Method for reducing total iron content of converter final slag

By adjusting the proportion of scrap steel and iron ore, enhancing the melt pool stirring and adjusting the oxidation reaction, the problem of high iron content in the final slag of the converter is solved, and the effect of reducing steel material consumption and production costs is achieved.

CN118996033APending Publication Date: 2024-11-22SHANXI ZHONGYANG IRON & STEEL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410084497.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-01-19
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The high iron content of the converter final slag leads to waste of steel materials and an increase in production costs, affecting the yield of molten steel.

Method used

By adjusting the ratio of scrap steel and iron ore in the converter, blowing high-pressure gas in high-pressure gas with a high-pressure air gun to enhance molten pool stirring, reducing the process gun position and extending the end-point gun pressing time, increasing the oxidation reaction, and adjusting by observing the furnace fire morphology and color Oxygen supply to reduce the total iron content of the final slag.

Benefits of technology

It effectively reduces the total iron content of the final slag of the converter, improves the yield of molten steel, and reduces the consumption and production costs of steel materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004674238560000011
    Figure HDA0004674238560000011
Patent Text Reader

Abstract

The invention relates to the technical field of metallurgical engineering, and discloses a method for reducing the total iron content of converter final slag, and the method comprises the following steps: step 1, preparation: preparing scrap steel and iron ore according to a certain proportion, and loading the prepared scrap steel and iron ore into a converter; secondly, preheating is conducted, fuel is injected into the converter, preheating is conducted through flames, and the converter reaches the proper working temperature; 3, blowing: blowing high-pressure gas into the bottom of the converter through a high-pressure gas gun; 4, TSC temperature measurement sampling is carried out, and when 70%-80% of the to-be-supplied oxygen amount is achieved in the converter smelting process, TSC temperature measurement sampling is carried out; and 5, supplying oxygen, and adding a proper amount of lime and other desulfurizers. According to the method for reducing the total iron content of the final slag of the converter, the slag-gold reaction is more sufficient, the reaction in the converter is close to balance and the reaction of molten steel C in the molten pool and the total iron in the slag is more complete by increasing the bottom blowing gas amount and enhancing stirring of the molten pool, so that the total iron in the slag is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metallurgical engineering, in particular to a method for reducing the total iron content of converter final slag. Background Art

[0002] For most steel mills, the higher the total iron content of converter slag, the greater the waste of steel materials, leading to increased production costs. How to reduce the iron content of converter slag so that it can enter the molten steel and thus reduce steel material consumption is an issue that steelmakers have been paying attention to and studying.

[0003] Steel material consumption is an important economic indicator to measure the production, technology and management level of a steel plant, and the molten steel recovery rate is one of the important factors affecting steel material consumption. In the converter smelting process, the total iron content of the converter final slag directly affects the molten steel recovery rate at the converter end. The higher the total iron content of the final slag, the lower the molten steel recovery rate; conversely, the higher the molten steel recovery rate. Summary of the invention

[0004] The object of the present invention is to provide a method for reducing the total iron content of converter final slag to solve the problems raised in the above background technology.

[0005] To achieve the above object, the present invention provides the following technical solution: a method for reducing the total iron content of converter final slag, the method comprising the following steps:

[0006] Step 1: Preparation: prepare the scrap steel and iron ore in a certain proportion and load them into the converter;

[0007] Step 2: Preheating: inject fuel into the converter and use flame to preheat the converter to a suitable operating temperature;

[0008] Step 3: Blowing: Blow high-pressure gas into the bottom of the converter through a high-pressure air gun;

[0009] Step 4: TSC temperature measurement and sampling. When the amount of oxygen to be supplied reaches 70%-80% during the converter smelting process, TSC temperature measurement and sampling is performed;

[0010] Step 5: Supply oxygen and add appropriate amount of lime and other desulfurizers to reduce the sulfur content in the molten steel to a reasonable range;

[0011] Step 6: Blending alloys: according to the needs, some alloy elements such as chromium, nickel, manganese, etc. are added in the converter to improve the properties of the steel;

[0012] Step 7: Temperature control: According to the smelting requirements, the temperature in the converter is controlled to ensure the reaction in the furnace and the quality of the molten steel;

[0013] Step 8: Determine the composition. Take samples from the converter regularly for composition analysis to ensure that the quality of the steel meets the requirements.

