 8 mm. The rod mill material is screened by the fourth vibrating screen 302 to obtain 8-200 mm rod mill screen material and 0-8 mm rod mill screen material; the 8-200 mm rod mill screen material is magnetically separated by the second hanging magnetic separator 308 to obtain 8-200 mm rod mill screen material. The iron block material of 8-200mm and the slag block material of 8-200mm, among which the iron block material of 8-200mm (also called rod mill magnetic separation material) is used as direct supply slag iron block for steelmaking, and the slag block material of 8-200mm is used as padding material for reverse production; the 0-8mm rod mill undersize material is magnetically separated by a dry magnetic separator 304 to obtain 0-8mm iron powder material and 0-8mm slag powder material, among which the 0-8mm iron powder material is used as slag iron powder for ironmaking, and the 0-8mm slag powder material is used as steel slag fine powder for social use.

[0067] After testing, TFe in 8-200mm iron blocks is ≥96%, TFe in 0-8mm iron powder is ≥90%, and MFe in 5-16mm slag particles and 0-8mm slag powder is ≤1%, thus achieving complete separation of slag and iron and high value-added utilization of molten iron desulfurization slag.

[0068] Examples, such as Figure 1 As shown, a molten iron desulfurization slag processing system includes a slag-iron separation module 100, a slag material processing module 200 and a magnetic separation material processing module 300.

[0069] The slag iron separation module 100 includes a slag receiving point 101, a pretreatment device 102, a feeder 103, a first magnetic separation belt conveyor 104 and a first suspension magnetic separator 105; the tank car can be loaded with molten iron desulfurization slag at the slag receiving point 101; the pretreatment device 102 can perform a drum method treatment on the molten iron desulfurization slag and obtain a primary treatment material with a particle size of less than 300 mm; the feeder 103 is arranged at the feeding end of the first magnetic separation belt conveyor 104, and the primary treatment material is fed into the tank car by a loader. The feeder 103 can continuously supply the primary processed material to the first magnetic separation belt conveyor 104; the first suspended magnetic separator 105 is arranged above the middle of the first magnetic separation belt conveyor 104, and the first suspended magnetic separator 105 can magnetically separate the first magnetic material from the surface of the primary processed material; the head wheel of the first magnetic separation belt conveyor 104 is a permanent magnet roller, which can magnetically separate the first magnetic material from the inside of the primary processed material, and the first magnetic material is stored in the first magnetic separation tank 106.

[0070] The slag processing module 200 includes a first vibrating screen 201, a second magnetic separation belt conveyor 203, a second vibrating screen 205, a third magnetic separation belt conveyor 207 and a third vibrating screen 209; the first vibrating screen 201 is located below the discharge end of the first magnetic separation belt conveyor 104, and the first vibrating screen 201 can screen the primary slag output by the first magnetic separation belt conveyor 104 into primary undersize material and slag block material, and the slag block material is stored in the first material trough 202; the second magnetic separation belt conveyor 203 is arranged between the first vibrating screen 201 and the second vibrating screen 205, and is used to transport the primary undersize material screened by the first vibrating screen 201 to the second vibrating screen 205, and magnetically select the second magnetic material from the primary undersize material during the transportation process, and the second magnetic material The slag is stored in the second magnetic separation tank 204; the second vibrating screen 205 can screen the secondary slag output from the second magnetic separation belt conveyor 203 into secondary undersize material and slag granules, and the slag granules are stored in the second material tank 206; the third magnetic separation belt conveyor 207 is arranged between the second vibrating screen 205 and the third vibrating screen 209, and is used to transport the secondary undersize material screened by the second vibrating screen 205 to the third vibrating screen 209, and magnetically select iron powder from the secondary undersize material during the transportation process, and the iron powder is stored in the first iron powder tank 208; the third vibrating screen 209 can screen the tertiary slag output from the third magnetic separation belt conveyor 207 into slag powder and slag granules, and the slag powder is stored in the third material tank 210, and the slag granules are stored in the fourth material tank 211;

[0071] The magnetic separation material processing module 300 includes a rod mill 301, a fourth vibrating screen 302, a dry magnetic separator 304 and a second suspended magnetic separator 308; the rod mill 301 can perform rod grinding on the primary magnetic separation material and the secondary magnetic separation material; the fourth vibrating screen 302 can screen the rod mill material output by the rod mill 301 into a rod mill screen upper material and a rod mill screen lower material; the rod mill screen lower material is transported by the first belt conveyor 303, and the dry magnetic separator 304 can magnetically separate the rod mill screen lower material from the first belt conveyor 303. The iron powder is selected and stored in the second iron powder trough 305. The first belt conveyor 303 conveys the remaining slag powder to the slag powder trough 306. The rod mill screen feed is transported by the second belt conveyor 307. The second suspended magnetic separator 308 is arranged above the second belt conveyor 307, and can magnetically select iron blocks from the rod mill screen feed, and the iron blocks are stored in the rod mill iron block trough 309. The second belt conveyor 307 conveys the remaining slag blocks to the rod mill slag block trough 310.

[0072] Compared with the prior art, this application has at least the following beneficial technical effects:

[0073] The present application not only effectively separates the slag and iron of molten iron desulfurization slag, maximizes the recycling value of molten iron desulfurization slag, but also avoids dust, wastewater and air pollution, while also reducing the processing time of molten iron desulfurization slag and improving production efficiency.

[0074] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and substitutions can be made without departing from the technical principles of the present invention. These improvements and substitutions should also be regarded as the scope of protection of the present invention.

