Casting blank low-power non-metallic inclusion control method
By performing heating pretreatment, blowing oxygen, blowing argon, adding deoxidant and alloy elements during the converter steelmaking process, combining the adjustment of the angle of the double breathable brick of the ladle and the parameters of the continuous casting machine, the non-metal inclusions in the casting billet are solved. Many problems have improved the surface quality and composition consistency of the castings.
Patent Information
- Application Number
- CN202410086000.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-22
- Publication Date
- 2024-11-22
AI Technical Summary
During the converter steelmaking process, non-metallic inclusions exist in the casting billet, resulting in defects such as pores and inclusions on the surface of the casting, reducing the surface quality of the casting.
By heating pretreatment, blowing oxygen, blowing argon, adding deoxidant and alloy elements in the converter, sampling and analysis, mechanical slag scraping and other steps, controlling the oxygen content and composition of the molten steel, adjusting the angle of the double breathable brick of the ladle and the insertion depth of the immersion port in the immersion port and continuous casting speed to ensure that the cleanliness and composition of the molten steel meet the requirements.
It effectively reduces the content of non-metallic inclusions in the casting billet, improves product quality, reduces the occurrence of pores and inclusion defects, and improves the cleanliness and composition consistency of the molten steel.
Smart Images

Figure CN118996032A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal processing, in particular to a method for controlling low-magnification non-metallic inclusions in a casting. Background Art
[0002] Converter steelmaking is a complex oxidation process. During the blowing process, oxygen is continuously supplied, which allows oxygen to react with molten steel and refractory materials, causing a certain amount of oxygen to dissolve in the molten steel. The oxygen content of molten steel at the end of blowing is also called the oxidizability of molten steel. The main factors affecting the high oxidizability of molten steel are low C content at the end, high temperature at the end, poor operating process (re-blowing of molten steel), and slag discharge during steel tapping. In order to ensure smooth casting and molten steel quality, the molten steel must be deoxidized. The purpose of deoxidation is to remove excess oxygen in the molten steel to the required range (70-100PPm free oxygen for Q195 steel). The total oxygen in the steel T[O] = [O] dissolved + [O] included. Therefore, the total oxygen can be used T[O] to represent the cleanliness of the molten steel, that is, the level of inclusions in the molten steel. If the total T[O] is low, the molten steel is "clean".
[0003] The inclusions in steel are mainly deoxidation products, secondary oxides, and refractory materials mixed in steel, etc. The non-metallic inclusions in the ingot are mainly distributed in the inner arc of the ingot, which is the characteristic of the arc continuous casting machine. However, when there are many non-metallic inclusions in the ingot, it will cause defects such as pores and inclusions on the surface of the casting, reducing the surface quality of the casting. Summary of the invention
[0004] The object of the present invention is to provide a method for controlling low-magnification non-metallic inclusions in a casting to solve the problems raised in the above-mentioned background technology.
[0005] To achieve the above object, the present invention provides the following technical solution: a method for controlling low-magnification non-metallic inclusions in a casting, the method comprising the following steps:
[0006] Step 1: Filling: put the raw materials such as concentrate, scrap steel, scrap iron, limestone, dolomite, etc. into the converter in a certain proportion;
[0007] Step 2: Heating pretreatment: heating the raw materials in a converter to make them melt. At the same time, injecting a certain amount of oxygen for pretreatment to increase the temperature in the furnace and remove some undesirable impurities.
[0008] Step 3: Blowing oxygen into the converter. After heating pretreatment, close the furnace neck and inject high-purity oxygen through the converter's blast system. The oxygen reacts with carbon, silicon, manganese and other elements in the furnace, oxidizing them to generate gas, which is used to further increase the furnace temperature and increase the carbon content of the molten steel.
[0009] Step 4: Argon blowing. Determine the start and end time of argon blowing and the duration of argon blowing. Argon blowing usually starts after the oxygen injection is completed and lasts until the end of steelmaking. The intensity of argon blowing needs to be adjusted according to the furnace conditions and needs. The intensity of argon blowing can be achieved by controlling the argon blowing pressure, argon flow rate and the layout angle of the double-permeable bricks of the ladle;
[0010] Step 5: Purification of molten steel. The bubbles generated by the oxygen blowing reaction will bring impurities to the furnace surface and form bubble leakage. At the same time, desulfurizers such as limestone are added during the oxygen blowing process to remove sulfur from the molten steel and purify the undesirable impurities in the molten steel.