[0014] Step nine: Out of the furnace. When the smelting time is reached or meets the requirements, the molten steel is poured out of the furnace and enters the continuous casting machine for molding.

[0015] Preferably, the detailed operation of step 1 is: according to the required alloy formula, determine the ratio of scrap steel and iron ore. According to different requirements, the ratio of scrap steel and iron ore can be adjusted to obtain the required alloy composition. Prepare the required scrap steel and iron ore. The scrap steel can be from waste machinery and equipment, waste building materials, etc., and the iron ore can be raw materials mined from mines. Close the door of the converter to ensure that the converter is sealed.

[0016] Preferably, the detailed operation of the step 2 is: ensure that the inside of the converter is clean, and check whether the door and ventilation system of the converter are working properly, prepare the required fuel, commonly used fuels include coal, natural gas, liquefied petroleum gas, etc., select appropriate fuel according to the type and scale of the converter, inject fuel into the combustion chamber below the converter, and the fuel can enter the combustion chamber through nozzles, pipes, etc., open the fuel supply system, and ignite the fuel. The fuel can be ignited by using an igniter, flame, etc., adjust the fuel supply and oxygen supply in the combustion chamber to ensure stable and efficient combustion, use flame to preheat the converter, spray the flame into the inside of the converter to cover the entire furnace, use flame nozzles and angle adjustment devices to make the flame evenly irradiate various parts of the inside of the converter, and as time goes by, the inside of the converter gradually heats up, adjust the temperature and intensity of the flame to reach the required operating temperature, use thermometers and other equipment to monitor the temperature changes inside the converter to ensure that the converter gradually reaches a suitable operating temperature, and when the converter reaches a suitable operating temperature, stop injecting fuel and close the fuel supply system.

[0017] Preferably, the detailed operation of step three is as follows: when the steel grade is Q195, argon is used as the high-pressure gas, the gas flow rate is 0.036Nm3 / min, the gun position is adjusted to 1350-1500mm, and the gun pressing time is 80 seconds; when the steel grade is HRB400, the gas flow rate is 0.036Nm3 / min, the gun position is adjusted to 1450-1600mm, and the gun pressing time is 40 seconds; the parameters of the oxygen gun copper head are optimized, and the nozzle angle is adjusted to 12.15°-12.5°; the throat diameter is adjusted to 34.6mm-33.5mm, and the stirring of the molten pool is enhanced by increasing the bottom blowing volume, so that the slag-metal reaction is more sufficient, the reaction in the furnace is close to equilibrium, and the molten steel C in the molten pool reacts more completely with the total iron in the slag, so that the total iron in the slag is reduced, and lowering the process gun position and extending the terminal gun pressing time can increase the oxidation reaction in the furnace, increase the iron oxide content in the slag, and thus reduce the total iron content in the final slag.

[0018] Preferably, the detailed operation of step four is: when the oxygen supply reaches 70%-80% during the converter smelting process, TSC temperature measurement and sampling is performed. Before performing this step, in order to ensure the accuracy of temperature measurement and sampling and prevent interference between the oxygen lance and the sampling cup, the oxygen lance needs to be lowered. This lowering process is carried out in two stages, namely, the oxygen lance is gradually lowered to the position of the carbon pulling lance. The carbon pulling lance position is a nozzle in the converter, which is mainly used for spraying pure carbon or reducing agent, and is used to reduce the oxygen content in the molten steel and adjust the composition of the molten steel. By lowering the oxygen lance to the carbon pulling lance position, it can be ensured that during TSC temperature measurement and sampling, the oxygen lance will not interfere with the temperature of the molten steel in the sampling cup. In this way, the temperature information of the molten steel can be obtained more accurately, providing accurate data basis for the control and regulation of the smelting process.

