High-strength corrosion-resistant zirconium-cerium binary alloy and preparation method thereof

By adding cerium elements to the zirconium alloy, a stable oxide film is formed and the phase boundary is reduced. The vacuum arc smelting and annealing process is adopted to solve the problem of insufficient corrosion resistance of zirconium alloy, which significantly improves its mechanical properties and corrosion resistance. It is suitable for High temperature and high pressure environment.

CN118996202APending Publication Date: 2024-11-22HEBEI UNIV OF TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410968714.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing zirconium alloys have insufficient corrosion resistance in high temperature and high pressure environments, and their mechanical properties are demanded in the non-nuclear field year by year. However, the domestic development of new industrial zirconium products is difficult to meet the needs of improving mechanical properties.

Method used

By adding cerium elements, a more stable and dense oxide film is formed, the number of α/β phase boundaries is reduced, and a high-strength corrosion-resistant zirconium cerium binary alloy is prepared by vacuum arc smelting and annealing process to improve its corrosion resistance and comprehensive mechanical properties.

Benefits of technology

It significantly improves the yield strength, hardness and corrosion resistance of zirconium cerium binary alloy, and has simple process and is suitable for engineering structural parts, which has a wide range of application value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996202A_ABST
    Figure CN118996202A_ABST
Patent Text Reader

Abstract

The invention relates to a high-strength corrosion-resistant zirconium-cerium binary alloy and a preparation method thereof. The alloy comprises the following two elements in atomic ratio: 99 to 99.9 at% of Zr, 0.1 to 1.0 at% of Ce and the balance of unavoidable impurities. According to the alloy, by adding the cerium element, formation of a more stable and compact oxidation film is promoted, the number of alpha / beta phase boundaries is reduced, and the corrosion resistance and the comprehensive mechanical property of the zirconium alloy can be effectively improved. Compared with the original zirconium without cerium element, the alloy obtained by the invention shows excellent yield strength and hardness and good corrosion resistance in a room temperature environment, and also has the characteristics of simple production process, good plasticity and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of zirconium alloys, and in particular to a high-strength, corrosion-resistant zirconium-cerium binary alloy and a preparation method thereof. Background Art

[0002] Zirconium (Zr) and zirconium alloys have the characteristic of low thermal neutron cross-sectional absorption rate. The neutron absorption cross-sectional area of ​​zirconium is (0.18×10-28m 2 ), effectively reducing the damage caused by radiation to the material itself, and the density of zirconium is not high (6.49g / cm 3 ), small thermal expansion coefficient, high melting point (1825℃), so it has significant advantages in completing work in harsh environments. It still has good mechanical properties and corrosion resistance under high temperature and high pressure environments. It is widely used in acetic acid applications, as well as the chemical industry and nuclear industry. Zirconium's excellent corrosion resistance can be reflected under high temperature conditions, and it still performs well in an environment full of water and steam. In addition, zirconium has very excellent resistance to neutron irradiation in nuclear reactors, and has strong mechanical properties and good processing properties. Zirconium and zirconium alloys are excellent structural materials for nuclear power reactors, as well as their fuel cladding materials, and have a wide range of application value.

[0003] Zirconium is an active metal, but a dense oxide film can be formed on its surface. If the passivation zone is damaged, the corrosion resistance of zirconium and zirconium alloys will drop rapidly, often causing inevitable losses. Therefore, from this aspect, zirconium needs to improve its corrosion resistance. In recent years, zirconium alloys have also shown an increasing demand in non-nuclear fields such as chemical industry, biomedicine, and marine engineering, and the mechanical requirements for zirconium alloys have been continuously improved. However, my country's new industrial zirconium products are still in the early stages of research and development. Therefore, it is of great significance to study how to improve the mechanical properties of zirconium alloys.

[0004] Due to their unique chemical properties, rare earth metals are widely used in high-tech fields such as electronics, communications, optics, magnetic materials and catalysts. In addition, rare earth metals are also widely used in green energy, energy conservation and environmental protection, new materials and other fields. Studies have shown that the rare metal cerium (Ce) can improve the mechanical properties and corrosion resistance of alloys. Through the study of Ce-doped aluminum (Al) alloys by Yang et al., it was found that the addition of Ce to Al alloys can greatly refine the grains and generate Al11Ce3 second phases, which plays a role in strengthening the second phase and greatly improves the hardness, strength, high temperature resistance and conductivity of Al alloys. my country is rich in rare earth resources (Ce content reaches 0.0046%), and the study of the potential value of rare earths is of great significance to promoting the transformation and upgrading of economic structure.