Claims

1. A method for treating molten iron desulfurization slag, characterized in that: The steps include: S1: pre-treating the molten iron desulfurization slag by a drum method to obtain a primary treated material; S2: During the transportation process, the primary processed material is subjected to magnetic separation to obtain a primary magnetically separated material and a primary slag material; S3: Screening the primary slag material to obtain primary undersize material and slag block material; S4: During the conveying process, the primary undersize material is subjected to magnetic separation to obtain secondary magnetic separation material and secondary slag material; S5: Screening the secondary slag material to obtain secondary undersize material and slag granules; S6: During the conveying process, the secondary screened material is subjected to magnetic separation to obtain iron powder and tertiary slag; S7: Screening the three slag materials to obtain slag powder and slag granules; S8: performing rod grinding on the primary magnetic separation material and the secondary magnetic separation material to obtain rod grinding material; S9: Screening the rod mill material to obtain rod mill screen upper material and rod mill screen lower material; S10: performing magnetic separation on the rod mill screen material to obtain iron powder and slag powder, and performing magnetic separation on the rod mill screen material to obtain iron block material and slag block material.

2. A method for treating molten iron desulfurization slag according to claim 1, characterized in that: In S2, the primary processed material is conveyed by the first magnetic separation belt conveyor (104), and the primary processed material being conveyed is magnetically separated successively by the first suspended magnetic separator (405) and the first magnetic separation belt conveyor (104).

3. The method for treating molten iron desulfurization slag according to claim 1, characterized in that: In S3, the primary slag material is screened by a first vibrating screen (201) with a screening particle size of 16 mm to obtain primary undersize material of 0 to 16 mm and slag block material of 16 to 300 mm.

4. The method for treating molten iron desulfurization slag according to claim 1, characterized in that: In S5, the secondary slag material is screened by a second vibrating screen (205) with a screening particle size of 8 mm to obtain secondary undersize material of 0 to 8 mm and slag particles of 8 to 16 mm.

5. The method for treating molten iron desulfurization slag according to claim 1, characterized in that: In S7, the tertiary slag material is screened by a third vibrating screen (209) with a screening particle size of 5 mm to obtain slag powder material with a size of 0 to 5 mm and slag granular material with a size of 5 to 8 mm.

6. The method for treating molten iron desulfurization slag according to claim 1, characterized in that: In S9, the rod mill material is screened by a fourth vibrating screen (302) with a screening particle size of 8 mm to obtain rod mill screen undersize of 0 to 8 mm and rod mill screen oversize of 8 to 200 mm.

7. The method for treating molten iron desulfurization slag according to claim 1, characterized in that: In S10, the rod mill screen material is magnetically separated by a dry magnetic separator (304) to obtain iron powder material of 0 to 8 mm and slag powder material of 0 to 8 mm, and the rod mill screen material is magnetically separated by a second hanging magnetic separator (308) to obtain slag iron block material of 8 to 200 mm and slag block material of 8 to 200 mm.

8. A molten iron desulfurization slag treatment system, characterized in that: It comprises a slag-iron separation module (100), a slag material processing module (200) and a magnetic separation material processing module (300); The slag-iron separation module (100) comprises a pretreatment device (102), a feeder (103), a first magnetic separation belt conveyor (104) and a first suspension magnetic separator (105); the pretreatment device (102) is capable of performing a drum process on the molten iron desulfurization slag and obtaining a primary treatment material; the feeder (103) is arranged at the feeding end of the first magnetic separation belt conveyor (104), and the feeder (103) is used to supply the primary treatment material to the first magnetic separation belt conveyor (104); the first suspension magnetic separator (105) is arranged above the first magnetic separation belt conveyor (104), and is capable of magnetically separating the first magnetic separation material from the surface layer of the primary treatment material; the head wheel of the first magnetic separation belt conveyor (104) is a permanent magnet roller, and is capable of magnetically separating the first magnetic separation material from the inside of the primary treatment material; The slag processing module (200) comprises a first vibrating screen (201), a second magnetic separation belt conveyor (203), a second vibrating screen (205), a third magnetic separation belt conveyor (207) and a third vibrating screen (209); the first vibrating screen (201) is capable of screening the primary slag output by the first magnetic separation belt conveyor (104) into primary undersize material and slag block material; the second magnetic separation belt conveyor (203) is arranged between the first vibrating screen (201) and the second vibrating screen (205), and is used to transport the primary undersize material screened by the first vibrating screen (201) to the second vibrating screen (205), and to remove the primary undersize material from the first vibrating screen (201) during the transport process; The magnetically selected material is used to produce the second magnetically selected material from the primary undersize material; the second vibrating screen (205) is capable of screening the secondary slag material outputted from the second magnetic separation belt conveyor (203) into secondary undersize material and slag granules; the third magnetic separation belt conveyor (207) is arranged between the second vibrating screen (205) and the third vibrating screen (209), and is used to transport the secondary undersize material screened by the second vibrating screen (205) to the third vibrating screen (209), and magnetically select iron powder from the secondary undersize material during the transport process; the third vibrating screen (209) is capable of screening the tertiary slag material outputted from the third magnetic separation belt conveyor (207) into slag powder and slag granules; The magnetic material processing module (300) comprises a rod mill (301), a fourth vibrating screen (302), a dry magnetic separator (304) and a second suspended magnetic separator (308); the rod mill (301) is capable of performing rod milling on the primary magnetic material and the secondary magnetic material; the fourth vibrating screen (302) is capable of screening the rod mill material output from the rod mill (301) into rod mill screen upper material and rod mill screen lower material; The dry magnetic separator (304) can magnetically separate iron powder from the rod mill screen under-material; the second suspended magnetic separator (308) can magnetically separate iron block materials from the rod mill screen over-material.