[0011] Step 6: Add appropriate deoxidizer to reduce the oxygen content in the molten steel, and add appropriate alloying elements to adjust the composition and properties of the molten steel;
[0012] Step 7: Add alloy elements according to product requirements. Appropriate amounts of alloy elements (such as chromium, manganese, nickel, etc.) can be added during the converter smelting process to adjust the composition of the steel.
[0013] Step 8: Sampling and analysis: regularly take samples from the furnace body for chemical composition analysis to ensure that the quality of the molten steel meets the requirements;
[0014] Step 9: Blowing and scraping slag. After the oxygen blowing is completed, close the blast port and use a mechanical scraper to discharge the slag;
[0015] Step 10: Steel tapping. When the smelting is completed, the prepared molten steel is poured from the converter or ladle into the continuous casting mold and continuously cast into billets or slabs through the continuous casting machine.
[0016] Preferably, the detailed operations of step one are as follows: determining the required types and proportions of raw materials according to the steelmaking production plan, the raw materials including concentrate, scrap steel, scrap iron, etc., raw material pretreatment: for recycled materials such as scrap steel and scrap iron, pretreatment is required first, which includes removing dirt and oxides attached to the surface of the scrap steel and scrap iron, and cutting and sorting the scrap steel, etc., weighing raw materials: according to the steelmaking production plan, weighing the prepared raw materials according to a certain proportion, the proportions of raw materials such as concentrate, scrap steel, scrap iron and fluxes such as limestone and dolomite are usually adjusted according to the required composition and properties of the steel.
[0017] Preferably, the detailed operation of the step 2 is: ensure that the inside of the converter is clean, and check whether the door and ventilation system of the converter are working properly, prepare the required fuel, commonly used fuels include coal, natural gas, liquefied petroleum gas, etc., select appropriate fuel according to the type and scale of the converter, inject fuel into the combustion chamber below the converter, and the fuel can enter the combustion chamber through nozzles, pipes, etc., open the fuel supply system, and ignite the fuel. The fuel can be ignited by using an igniter, flame, etc., adjust the fuel supply and oxygen supply in the combustion chamber to ensure stable and efficient combustion, use flame to preheat the converter, spray the flame into the inside of the converter to cover the entire furnace, use flame nozzles and angle adjustment devices to make the flame evenly irradiate various parts of the inside of the converter, and as time goes by, the inside of the converter gradually heats up, adjust the temperature and intensity of the flame to reach the required operating temperature, use thermometers and other equipment to monitor the temperature changes inside the converter to ensure that the converter gradually reaches a suitable operating temperature, and when the converter reaches a suitable operating temperature, stop injecting fuel and close the fuel supply system.
[0018] Preferably, the detailed operation of step three is: injecting high-purity oxygen into the furnace cavity through the blast device of the converter, so that the oxygen reacts with carbon, silicon, manganese and other elements in the furnace to produce an oxidation reaction, and the temperature in the furnace is further increased. During the oxygen blowing process, it is necessary to continuously observe and monitor the temperature in the furnace, the gas generation situation and the changes in the chemical element content in the furnace. According to production needs, an appropriate amount of oxygen is continuously injected to ensure that the temperature and carbon content in the furnace are further increased. After the oxygen blowing is completed, the end time of the oxygen blowing is determined according to the required molten steel temperature and carbon content. Generally, the oxygen injection is stopped after the set indicators are reached.
[0019] Preferably, the adjustment and control of argon blowing in step 4 is carried out in accordance with "strong-medium-weak" to ensure the soft argon blowing effect, which is achieved by automatically setting the argon blowing flow rate and time of each stage. At the same time, the angle of the double air-permeable bricks of the ladle is changed to 120°, and the position is changed from non-equal diameter to equal diameter.