[0005] In the current technology, the research on binary zirconium alloys is usually focused on adding β-phase stabilizing elements (such as: "CN115896496B A high-strength and tough zirconium-iron binary alloy and its preparation method"). The mechanism of the influence of iron on the microstructure of zirconium alloy is used to improve the hardness and strength of zirconium alloy (the iron element is used to increase the stability of the β phase, so that the alloy has a higher dislocation density and a more complex structure). However, due to the number of α / β phase boundaries and the characteristics of the oxide film, this has limited improvement on the comprehensive performance of the good mechanical properties and corrosion resistance of the zirconium alloy; therefore, it is necessary to increase the research on mixed binary zirconium alloys. Summary of the invention

[0006] The purpose of the present invention is to provide a strong, tough and corrosion-resistant zirconium-cerium binary alloy and a preparation method thereof in view of the deficiencies in the current technology. The alloy promotes the formation of a more stable and dense oxide film by adding cerium, and reduces the number of α / β phase boundaries, which can effectively improve the corrosion resistance and comprehensive mechanical properties of the zirconium alloy. Compared with the original zirconium without cerium, the alloy obtained by the present invention exhibits excellent yield strength and hardness and good corrosion resistance at room temperature. In addition to the above, it also has the characteristics of simple production process and good plasticity.

[0007] The technical solution of the present invention is:

[0008] A high-strength, corrosion-resistant zirconium-cerium binary alloy, in which the atomic ratios of two elements are respectively: Zr 99-99.9at%, Ce 0.1-1.0at%, and the remainder is inevitable impurities.

[0009] The method for preparing the high-strength and corrosion-resistant zirconium-cerium binary alloy comprises the following steps:

[0010] (1) adding pure zirconium and pure cerium to anhydrous ethanol for ultrasonic cleaning for 18 to 20 minutes, drying them, and mixing them according to the designed ratio;

[0011] (2) Place the prepared materials in the crucible of a non-consumable vacuum arc melting furnace, close the valve, and draw a high vacuum to 0.92-1.02×10 -3 Pa;

[0012] (3) Filling the arc furnace cavity with high-purity argon gas, and then starting arc melting; melting for 4-6 minutes each time, turning on the electromagnetic stirring technology and repeatedly melting and turning the ingot 6-8 times, and obtaining the ingot alloy after cooling;

[0013] Among them, the smelting current is 140~150A / S;

[0014] (4) placing the ingot in a vacuum high-temperature tube furnace, and after 2 to 4 gas washing processes, annealing is performed in a high-purity argon atmosphere at 800 to 1100° C. for 4 to 6 hours, and then cooling to room temperature with the furnace to obtain a high-strength and tough zirconium-cerium binary alloy.

[0015] The purity of the high-purity argon gas is 99.999%;

[0016] The above-mentioned pure zirconium is industrial-grade sponge zirconium, and the purity of pure cerium is 99.9%.

[0017] The pressure of argon gas in step (3) and step (4) is -0.04 MPa to -0.06 MPa.

[0018] The essential features of the present invention are:

[0019] The materials used in the present invention are zirconium and cerium elements. Due to the different types of added elements, the basic properties (melting point and boiling point) of the single elements will also be different; in addition, the phase change conversion temperature of the alloy will also be different due to the different proportions of cerium added.

[0020] Through a large number of studies and experiments, the present invention obtains a zirconium-cerium binary alloy at a smelting current of 140-150A / S (current technology is generally 80-100A / S). The crystal phase microstructure of the zirconium-cerium binary alloy with a Ce content of 0.1at.% is a dual-phase structure of β grain boundaries, and the α laths are transformed into needle-shaped structures, which reduces the spacing between the α and β phase layers of the dual-phase titanium alloy, coarsens the grain boundaries, and improves the microstructure and properties of the material, showing good plasticity and mechanical properties, as well as corrosion resistance.