[0019] Preferably, the detailed operation of step five is: determine the amount of lime and desulfurizer to be used according to the weight of the molten steel and the sulfur content target, and at the same time, ensure that the oxygen supply is sufficient and conduct safety checks, gradually add lime to the molten steel, the addition of lime can be controlled by a feeding device to ensure uniform addition and does not cause sputtering or splashing, calculate the amount of desulfurizer, gradually add desulfurizer to the molten steel, the desulfurizer can be a calcium-aluminum composite desulfurizer, a silicon-aluminum composite desulfurizer, etc., ensure that the desulfurizer is added evenly and avoid violent reactions, stir the molten steel, and the lime and other desulfurizers are in full contact with the molten steel to improve the desulfurization effect. The stirring time is generally a few minutes to more than ten minutes.

[0020] Preferably, the detailed operation of step 6 is: open the feed port of the converter, add the raw material of the alloy element into the converter in the charge feeding area above the scrap steel and iron ore. The alloy element may be chromium, nickel, manganese, etc., and evenly spread the raw material of the alloy element above the scrap steel and iron ore to ensure that the alloy raw material is fully in contact with the scrap steel and iron ore, and close the feed port of the converter to ensure that the atmosphere in the converter remains in a closed state.

[0021] Preferably, the detailed operation of step seven is: during the operation of the converter, use a temperature probe or an infrared thermometer and other equipment to regularly monitor the temperature inside the furnace. Temperature probes can be set on the top, side or bottom of the converter to obtain temperature data at different positions. When the temperature needs to be lowered, an appropriate amount of coolant can be added to lower the temperature inside the converter. Commonly used coolants include molten iron, scrap steel, waste bricks, etc.

[0022] Preferably, the detailed operations of step eight are: determine the number and location of samples to be extracted, use appropriate tools to take the samples out of the converter to ensure the representativeness of the samples, grind the samples into powder and mix them evenly to ensure the representativeness during sampling, select appropriate analysis methods such as spectral analysis, chemical analysis, etc. according to different components, record the measurement results and perform data processing, analyze the measurement results, and compare them with the specified steel quality requirements.

[0023] Preferably, the oxygen supply in step 5 requires the operator to judge the required flow rate of oxygen supply through the flame to increase the carbon content of molten steel, and to judge the combustion state in the furnace by observing the shape, color and lighting degree of the furnace wall of the converter. The height, brightness and color of the flame are used to timely adjust the bottom blowing volume of the converter, so that the carbon content of the molten steel is increased, thereby reducing the total iron content in the final slag.

[0024] Compared with the prior art, the present invention provides a method for reducing the total iron content of converter final slag, which has the following beneficial effects:

[0025] 1. The method for reducing the total iron content in the final slag of the converter increases the bottom blowing volume to enhance the stirring of the molten pool, so that the slag-metal reaction is more complete, the reaction in the furnace is close to equilibrium, and the molten steel C in the molten pool reacts more completely with the total iron in the slag, so that the total iron in the slag can be reduced.

[0026] 2. The method for reducing the total iron content of the converter final slag, lowering the process gun position and extending the terminal gun pressure time can increase the oxidation reaction in the furnace, increase the iron oxide content in the slag, and thus reduce the total iron content in the final slag.

[0027] 3. The method of reducing the total iron content in the final converter slag is to judge the combustion state in the converter by observing the shape, color and lighting degree of the furnace wall in the converter. The converter bottom blowing volume is adjusted in time according to the height, brightness and color of the flame, so that the carbon content of the molten steel is increased, thereby reducing the total iron content in the final slag. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a schematic diagram of the process of the present invention. DETAILED DESCRIPTION

[0029] like Figure 1 As shown, the present invention provides a technical solution: a method for reducing the total iron content of converter final slag, the method comprises the following steps:

[0030] Step 1: Preparation: prepare the scrap steel and iron ore in a certain proportion and load them into the converter;

[0031] Step 2: Preheating: inject fuel into the converter and use flame to preheat the converter to a suitable operating temperature;

[0032] Step 3: Blowing: Blow high-pressure gas into the bottom of the converter through a high-pressure air gun;

[0033] Step 4: TSC temperature measurement and sampling. When the amount of oxygen to be supplied reaches 70%-80% during the converter smelting process, TSC temperature measurement and sampling is performed;

[0034] Step 5: Supply oxygen and add appropriate amount of lime and other desulfurizers to reduce the sulfur content in the molten steel to a reasonable range;

[0035] Step 6: Blending alloys: according to the needs, some alloy elements such as chromium, nickel, manganese, etc. are added in the converter to improve the properties of the steel;

[0036] Step 7: Temperature control: According to the smelting requirements, the temperature in the converter is controlled to ensure the reaction in the furnace and the quality of the molten steel;

[0037] Step 8: Determine the composition. Take samples from the converter regularly for composition analysis to ensure that the quality of the steel meets the requirements.