[0020] Preferably, the suitable deoxidizer added in step six is steel core aluminum. The steel core aluminum generally exists in the form of wire or block and is sealed with packaging materials to prevent air oxidation. The packaging materials can be aluminum foil, plastic film, etc. Before the converter is put into the furnace, the mouth of the converter bag covering material is opened, and the accurately weighed steel core aluminum blocks or wires are evenly placed in the bag, and then, the mouth of the bag covering material is sealed to ensure the sealing of the inside of the converter. The steel core aluminum melts rapidly at high temperature, and the oxides in the molten steel react to reduce the oxygen content in the steel.
[0021] Preferably, the detailed operation of step 7 is: open the feed port of the converter, add the raw material of the alloy element into the converter in the charge feeding area above the scrap steel and iron ore. The alloy element may be chromium, nickel, manganese, etc., and evenly spread the raw material of the alloy element above the scrap steel and iron ore to ensure that the alloy raw material is fully in contact with the scrap steel and iron ore, and close the feed port of the converter to ensure that the atmosphere in the converter remains closed.
[0022] Preferably, the detailed operations of step eight are: determine the number and location of samples to be extracted, use appropriate tools to take the samples out of the converter to ensure the representativeness of the samples, grind the samples into powder and mix them evenly to ensure the representativeness during sampling, select appropriate analysis methods such as spectral analysis, chemical analysis, etc. according to different components, record the measurement results and perform data processing, analyze the measurement results, and compare them with the specified steel quality requirements.
[0023] Preferably, the detailed operation of step nine is: close the blast port of the converter through the operating control system, stop injecting air into the furnace, prepare the mechanical scraper to ensure its normal operation, the mechanical scraper is usually composed of a scraper and a scraping mechanism, start the mechanical scraper, control the movement of the scraper to scrape off the oxidized slag along the converter wall, and at the same time, the scraping mechanism pushes the scraped slag blocks out of the converter for transportation and processing.
[0024] Preferably, in the step 10, the insertion depth of the submerged nozzle of the continuous casting machine is 80-100 mm, the erosion amount of the nozzle diameter is not more than 40 mm, the thickness of the crystallizer slag layer is 40-50 mm, and the continuous casting speed is controlled at 2.5 m / min.
[0025] Compared with the prior art, the present invention provides a method for controlling low-magnification non-metallic inclusions in a casting, which has the following beneficial effects:
[0026] 1. The method for controlling low-magnification non-metallic inclusions in the ingot is to judge the combustion state in the furnace by observing the shape, color and lighting degree of the furnace wall in the converter, and to adjust the converter bottom blowing volume in time according to the height, brightness and color of the flame, so as to increase the C content of the Q195 endpoint, reduce the oxidizability of the molten steel, and reduce the low-magnification inclusions in the ingot.
[0027] 2. The method for controlling low-magnification non-metallic inclusions in the ingot can improve the distribution of bottom-blown gas in molten steel and enhance the floating effect of inclusions by adjusting the angle of the double-permeable bricks in the ladle, thereby reducing the inclusion content in the ingot and improving product quality.
[0028] 3. The method for controlling low-magnification non-metallic inclusions in the ingot reduces the content of low-magnification non-metallic inclusions in the ingot by adjusting the insertion depth of the immersion nozzle, the erosion amount of the nozzle diameter and the thickness of the slag layer of the crystallizer, as well as controlling the continuous casting speed. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a schematic diagram of the process of the present invention. DETAILED DESCRIPTION
[0030] like Figure 1 As shown, the present invention provides a technical solution: a method for controlling low-magnification non-metallic inclusions in a casting, the method for controlling low-magnification non-metallic inclusions in a casting comprises the following steps:
[0031] Step 1: Filling: put the raw materials such as concentrate, scrap steel, scrap iron, limestone, dolomite, etc. into the converter in a certain proportion;
[0032] Step 2: Heating pretreatment: heating the raw materials in a converter to make them melt. At the same time, injecting a certain amount of oxygen for pretreatment to increase the temperature in the furnace and remove some undesirable impurities.