[0021] The beneficial effects of the present invention are:

[0022] 1. Compared with zirconium metal, by introducing an appropriate amount of cerium element, the zirconium-cerium binary alloy prepared has the characteristics of high yield strength, greater hardness, and good toughness;

[0023] 2. my country has abundant reserves of cerium rare earth elements. The introduction of Ce elements improves the stability of the metal β phase and inhibits the α phase, which is more conducive to the microstructure of gold adjustment;

[0024] 3. Compared with zirconium metal, the Vickers hardness of all cerium-containing zirconium-cerium binary alloys in the present invention is increased by 11% to 12% compared with the material, and the corrosion resistance is effectively improved, and can be widely used in the field of engineering structural parts;

[0025] 4. The processing process of zirconium-cerium alloy series is simple. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The metallographic optical micrographs of the zirconium alloys prepared in Comparative Example 1 and Examples 1-3; Figure 1(a) is a metallographic optical micrograph of the zirconium alloy of Comparative Example 1; Figure 1 (b) is a metallographic optical micrograph of the zirconium alloy obtained in Example 1, Figure 1 (c) is a metallographic optical micrograph of the zirconium alloy obtained in Example 2, Figure 1 (d) is a metallographic optical micrograph of the zirconium alloy prepared in Example 3;

[0027] Figure 2 The xrd spectra of zirconium-iron alloys of comparative example 1 and examples 1-3 are shown;

[0028] Figure 3 Vickers hardness diagram of zirconium-cerium alloys of Comparative Example 1 and Examples 1-3;

[0029] Figure 4 The electrochemical open circuit potential curves of zirconium-cerium alloys in NaCl solution of Comparative Example 1 and Examples 1-3;

[0030] Figure 5 The electrochemical impedance spectra of the zirconium-cerium alloys in NaCl solution are shown in Comparative Example 1 and Examples 1-3, wherein: Figure 5 (a) is the Nyquist plot of electrochemical impedance spectroscopy of Zr and Ce alloy in NaCl solution; Figure 5 (b) is the Nyquist amplitude diagram of electrochemical impedance spectroscopy. Figure 5 (c) is the Nyquist phase diagram of electrochemical impedance spectroscopy;

[0031] Figure 6 Polarization curves of zirconium-cerium alloys of comparative example 1 and examples 1-3 in NaCl solution. DETAILED DESCRIPTION

[0032] The following is a further detailed description of the embodiments of the present invention to make the technology, purpose and advantages of the present invention clearer.

[0033] The invention provides a high-strength corrosion-resistant zirconium-cerium binary alloy and a preparation method thereof. Calculated by atomic content, the atomic ratios of the two elements are: Zr 99-99.9at%, Ce 0.1-1.0at%, and the remainder is inevitable impurities.

[0034] The Ce element introduced in the present invention is a β-phase stabilizing element. The introduction of the Ce element improves the stability of the metal β phase and inhibits the α phase, thereby increasing the hardness of the alloy and facilitating the regulation of the alloy's microstructure. On the other hand, a certain content of the Ce element can improve the mechanical properties and corrosion resistance of the alloy;

[0035] The present invention also provides a high-strength and tough zirconium-cerium binary alloy and a preparation method thereof, comprising the following steps:

[0036] (1) melting the alloy raw materials to obtain a cast alloy billet;

[0037] (2) Annealing the cast alloy billet obtained in step (1) to obtain a high-strength, corrosion-resistant zirconium-cerium binary alloy with uniform structure.

[0038] The present invention obtains a cast alloy billet after melting the alloy raw material. The present invention has no special restrictions on the type of the alloy raw material, and adopts alloy raw materials well known to those skilled in the art, so as to obtain a zirconium alloy of the target component. In the present invention, the alloy raw materials are industrial-grade sponge zirconium and pure cerium. The present invention has special restrictions on the ratio of the cerium alloy raw material.