[0038] Step nine: Out of the furnace. When the smelting time is reached or meets the requirements, the molten steel is poured out of the furnace and enters the continuous casting machine for molding.

[0039] The detailed operation of step 1 is: Determine the ratio of scrap steel and iron ore according to the required alloy formula. According to different needs, the ratio of scrap steel and iron ore can be adjusted to obtain the required alloy composition. Prepare the required scrap steel and iron ore. Scrap steel can come from waste machinery and equipment, waste building materials, etc. Iron ore can be raw materials mined from mines. Close the door of the converter to ensure that the converter is sealed.

[0040] The detailed operations of step two are: ensure that the inside of the converter is clean, and check whether the door and ventilation system of the converter are working properly, prepare the required fuel, commonly used fuels are coal, natural gas, liquefied petroleum gas, etc., select appropriate fuel according to the type and scale of the converter, inject fuel into the combustion chamber below the converter, and the fuel can enter the combustion chamber through nozzles, pipes, etc., open the fuel supply system and ignite the fuel. The fuel can be ignited by using igniters, flames, etc., adjust the fuel supply and oxygen supply in the combustion chamber to ensure stable and efficient combustion, use flames to preheat the converter, spray the flame into the inside of the converter, covering the entire furnace, can use flame nozzles and angle adjustment devices to make the flame evenly irradiate various parts of the inside of the converter, as time goes by, the inside of the converter gradually heats up, adjust the temperature and intensity of the flame to reach the required operating temperature, use thermometers and other equipment to monitor the temperature changes inside the converter to ensure that the converter gradually reaches a suitable operating temperature, when the converter reaches a suitable operating temperature, stop injecting fuel and close the fuel supply system.

[0041] The detailed operation of step three is as follows: when it is Q195 steel, argon is used as high-pressure gas, the gas flow rate is 0.036Nm3 / min, the gun position is adjusted to 1350-1500mm, and the gun pressing time is 80 seconds. When it is HRB400 steel, the gas flow rate is 0.036Nm3 / min, the gun position is adjusted to 1450-1600mm, and the gun pressing time is 40 seconds; optimize the copper head parameters of the oxygen gun, adjust the nozzle angle to 12.15°-12.5°; adjust the throat diameter to 34.6mm-33.5mm, increase the bottom blowing volume, enhance the stirring of the molten pool, make the slag-metal reaction more complete, the reaction in the furnace is close to equilibrium, and the molten steel C in the molten pool reacts more completely with the full iron in the slag, so the full iron in the slag is reduced;

[0042] According to actual data: when the converter bottom blowing gas flow rate is: 0.006m3 / min per ton of steel, the average total iron content of the converter final slag is (15.96% for Q195 steel and 12.75% for HRB400 steel); when the converter bottom blowing gas flow rate is: 0.009m3 / min, the converter first pouring rate is 90.29% (12.99% for Q195 steel and 12.15% for HRB400 steel). It is concluded that increasing the bottom blowing gas volume can reduce the total iron in the slag.

[0043] At the same time, the parameters of the oxygen lance copper head have been optimized. The nozzle angle has been optimized from the original 12° to the current 12.15°-12.5°; the throat diameter has been optimized from the original 33mm to the current 34.6mm-33.5mm, so the gun position can be lowered, the process gun position is reduced, and the end gun pressing time is extended;

[0044] In the converter smelting process, lowering the process gun position and extending the final gun pressure time can reduce the total iron content of the final slag. This is because the adjustment of the process gun position and gun pressure time will affect the oxidation-reduction conditions and reaction rate in the furnace, and thus affect the iron content in the slag.