[0033] Step 3: Blowing oxygen into the converter. After heating pretreatment, close the furnace neck and inject high-purity oxygen through the converter's blast system. The oxygen reacts with carbon, silicon, manganese and other elements in the furnace, oxidizing them to generate gas, which is used to further increase the furnace temperature and increase the carbon content of the molten steel.
[0034] Step 4: Argon blowing. Determine the start and end time of argon blowing and the duration of argon blowing. Argon blowing usually starts after the oxygen injection is completed and lasts until the end of steelmaking. The intensity of argon blowing needs to be adjusted according to the furnace conditions and needs. The intensity of argon blowing can be achieved by controlling the argon blowing pressure, argon flow rate and the layout angle of the double-permeable bricks of the ladle;
[0035] Step 5: Purification of molten steel. The bubbles generated by the oxygen blowing reaction will bring impurities to the furnace surface and form bubble leakage. At the same time, desulfurizers such as limestone are added during the oxygen blowing process to remove sulfur from the molten steel and purify the undesirable impurities in the molten steel.
[0036] Step 6: Add appropriate deoxidizer to reduce the oxygen content in the molten steel, and add appropriate alloying elements to adjust the composition and properties of the molten steel;
[0037] Step 7: Add alloy elements according to product requirements. Appropriate amounts of alloy elements (such as chromium, manganese, nickel, etc.) can be added during the converter smelting process to adjust the composition of the steel.
[0038] Step 8: Sampling and analysis: regularly take samples from the furnace body for chemical composition analysis to ensure that the quality of the molten steel meets the requirements;
[0039] Step 9: Blowing and scraping slag. After the oxygen blowing is completed, close the blast port and use a mechanical scraper to discharge the slag;
[0040] Step 10: Steel tapping. When the smelting is completed, the prepared molten steel is poured from the converter or ladle into the continuous casting mold and continuously cast into billets or slabs through the continuous casting machine.
[0041] The detailed operations of step one are as follows: determine the types and proportions of raw materials required according to the steelmaking production plan. The raw materials include concentrate, scrap steel, scrap iron, etc. Raw material pretreatment: For recycled materials such as scrap steel and scrap iron, pretreatment is required first, which includes removing dirt and oxides attached to the surface of scrap steel and scrap iron, as well as cutting and sorting the scrap steel. Weigh raw materials: According to the steelmaking production plan, weigh the prepared raw materials in a certain proportion. The proportions of raw materials such as concentrate, scrap steel, scrap iron and fluxes such as limestone and dolomite are usually adjusted according to the required composition and properties of the steel.
[0042] The detailed operations of step two are: ensure that the inside of the converter is clean, and check whether the door and ventilation system of the converter are working properly, prepare the required fuel, commonly used fuels are coal, natural gas, liquefied petroleum gas, etc., select appropriate fuel according to the type and scale of the converter, inject fuel into the combustion chamber below the converter, and the fuel can enter the combustion chamber through nozzles, pipes, etc., open the fuel supply system and ignite the fuel. The fuel can be ignited by using igniters, flames, etc., adjust the fuel supply and oxygen supply in the combustion chamber to ensure stable and efficient combustion, use flames to preheat the converter, spray the flame into the inside of the converter, covering the entire furnace, can use flame nozzles and angle adjustment devices to make the flame evenly irradiate various parts of the inside of the converter, as time goes by, the inside of the converter gradually heats up, adjust the temperature and intensity of the flame to reach the required operating temperature, use thermometers and other equipment to monitor the temperature changes inside the converter to ensure that the converter gradually reaches a suitable operating temperature, when the converter reaches a suitable operating temperature, stop injecting fuel and close the fuel supply system.