[0039] In the present invention, the smelting is preferably vacuum arc melting, and the equipment used is a WK series vacuum arc furnace, and the current of the vacuum arc melting is 140-150A / S. In the present invention, the vacuum degree of the vacuum arc melting is preferably carried out under argon conditions of -0.04 to -0.06MPa. When vacuum arc melting is adopted, the present invention preferably first evacuates the vacuum degree in the furnace chamber to below -4.5×10-3Pa, and then introduces argon gas; the amount of argon introduced is sufficient to meet the amount of ionized gas for arc melting. The present invention has no special requirements for the specific implementation of the vacuum arc, and it can be adopted by those skilled in the art. The present invention adopts the method of first evacuating the vacuum and then introducing argon gas to first avoid Zr absorbing a large amount of hydrogen, oxygen and nitrogen at high temperature, and causing hydrogenation, oxidation and nitridation, and can also provide ionized gas for arc melting. In the present invention, the number of smelting is preferably more than 5 times, and more preferably 7 times, and a cast alloy billet is obtained after smelting; the time of each smelting is preferably 4 to 5 minutes. In the present invention, when smelting is repeated, the smelting is preferably carried out in a vacuum arc melting furnace; specifically, the metal raw material is smelted in the arc melting furnace to obtain a molten liquid; then cooled to obtain a cast billet, and then the cast billet is turned over. Then smelting is performed again to obtain a molten liquid, and the molten liquid is cooled again to obtain a cast billet, and this is repeated for more than 5 times to ensure that the composition of the cast billet is uniform.

[0040] Before the smelting, the present invention preferably performs ultrasonic cleaning on the alloy raw material; the present invention has no special requirements on the specific implementation of the ultrasonic cleaning, and can adopt the method known to those skilled in the art. The cast alloy billet is obtained, and the present invention performs annealing on the cast alloy billet to obtain an ingot with uniform structure.

[0041] In the present invention, the temperature of the annealing treatment is 900° C., and the time of the annealing treatment is 5 hours.

[0042] In order to further illustrate the present invention, a high-strength and corrosion-resistant zirconium-cerium binary alloy and a preparation method thereof are described in detail below in conjunction with embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0043] Comparative Example 1

[0044] (1) According to the alloy component Zr, 50 g of industrial-grade sponge zirconium is taken, the raw material is placed in a beaker containing anhydrous ethanol, and the surface impurities are removed by ultrasonic cleaning for 10 minutes. After cleaning, the ingredients are mixed according to the designed ratio;

[0045] (2) Place the prepared materials in a water-cooled copper crucible in a non-consumable vacuum arc melting furnace, close the valve, and evacuate to a high vacuum of 0.92 to 1.02 × 10 -3 Pa;

[0046] (3) Before arc smelting, high-purity argon gas (purity of 99.999%) at -0.04MPa to -0.06MPa is filled into the arc furnace cavity for smelting. Each smelting lasts for 5 minutes. The ingot is smelted and turned over seven times to obtain an ingot alloy. The smelting current is 160 to 180A / S. During the smelting process, attention is paid to the changes in the pressure gauge value to prevent leakage from affecting the quality of the ingot.

[0047] (4) The ingot was placed in a SK-G08143 vacuum tube furnace. After three gas washing processes, it was annealed in an argon atmosphere at 900°C for 5 hours and cooled in the furnace to obtain pure Zr.

[0048] Each gas washing process in step (4) is as follows: evacuate with a vacuum pump to -0.1 MPa, turn off the vacuum pump, and then introduce argon gas; the argon gas atmosphere is -0.04 MPa to -0.06 MPa;

[0049] (5) After the ingot is completely cooled, the oxide scale on the surface of the prepared ingot is polished clean, and the required sample is prepared to test its performance;

[0050] (6) The microstructure of the pure Zr alloy obtained in this example was observed. Figure 1 As shown, it can be seen that the structure of this example is a staggered woven basket structure, which is an α-phase lath. XRD analysis shows that the matrix of this example is an α-phase, which is consistent with the metallographic analysis result. The test instrument for metallographic structure observation is a Zeiss inverted optical microscope.

[0051] Operation process: 1) First adjust "Extern" to the lowest position and rotate it counterclockwise to the left.

[0052] 2) Turn on the power switch "Powder". If it turns green, it means the power output is normal. Select RL mode.