[0045] Lowering the process gun position: The process gun position refers to the position where the oxygen gun is placed in the converter bosh. By injecting oxygen, the metal ore in the furnace is quickly oxidized and melted. When the process gun position is lowered, the oxygen blowing speed slows down, and the contact time between oxygen and metal ore becomes longer. This can increase the contact area between metal ore and oxygen, make the oxidation reaction more complete, increase the iron oxide content in the slag, and thus reduce the total iron content in the final slag.

[0046] Prolong the terminal gun pressure time: The terminal gun pressure is to increase the oxygen supply in the last few minutes before the end of furnace smelting to increase the temperature and oxidation reaction in the furnace. Prolonging the terminal gun pressure time can make the redox reaction in the furnace continue, further oxidize the metal ore, and further increase the iron oxide in the slag, thereby reducing the total iron content in the final slag - by lowering the process gun position and prolonging the terminal gun pressure time, the oxidation reaction in the furnace can be increased, the iron oxide content in the slag can be increased, and the total iron content in the final slag can be reduced.

[0047] The detailed operation of step four is: when the oxygen supply reaches 70%-80% during the converter smelting process, TSC temperature measurement and sampling is carried out. Before performing this step, in order to ensure the accuracy of temperature measurement and sampling and prevent interference between the oxygen lance and the sampling cup, the oxygen lance needs to be lowered. This lowering process is carried out in two stages, namely, the oxygen lance is gradually lowered to the position of the carbon pulling gun. The carbon pulling gun position is a nozzle in the converter. It is mainly used to spray pure carbon or reducing agent to reduce the oxygen content in the molten steel and adjust the composition of the molten steel. By lowering the oxygen lance to the carbon pulling gun position, it can be ensured that during TSC temperature measurement and sampling, the oxygen lance will not interfere with the temperature of the molten steel in the sampling cup. In this way, the temperature information of the molten steel can be obtained more accurately, providing accurate data basis for the control and adjustment of the smelting process.

[0048] The detailed operation of step five is: determine the amount of lime and desulfurizer to be used according to the weight of the molten steel and the sulfur content target. At the same time, ensure that the oxygen supply is sufficient and conduct safety checks. Gradually add lime to the molten steel. The addition of lime can be controlled by a feeding device to ensure uniform addition and no sputtering or splashing. According to the amount of desulfurizer, gradually add desulfurizer to the molten steel. The desulfurizer can be a calcium-aluminum composite desulfurizer, a silicon-aluminum composite desulfurizer, etc. Ensure that the desulfurizer is added evenly and avoid violent reactions. Stir the molten steel so that the lime and other desulfurizers are in full contact with the molten steel to improve the desulfurization effect. The stirring time is generally a few minutes to more than ten minutes.

[0049] The detailed operation of step six is ​​as follows: open the feed port of the converter, add the raw materials of alloy elements into the converter in the charge feeding area above the scrap steel and iron ore. The alloy elements can be chromium, nickel, manganese, etc., and evenly spread the raw materials of alloy elements above the scrap steel and iron ore to ensure that the alloy raw materials are fully in contact with the scrap steel and iron ore, and close the feed port of the converter to ensure that the atmosphere in the converter remains closed.

[0050] The detailed operation of step seven is: during the operation of the converter, use temperature probes or infrared thermometers and other equipment to regularly monitor the temperature inside the furnace. Temperature probes can be set on the top, side or bottom of the converter to obtain temperature data at different positions. When the temperature needs to be lowered, an appropriate amount of coolant can be added to lower the temperature inside the converter. Commonly used coolants include molten iron, scrap steel, waste bricks, etc.

[0051] The detailed operations of step eight are: determine the number and location of samples to be extracted, use appropriate tools to take samples out of the converter to ensure the representativeness of the samples, grind the samples into powder and mix them evenly to ensure the representativeness during sampling, select appropriate analysis methods according to different components, such as spectral analysis, chemical analysis, etc., record the measurement results and perform data processing, analyze the measurement results, and compare them with the specified steel quality requirements.