[0043] The detailed operation of step three is: inject high-purity oxygen into the furnace cavity through the blast device of the converter, so that the oxygen reacts with carbon, silicon, manganese and other elements in the furnace to produce an oxidation reaction, and the temperature in the furnace is further increased. During the oxygen blowing process, it is necessary to continuously observe and monitor the temperature in the furnace, the gas generation and the changes in the chemical element content in the furnace. According to production needs, a proper amount of oxygen is continuously injected to ensure that the temperature and carbon content in the furnace are further increased. After the oxygen blowing is completed, the end time of the oxygen blowing is determined according to the required molten steel temperature and carbon content. Generally, after the set indicators are reached, the oxygen injection is stopped, and the shape, color and illumination degree of the furnace wall of the converter are observed to judge the combustion state in the furnace. The height, brightness and color of the flame are used to adjust the converter bottom blowing volume in time to increase the Q195 endpoint C content and reduce the oxidizability of the molten steel. The height, brightness and color of the flame can reflect the combustion state in the furnace. The height of the furnace fire mainly reflects the intensity of combustion. A high flame indicates strong combustion, while a low flame indicates weak combustion. The brightness of the flame mainly reflects the degree of completeness of combustion. A bright flame indicates complete combustion, while a dim flame indicates incomplete combustion. The color of the flame mainly reflects the stability of combustion. A blue flame indicates stable combustion, while a yellow or red flame indicates unstable combustion. By observing these indicators, the combustion state in the furnace can be judged. If the flame is high, bright, and blue, it means that the combustion intensity is moderate, and the combustion is complete and stable. At this time, the air blowing volume at the bottom of the converter can be appropriately reduced to reduce the amount of oxygen entering the furnace and reduce the oxidizability of the molten steel, thereby reducing the formation of low-multiple inclusions in the ingot. On the contrary, if the flame is low, dim, and yellow or red, it means that the combustion is incomplete or unstable. At this time, it is necessary to increase the air blowing volume at the bottom of the converter, increase the oxygen supply, and improve the intensity and completeness of the combustion to reduce the reducibility of the molten steel and reduce the formation of inclusions.
[0044] According to the data, the Q195 endpoint C < 0.035% accounted for 9.33% from June to August 2022, while the Q195 endpoint C < 0.035% accounted for 4.86% from September 2022 to February 2023 after the operator strictly controlled the oxygen supply flow through flame judgment, which was 4.47% lower than before.
[0045] The adjustment and control of argon blowing in step 4 is carried out according to "strong-medium-weak" to ensure the soft argon blowing effect, which is achieved by automatically setting the argon blowing flow and time of each stage. Argon blowing is to control the oxygen content of molten steel by injecting argon into the molten steel to reduce the formation of non-metallic inclusions. The "strong-medium-weak" argon blowing method is adopted, that is, the argon flow rate is large at the beginning and then gradually decreases. The purpose of doing this is to consider two aspects: first, the argon flow rate is large at the beginning of argon blowing, which can quickly flush out the oxygen in the molten steel, so that the oxygen content is rapidly reduced, thereby reducing the formation of non-metallic inclusions. Secondly, the argon flow rate gradually decreases in the middle and late stages of argon blowing, which can avoid excessive stirring of molten steel caused by excessive argon blowing, reduce further contamination of slag, and thus reduce the generation of non-metallic inclusions. At the same time, the angle of the double-permeable bricks of the ladle is changed to 120°, and the position is changed from the original non-equal diameter to equal diameter. The original double-permeable brick arrangement angle of the ladle is 900 (provided by the water model test of Chongqing University), and the original ladle diameter is (bottom 2306mm / upper mouth 2635mm); the diameter of the 120-ton ladle after overhaul is (2486mm / 2876mm). There will be dead corners when blowing argon at the bottom, resulting in some inclusions not being able to float up well. Through low-power analysis of the billet, after adjusting the angle of the double-permeable bricks of the ladle, the low-power inclusions of the billet are significantly reduced; the adjustment of the arrangement angle of the double-permeable bricks of the ladle can improve the airflow distribution when blowing at the bottom of the ladle, reduce the existence of dead corners, and thus reduce inclusions in the billet. In the case where the original ladle diameter and the ladle diameter after overhaul are different, it may be necessary to re-evaluate and adjust the arrangement angle of the double-permeable bricks. Adjusting the layout angle of the double-permeable bricks can change the flow direction and speed of the bottom-blowing gas, thereby optimizing the distribution of the bottom airflow. The inclusion content in the molten steel can be evaluated through the low-magnification analysis of the ingot. If the low-magnification inclusions in the ingot are significantly reduced after adjusting the angle of the double-permeable bricks, it means that the adjusted bottom-blowing airflow can better promote the floating of inclusions and reduce the possibility of them remaining in the ingot. Therefore, by adjusting the angle of the double-permeable bricks in the ladle, the distribution of the bottom-blowing gas in the molten steel can be improved, the floating effect of inclusions can be improved, thereby reducing the inclusion content in the ingot and improving product quality.