[0053] 3) Place the sample upside down on the stage;

[0054] 4) Select the photography mode (the white lines aligned from the outside to the inside represent 1 bright field, 2 polarized light, 3 dark field mode, and you will hear a click when you rotate counterclockwise);

[0055] 5) Focusing at low magnification (the colors of the objective lens are red, yellow, green, blue and white, representing the objective lens of 5, 10, 20, 50 and 100 times respectively);

[0056] 6) Open the "AxioVision LE64" software from the desktop, select "Preview", corresponding to "Multiplier", adjust the brightness and contrast, and "Take Photo";

[0057] 7) Then add a ruler, save the image, and copy the data;

[0058] 8) Adjust the light intensity to minimum, turn off the power switch, and shut down the personal computer.

[0059] The XRD test instrument is German Cu target K α Bruker D8-Discover X-ray diffractometer with 100 nm radiation.

[0060] The operation process is: place the sample on the stage, then scan it in the range of 0-90° at a speed of 6° per minute, and save the data after completion.

[0061] The testing instrument for Vickers hardness is HMV Vickers hardness tester.

[0062] The operation process is as follows: use HMV Vickers hardness tester to measure the sample hardness, load value 1N, load time 15S, test ten points on the sample, remove the maximum and minimum values, and take the average value

[0063] Electrochemical corrosion experiment

[0064] The operation process is:

[0065] The etched samples were mechanically ground to 3000 mesh using SiC sandpaper and then polished with 0.04 mm silica suspension to obtain a scratch-free surface. The polished samples were cleaned in an ultrasonic cleaner filled with acetone solution. Finally, the surface of the samples was cleaned with deionized water.

[0066] The treated zirconium alloy sample was placed in a 3.5% NaCl aqueous solution and the electrochemical corrosion performance test was performed using an electrochemical workstation at room temperature.

[0067] A three-electrode electrochemical cell system was used, with a platinum foil electrode as the auxiliary electrode and a saturated calomel electrode as the reference electrode. Before each electrochemical impedance spectroscopy (EIS) experiment, an open circuit potential (OCP) test of 600 s was performed to obtain a stable potential. The frequency range of the impedance spectrum was 10 MHz–100 kHz, and the amplitude of the sinusoidal perturbation potential was 10 mv. ZSimpWin software was used for impedance spectrum analysis and equivalent circuit fitting. At a scan rate of 1 mv / s, the potential kinetic polarization curves in the range of -1000 mv (SCE) to 2500 mv (SCE) were recorded.

[0068] Example 1

[0069] (1) According to the alloy composition Zr-0.1Ce, 44.955 g of industrial-grade sponge zirconium and 0.045 g of pure cerium were taken, and the raw materials were placed in a beaker containing anhydrous ethanol, and cleaned with an ultrasonic cleaner for 20 minutes to remove surface impurities. After cleaning, the ingredients were mixed according to the designed ratio;

[0070] (2) Place the prepared materials in a water-cooled copper crucible in a non-consumable vacuum arc melting furnace, close the valve, and evacuate to a high vacuum of 0.92 to 1.02×10 -3 Pa;

[0071] (3) Before arc smelting, high-purity argon gas (purity of 99.999%) at -0.04MPa to -0.06MPa is filled into the arc furnace cavity for smelting. Each smelting lasts for 5 minutes. The ingot is smelted and turned over seven times. After cooling, the ingot alloy is obtained. The smelting current is 140 to 145A / S. During the smelting process, attention is paid to the changes in the pressure gauge value to prevent leakage from affecting the quality of the ingot.

[0072] (4) The ingot was placed in a SK-G08143 vacuum tube furnace and, after three gas washing processes, annealed at 900° C. for 5 hours in a high-purity argon atmosphere and cooled in the furnace to obtain a Zr-0.1Ce alloy.

[0073] Each gas washing process in step (4) is as follows: evacuate with a vacuum pump to -0.1 MPa, turn off the vacuum pump, and then introduce argon gas; the argon gas atmosphere is -0.04 MPa to -0.06 MPa;

[0074] (5) After the ingot is completely cooled, the oxide scale on the surface of the prepared ingot is polished clean, and the required sample is prepared to test its performance;

[0075] (6) The microstructure of the zirconium-cerium binary alloy obtained in this example was observed. The results are as follows: Figure 2As shown, it can be seen that in this example, the α lath of the original grain is transformed into a needle-like structure, the β grain boundary begins to appear, and the overall microstructure of the zirconium alloy becomes that all grains are filled with needle-like structures. The increase of the new phase is the reason for the improved stability of the β phase, which is consistent with the results of metallographic analysis.