[0052] The oxygen supply in step 5 requires the operator to judge the required oxygen flow rate through the flame to increase the carbon content of molten steel. Flame judgment: the combustion state in the converter is judged by observing the shape, color and illumination of the furnace wall. The height, brightness and color of the flame will be affected by the oxygen supply. Generally speaking, when the flame is bright and the color is dark, it means that the combustion is more complete and the oxygen supply is moderate; when the flame is low and the color is bright, it means that the combustion is incomplete and the oxygen supply is too little.

[0053] Adjust the oxygen supply flow: According to the flame judgment results, the operator can adjust the converter bottom blowing volume in time to control the amount of oxygen supply. If the flame is bright and the color is dark, it means that the oxygen supply is moderate. At this time, the bottom blowing volume can be kept unchanged or slightly increased; if the flame is low and the color is bright, it means that the oxygen supply is too little. At this time, the bottom blowing volume can be appropriately increased to increase the oxygen input and improve the combustion completeness, which is conducive to increasing the carbon content of the molten steel and thus reducing the total iron content in the final slag.

[0054] The above generally describes the present invention in detail, but it is obvious to a person skilled in the art that some modifications or improvements can be made to the present invention. Therefore, modifications or improvements that do not depart from the spirit of the present invention are within the scope of protection of the present invention.

Claims

1. A method for reducing the total iron content of converter final slag, characterized in that: The method comprises the following steps: Step 1: Preparation: prepare the scrap steel and iron ore in a certain proportion and load them into the converter; Step 2: Preheating: inject fuel into the converter and use flame to preheat the converter to a suitable operating temperature; Step 3: Blowing: Blow high-pressure gas into the bottom of the converter through a high-pressure air gun; Step 4: TSC temperature measurement and sampling. When the amount of oxygen to be supplied reaches 70%-80% during the converter smelting process, TSC temperature measurement and sampling is performed; Step 5: Supply oxygen and add appropriate amount of lime and other desulfurizers to reduce the sulfur content in the molten steel to a reasonable range; Step 6: Blending alloys: according to the needs, some alloy elements such as chromium, nickel, manganese, etc. are added in the converter to improve the properties of the steel; Step 7: Temperature control: According to the smelting requirements, the temperature in the converter is controlled to ensure the reaction in the furnace and the quality of the molten steel; Step 8: Determine the composition. Take samples from the converter regularly for composition analysis to ensure that the quality of the steel meets the requirements. Step nine: Out of the furnace. When the smelting time is reached or meets the requirements, the molten steel is poured out of the furnace and enters the continuous casting machine for molding.

2. The method for reducing the total iron content of converter final slag according to claim 1, characterized in that: The detailed operation of step 1 is: according to the required alloy formula, determine the ratio of scrap steel and iron ore, according to different needs, the ratio of scrap steel and iron ore can be adjusted to obtain the required alloy composition, prepare the required scrap steel and iron ore. Scrap steel can come from waste machinery and equipment, waste building materials, etc., and iron ore can be raw materials mined from mines. Close the door of the converter to ensure that the converter is sealed.

3. The method for reducing the total iron content of converter final slag according to claim 1, characterized in that: The detailed operation of the step two is: ensure that the inside of the converter is clean, and check whether the door and ventilation system of the converter are working properly, prepare the required fuel, commonly used fuels include coal, natural gas, liquefied petroleum gas, etc., select appropriate fuel according to the type and scale of the converter, inject fuel into the combustion chamber below the converter, and the fuel can enter the combustion chamber through nozzles, pipes, etc., open the fuel supply system and ignite the fuel, and the fuel can be ignited by using igniters, flames, etc., adjust the fuel supply and oxygen supply in the combustion chamber, use flames to preheat the converter, and spray the flame into the inside of the converter to cover the entire furnace, and use flame nozzles and angle adjustment devices to make the flame evenly irradiate various parts of the inside of the converter. As time goes by, the inside of the converter gradually heats up, adjust the temperature and intensity of the flame to reach the required operating temperature, use thermometers and other equipment to monitor the temperature changes inside the converter to ensure that the converter gradually reaches a suitable operating temperature, when the converter reaches a suitable operating temperature, stop injecting fuel and close the fuel supply system.