[0046] In step six, the appropriate deoxidizer added is steel core aluminum. Steel core aluminum generally exists in the form of wire or block and is sealed with packaging materials to prevent air oxidation. The packaging materials can be aluminum foil, plastic film, etc. Before the converter enters the furnace, the mouth of the converter bag covering material is opened, and the accurately weighed steel core aluminum blocks or wires are evenly placed in the bag, and then, the mouth of the bag covering material is sealed to ensure the sealing of the inside of the converter. The steel core aluminum melts rapidly at high temperature, and the oxides in the molten steel react to reduce the oxygen content in the steel.
[0047] The detailed operation of step seven is: open the feed port of the converter, add the raw materials of alloy elements into the converter in the charge feeding area above the scrap steel and iron ore. The alloy elements can be chromium, nickel, manganese, etc., and evenly spread the raw materials of alloy elements above the scrap steel and iron ore to ensure that the alloy raw materials are fully in contact with the scrap steel and iron ore, and close the feed port of the converter to ensure that the atmosphere in the converter remains closed.
[0048] The detailed operations of step eight are: determine the number and location of samples to be extracted, use appropriate tools to take samples out of the converter to ensure the representativeness of the samples, grind the samples into powder and mix them evenly to ensure the representativeness during sampling, select appropriate analysis methods according to different components, such as spectral analysis, chemical analysis, etc., record the measurement results and perform data processing, analyze the measurement results, and compare them with the specified steel quality requirements.
[0049] The detailed operation of step nine is: close the blast port of the converter through the operating control system, stop injecting air into the furnace, prepare the mechanical scraper to ensure its normal operation. The mechanical scraper is usually composed of a scraper and a scraping mechanism. Start the mechanical scraper and control the movement of the scraper to scrape off the oxidized slag along the wall of the converter. At the same time, the scraping mechanism pushes the scraped slag blocks out of the converter for transportation and treatment.
[0050] In step 10, the insertion depth of the immersion nozzle of the continuous casting machine is 80-100mm, the erosion amount of the nozzle diameter is no more than 40mm, the thickness of the crystallizer slag layer is 40-50mm, and the continuous casting speed is controlled at 2.5m / min. The adjustment of the insertion depth of the immersion nozzle, the erosion amount of the nozzle diameter and the thickness of the crystallizer slag layer, as well as the control of the continuous casting speed, are all to reduce the content of low-multiple non-metallic inclusions in the ingot. The following are the specific principles and functions:
[0051] Adjust the insertion depth of the submerged nozzle and the amount of nozzle diameter erosion: The shallow insertion depth of the submerged nozzle can reduce the contact time between the molten steel and the nozzle, reducing the possibility of oxidation reaction and the formation of non-metallic inclusions. Controlling the amount of nozzle diameter erosion, that is, the diameter of the nozzle becomes smaller as the use time increases, can ensure the smooth flow of molten steel, reduce the time the molten steel stays in the nozzle, and reduce oxidation and the formation of inclusions.
[0052] Adjust the thickness of the mold slag layer: The main function of the mold slag layer is to prevent the molten steel from directly contacting the mold wall, reducing oxidation reactions and the formation of non-metallic inclusions. Increasing the thickness of the slag layer can increase the isolation distance between the molten steel and the mold, and reduce the possibility of inclusions entering the steel.
[0053] Control the continuous casting speed: Too high a continuous casting speed will cause shearing of the molten steel, increase the speed of the oxidation reaction, and also cause flow disturbance, making it easier for inclusions to enter the steel. Reducing the pulling speed can reduce the shearing and flow disturbance of the molten steel, reduce the oxidation reaction and the formation of inclusions. In summary, adjusting the insertion depth of the submerged nozzle, the amount of nozzle diameter erosion, and the thickness of the crystallizer slag layer, as well as controlling the continuous casting speed, are all aimed at reducing the contact time and shearing of the molten steel with the environment, reducing the possibility of oxidation reaction and the formation of non-metallic inclusions, and thus reducing the content of low-multiple non-metallic inclusions in the ingot.