[0076] Example 2

[0077] (1) According to the alloy composition Zr-0.5Ce, 44.775 g of industrial-grade sponge zirconium and 0.225 g of pure cerium were taken, and the raw materials were placed in a beaker containing anhydrous ethanol, and cleaned with an ultrasonic cleaner for 10 minutes to remove surface impurities. After cleaning, the ingredients were mixed according to the designed ratio;

[0078] (2) Place the prepared materials in a water-cooled copper crucible in a non-consumable vacuum arc melting furnace, close the valve, and evacuate to a high vacuum of 0.92 to 1.02 × 10 -3 Pa;

[0079] (3) Before arc smelting, high-purity argon gas (purity of 99.999%) at -0.04MPa to -0.06MPa is filled into the arc furnace cavity for smelting. Each smelting lasts for 5 minutes. The ingot is smelted and turned over seven times to obtain an ingot alloy. The smelting current is 144 to 147A / S. During the smelting process, attention is paid to the changes in the pressure gauge value to prevent leakage from affecting the quality of the ingot.

[0080] (4) The ingot was placed in a vacuum tube furnace, and after three gas washing processes, it was annealed in a high-purity argon atmosphere at 900° C. for 5 hours, and cooled in the furnace to obtain a Zr-0.5Ce alloy.

[0081] Each gas washing process in step (4) is as follows: evacuate with a vacuum pump to -0.1 MPa, turn off the vacuum pump, and then introduce argon gas; the argon gas atmosphere is -0.04 MPa to -0.06 MPa;

[0082] (5) After the ingot is completely cooled, the oxide scale on the surface of the prepared ingot is polished clean, and the required sample is prepared to test its performance;

[0083] (6) The microstructure of the zirconium-iron binary alloy obtained in this example was observed. The results are as follows: Figure 3 As shown, it can be seen that the α lath needle structure of the original grain of the crystal in this example is more obvious, the structure changes from α lath to a dual-phase structure with more obvious β grain boundaries, the β grain boundaries are clearer, and the stability of the β phase is further improved, which is consistent with the results of metallographic analysis.

[0084] Example 3

[0085] (1) According to the alloy composition Zr-1.0Ce, 44.550 g of industrial-grade sponge zirconium and 0.450 g of pure cerium were taken, and the raw materials were placed in a beaker containing anhydrous ethanol, and cleaned with an ultrasonic cleaner for 10 minutes to remove surface impurities. After cleaning, the ingredients were mixed according to the designed ratio;

[0086] (2) Place the prepared materials in a water-cooled copper crucible in a non-consumable vacuum arc melting furnace, close the valve, and evacuate to a high vacuum of -4.5 to -4.9×10 -3 Pa;

[0087] (3) Before arc smelting, high-purity argon gas of -0.04MPa to -0.06MPa is filled into the arc furnace cavity for smelting. Each smelting lasts for 5 minutes. The ingot is smelted and turned over seven times to obtain an ingot alloy. The smelting current is 147 to 150A / S. During the smelting process, attention is paid to the changes in the pressure gauge value to prevent leakage from affecting the quality of the ingot.

[0088] (4) The ingot was placed in a vacuum tube furnace, and after three gas washing processes, it was annealed in a high-purity argon atmosphere at 1000° C. for 5 hours, and cooled in the furnace to obtain (atomic ratio formulation) Zr-1.0Ce alloy.

[0089] Each gas washing process in step (4) is as follows: evacuate with a vacuum pump to -0.1 MPa, turn off the vacuum pump, and then introduce argon gas; the argon gas atmosphere is -0.04 MPa to -0.06 MPa;

[0090] (5) After the ingot is completely cooled, the oxide scale on the surface of the prepared ingot is polished clean, and the required sample is prepared to test its performance;

[0091] (6) The microstructure of the zirconium-cerium binary alloy obtained in this example was observed. With the increase of rare earth element content, the stability of the β phase was improved, and a dual-phase structure appeared. The needle-shaped α phase would preferentially nucleate and grow at the β grain boundary. The alloy showed an α+β phase structure, which was the main component of the alloy. It segregated at the grain boundary of the alloy, resulting in a decrease in the bonding strength of the phase boundary.