4. The method for reducing the total iron content of converter final slag according to claim 1, characterized in that: The detailed operation of step three is as follows: when it is Q195 steel, argon is used as high-pressure gas, the gas flow rate is 0.036Nm3 / min, the gun position is adjusted to 1350-1500mm, and the gun pressing time is 80 seconds; when it is HRB400 steel, the gas flow rate is 0.036Nm3 / min, the gun position is adjusted to 1450-1600mm, and the gun pressing time is 40 seconds; optimize the parameters of the oxygen gun copper head, adjust the nozzle angle to 12.15°-12.5°; adjust the throat diameter to 34.6mm-33.5mm.

5. The method for reducing the total iron content of converter final slag according to claim 1, characterized in that: The detailed operation of step four is: when the oxygen supply reaches 70%-80% during the converter smelting process, TSC temperature measurement and sampling is performed. Before performing this step, in order to ensure the accuracy of temperature measurement and sampling and prevent interference between the oxygen lance and the sampling cup, the oxygen lance needs to be lowered. This lowering process is carried out in two stages, namely, the oxygen lance is gradually lowered to the position of the carbon pulling lance. The carbon pulling lance is a nozzle in the converter, which is mainly used for spraying pure carbon or reducing agent, and is used to reduce the oxygen content in the molten steel and adjust the composition of the molten steel. By lowering the oxygen lance to the carbon pulling lance position, it can be ensured that during TSC temperature measurement and sampling, the oxygen lance will not interfere with the temperature of the molten steel in the sampling cup. In this way, the temperature information of the molten steel can be obtained more accurately, providing accurate data basis for the control and adjustment of the smelting process.

6. The method for reducing the total iron content of converter final slag according to claim 1, characterized in that: The detailed operation of step five is as follows: determine the amount of lime and desulfurizer to be used according to the weight of the molten steel and the sulfur content target, and at the same time, ensure that the oxygen supply is sufficient and conduct safety checks, gradually add lime to the molten steel, the addition of lime can be controlled by a feeding device to ensure uniform addition and will not cause sputtering or splashing, calculate the amount of desulfurizer, gradually add desulfurizer to the molten steel, the desulfurizer can be a calcium-aluminum composite desulfurizer, a silicon-aluminum composite desulfurizer, etc., ensure that the desulfurizer is added evenly and avoid violent reactions, stir the molten steel, and the lime and other desulfurizers are in full contact with the molten steel.

7. The method for reducing the total iron content of converter final slag according to claim 1, characterized in that: The detailed operation of step six is: open the feed port of the converter, add raw materials of alloy elements into the converter in the charge feeding area above the scrap steel and iron ore, the alloy elements may be chromium, nickel, manganese, etc., and evenly sprinkle the raw materials of alloy elements above the scrap steel and iron ore to ensure that the alloy raw materials are in full contact with the scrap steel and iron ore, close the feed port of the converter, and ensure that the atmosphere in the converter remains in a closed state.

8. The method for reducing the total iron content of converter final slag according to claim 1, characterized in that: The detailed operation of step seven is: during the operation of the converter, use a temperature probe or infrared thermometer and other equipment to regularly monitor the temperature inside the furnace. Temperature probes can be set on the top, side or bottom of the converter to obtain temperature data at different positions. When the temperature needs to be lowered, an appropriate amount of coolant can be added to lower the temperature inside the converter. Commonly used coolants include molten iron, scrap steel, waste bricks, etc.

9. The method for reducing the total iron content of converter final slag according to claim 1, characterized in that: The detailed operations of step eight are: determine the number and location of samples to be extracted, use appropriate tools to take samples out of the converter to ensure the representativeness of the samples, grind the samples into powder and mix them evenly to ensure the representativeness during sampling, select appropriate analysis methods such as spectral analysis, chemical analysis, etc. according to different components, record the measurement results and perform data processing, analyze the measurement results, and compare them with the specified steel quality requirements.

10. The method for reducing the total iron content of converter final slag according to claim 1, characterized in that: The oxygen supply in step five requires the operator to judge the required flow rate of oxygen supply through the flame.