[0054] The above generally describes the present invention in detail, but it is obvious to a person skilled in the art that some modifications or improvements can be made to the present invention. Therefore, modifications or improvements that do not depart from the spirit of the present invention are within the scope of protection of the present invention.
Claims
1. A method for controlling low-magnification non-metallic inclusions in a casting, characterized by: The method for controlling low-magnification non-metallic inclusions in a casting slab comprises the following steps: Step 1: Filling: put the raw materials such as concentrate, scrap steel, scrap iron, limestone, dolomite, etc. into the converter in a certain proportion; Step 2: Heating pretreatment, heating the raw materials in a converter to make them melt, and at the same time, injecting a certain amount of oxygen for pretreatment to increase the temperature in the furnace and remove some undesirable impurities; Step 3: Blowing oxygen into the converter. After heating pretreatment, close the furnace neck and inject high-purity oxygen through the converter's blast system. The oxygen reacts with carbon, silicon, manganese and other elements in the furnace to oxidize them into gas. Step 4: Argon blowing. Determine the start and end time of argon blowing and the duration of argon blowing. Argon blowing usually starts after the oxygen injection is completed and lasts until the end of steelmaking. The intensity of argon blowing needs to be adjusted according to the furnace conditions and needs. The intensity of argon blowing can be achieved by controlling the argon blowing pressure, argon flow rate and the layout angle of the double-permeable bricks of the ladle; Step 5: Purification of molten steel. The bubbles generated by the oxygen blowing reaction will bring impurities to the furnace surface and form bubble leakage. At the same time, desulfurization agents such as limestone are added during the oxygen blowing process. Step 6: Add appropriate deoxidizer to reduce the oxygen content in the molten steel and add appropriate alloying elements; Step 7: Add alloy elements according to product requirements. Appropriate amounts of alloy elements (such as chromium, manganese, nickel, etc.) can be added during the converter smelting process. Step 8: Sampling and analysis: regularly take samples from the furnace body for chemical composition analysis; Step 9: After blowing the hair and scraping the slag, and after the oxygen blowing is finished, close the blast port; Step 10: Steel tapping. When the smelting is completed, the prepared molten steel is poured from the converter or ladle into the continuous casting mold and continuously cast into billets or slabs through the continuous casting machine.
2. A method for controlling low-magnification non-metallic inclusions in a casting according to claim 1, characterized in that: The detailed operation of the step one is as follows: determine the required raw material types and proportions according to the steelmaking production plan, the raw materials include concentrate, scrap steel, scrap iron, etc., raw material pretreatment: for recycled materials such as scrap steel and scrap iron, pretreatment is required first, which includes removing dirt and oxides attached to the surface of scrap steel and scrap iron, as well as cutting and sorting the scrap steel, etc., weighing raw materials: according to the steelmaking production plan, weigh the prepared raw materials according to a certain proportion, and the proportions of raw materials such as concentrate, scrap steel, scrap iron and fluxes such as limestone and dolomite are usually adjusted according to the required composition and properties of the steel.
3. The method for controlling low-magnification non-metallic inclusions in a casting according to claim 1, characterized in that: The detailed operations of the step two are: ensure that the inside of the converter is clean, and check whether the door and ventilation system of the converter are working properly, prepare the required fuel, commonly used fuels include coal, natural gas, liquefied petroleum gas, etc., select appropriate fuel according to the type and scale of the converter, inject fuel into the combustion chamber below the converter, and the fuel can enter the combustion chamber through nozzles, pipes, etc., open the fuel supply system and ignite the fuel, and the fuel can be ignited by using igniters, flames, etc., adjust the fuel supply and oxygen supply in the combustion chamber to ensure stable and efficient combustion, use flames to preheat the converter, and spray the flame into the inside of the converter to cover the entire furnace, and use flame nozzles and angle adjustment devices to make the flame evenly irradiate various parts of the inside of the converter. As time goes by, the inside of the converter gradually heats up, adjust the temperature and intensity of the flame to reach the required operating temperature, use thermometers and other equipment to monitor the temperature changes inside the converter, and when the converter reaches a suitable operating temperature, stop injecting fuel and close the fuel supply system.