[0092] Table 1: Performance test results of comparative example 1 and embodiments 1-3 of the present invention

[0093]

[0094] The electrochemical corrosion results of zirconium-cerium alloys of Examples 1-3 and Comparative Example 1 are shown in Table 1. Figure 5 , Figure 6As shown in the figure, the experimental results show that with the increase of the rare earth element Ce content, the polarization curve tends to move towards the direction of low current density and high potential, and the self-corrosion current density value increases, indicating that the corrosion resistance is better. From the changing trends of the corrosion potential value and the self-corrosion current density value of the zirconium alloy, it can be seen that Example 2 has the best corrosion resistance.

[0095] From Table 1, Figure 6 As shown, the hardness of all zirconium-cerium alloys is greatly improved compared with that of comparative example 1, among which the hardness of Example 1 is improved by 122% compared with that of comparative example 1. The electrochemical corrosion effect of all zirconium alloys is improved in Example 2, and the hardness is improved by 111% compared with that of comparative example 1.

[0096] It can be seen that the reason why the corrosion resistance of Example 2 is superior is that when the content of rare earth element Ce is further increased to 0.5%, the matrix of Zr-1.0Ce alloy containing a small amount of α phase reduces the number of α / β phase boundaries, reduces the galvanic corrosion between the grain boundary and the matrix phase, and weakens the current interaction. Therefore, the corrosion resistance of Zr-0.5Ce alloy is better than that of Zr-0.1Ce alloy. At the same time, as the content of rare earth element Ce increases, the alloy grains are refined, and thus the hardness of the material is improved.

[0097] It can be seen that Example 2 is good because its yield strength is greatly improved without losing much plasticity, and its corrosion resistance is the best. In Example 1, 0.1% cerium is added, the hardness is increased by 122%, and the corrosion resistance improvement effect is still obvious.

[0098] The present invention is described through embodiments, but does not constitute a limitation to the present invention. With reference to the description of the present invention, other changes in the disclosed embodiments are easy to guess for researchers in the field of zirconium alloys, and such changes should fall within the scope defined by the patent requirements of the present invention.

[0099] Matters not covered by the present invention are known technologies.

Claims

1. A high-strength, corrosion-resistant zirconium-cerium binary alloy, characterized by The atomic ratios of the two elements in the alloy are: Zr 99-99.9at%, Ce 0.1-1.0at%, and the remainder is inevitable impurities.

2. The method for preparing the high-strength and corrosion-resistant zirconium-cerium binary alloy according to claim 1, characterized in that The following steps are involved: (1) adding pure zirconium and pure cerium to anhydrous ethanol for ultrasonic cleaning for 18 to 20 minutes, drying them, and mixing them according to the designed ratio; (2) Place the prepared materials in the crucible of a non-consumable vacuum arc melting furnace, close the valve, and draw a high vacuum to 0.92-1.02×10 -3 Pa; (3) Filling the arc furnace cavity with high-purity argon gas, and then starting arc melting; melting for 4-6 minutes each time, turning on the electromagnetic stirring technology and repeatedly melting and turning the ingot 6-8 times, and obtaining the ingot alloy after cooling; Among them, the smelting current is 140~150A / S; (4) placing the ingot in a vacuum high-temperature tube furnace, and after 2 to 4 gas washing processes, annealing is performed in a high-purity argon atmosphere at 800 to 1100° C. for 4 to 6 hours, and then cooling to room temperature with the furnace to obtain a high-strength and tough zirconium-cerium binary alloy.

3. The method for preparing the high-strength and corrosion-resistant zirconium-cerium binary alloy according to claim 2, characterized in that The purity of the high-purity argon gas is 99.999%.

4. The method for preparing the high-strength and corrosion-resistant zirconium-cerium binary alloy as described in claim 2, wherein the above-mentioned pure zirconium is industrial-grade sponge zirconium and the purity of pure cerium is 99.9%.

5. The method for preparing the high-strength and corrosion-resistant zirconium-cerium binary alloy as claimed in claim 2, characterized in that The pressure of argon gas in step (3) and step (4) is -0.04 MPa to -0.06 MPa.

Citation Information

Patent Citations

  • A high-strength and tough zirconium-iron binary alloy and preparation method thereof

    CN115896496B