4. The method for controlling low-magnification non-metallic inclusions in a casting according to claim 1, characterized in that: The detailed operation of step three is: injecting high-purity oxygen into the furnace cavity through the blast device of the converter, so that the oxygen reacts with carbon, silicon, manganese and other elements in the furnace to produce an oxidation reaction, and the temperature in the furnace is further increased. During the oxygen blowing process, it is necessary to continuously observe and monitor the temperature in the furnace, the gas generation and the changes in the chemical element content in the furnace. According to production needs, a proper amount of oxygen is continuously injected to ensure that the temperature and carbon content in the furnace are further increased. After the oxygen blowing is completed, the end time of the oxygen blowing is determined according to the required molten steel temperature and carbon content. Generally, the oxygen injection is stopped after the set indicators are reached.
5. The method for controlling low-magnification non-metallic inclusions in a casting according to claim 1, characterized in that: The adjustment and control of argon blowing in step 4 is carried out in accordance with "strong-medium-weak" to ensure the soft argon blowing effect, which is achieved by automatically setting the argon blowing flow rate and time of each stage. At the same time, the angle of the double air-permeable brick of the ladle is changed to 120°, and the position is changed from non-equal diameter to equal diameter.
6. The method for controlling low-magnification non-metallic inclusions in a casting according to claim 1, characterized in that: The appropriate deoxidizer added in step six is steel core aluminum. The steel core aluminum generally exists in the form of wire or block and is sealed with packaging materials to prevent air oxidation. The packaging materials can be aluminum foil, plastic film, etc. Before the converter is put into the furnace, the mouth of the converter bag covering material is opened, and the accurately weighed steel core aluminum blocks or wires are evenly placed in the bag, and then the mouth of the bag covering material is sealed to ensure the sealing of the inside of the converter. The steel core aluminum melts rapidly at high temperature, and the oxides in the molten steel react to reduce the oxygen content in the steel.
7. The method for controlling low-magnification non-metallic inclusions in a casting according to claim 1, characterized in that: The detailed operation of step seven is: open the feed port of the converter, add raw materials of alloy elements into the converter in the charge feeding area above the scrap steel and iron ore, the alloy elements may be chromium, nickel, manganese, etc., and evenly sprinkle the raw materials of alloy elements above the scrap steel and iron ore to ensure that the alloy raw materials are in full contact with the scrap steel and iron ore, close the feed port of the converter, and ensure that the atmosphere in the converter remains closed.
8. The method for controlling low-magnification non-metallic inclusions in a casting according to claim 1, characterized in that: The detailed operations of step eight are: determine the number and location of samples to be extracted, use appropriate tools to take samples out of the converter to ensure the representativeness of the samples, grind the samples into powder and mix them evenly to ensure the representativeness during sampling, select appropriate analysis methods such as spectral analysis, chemical analysis, etc. according to different components, record the measurement results and perform data processing, analyze the measurement results, and compare them with the specified steel quality requirements.
9. The method for controlling low-magnification non-metallic inclusions in a casting according to claim 1, characterized in that: The detailed operation of step nine is: close the blast port of the converter through the operating control system, stop injecting air into the furnace, prepare the mechanical scraper to ensure its normal operation. The mechanical scraper is usually composed of a scraper and a scraping mechanism. Start the mechanical scraper and control the movement of the scraper to scrape off the oxidized slag along the wall of the converter. At the same time, the scraping mechanism pushes the scraped slag blocks out of the converter for transportation and treatment.
10. The method for controlling low-magnification non-metallic inclusions in a casting according to claim 1, characterized in that: In the step 10, the insertion depth of the submerged nozzle of the continuous casting machine is 80-100 mm, the erosion amount of the nozzle diameter is not more than 40 mm, the thickness of the crystallizer slag layer is 40-50 mm, and the continuous casting speed is controlled at 2.5 m / min.