Method for refining original austenite grains of continuous casting billet of bainite steel rail

By accurately controlling the content of titanium, carbon and nitrogen and processing, fine austenite grains are formed, which solves the problem of insufficient performance of bainite rail materials and significantly improves its mechanical properties and service life.

CN118996243APending Publication Date: 2024-11-22PANZHIHUA IRON & STEEL RES INST OF PANGANG GROUP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411206672.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

There is a lack of effective methods in the prior art to refine the original austenite grains of continuous casting billets of bainite rails, resulting in insufficient material performance and difficult to meet the high performance needs of heavy-duty railways.

Method used

By accurately controlling the content of titanium, carbon and nitrogen, vacuum treatment and refining processes are used to form nanoscale fine MX-type precipitation phases, limiting the growth of austenite grains, and forming fine austenite through natural cooling and reheating. Grains improve the mechanical properties of the material.

Benefits of technology

It significantly improves the mechanical properties of bainite rails, reduces processing risks, meets the demand for high-performance rails in the rail transit field, and extends the service life of the rails.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996243A_ABST
    Figure CN118996243A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of steel rail manufacturing, and discloses a method for refining original austenite grains of a continuous casting billet of a bainite steel rail. The method comprises the following steps: primarily smelting raw materials to obtain molten steel; the molten steel is refined, in the refining process, the content of titanium is precisely controlled, so that the weight ratio of titanium in the molten steel is 0.08%-0.13%, the molten steel is subjected to vacuum treatment, so that the weight ratio of carbon in the molten steel is 0.21%-0.25%, and the weight ratio of nitrogen in the molten steel is 0.005%-0.008%; the refined molten steel is subjected to continuous casting, and a continuous casting blank is obtained; the continuous casting blank is naturally cooled to remove hydrogen till the room temperature is reached; and the cooled continuous casting billet is reheated for austenitizing, and the original austenite grain refined continuous casting billet is obtained. According to the method disclosed by the invention, a pinning effect is formed at a grain boundary by utilizing a nanoscale fine dispersed precipitated phase, so that the growth of original austenite grains is effectively limited.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rail manufacturing, and in particular to a method for refining original austenite grains of a continuous casting billet of a bainite rail. Background Art

[0002] For heavy-duty railways, the increasing axle weight increases the stress on the rails, the service conditions of the rails gradually deteriorate, the frequency of rail damage caused by wear and rolling contact fatigue increases significantly, and the railway maintenance costs of the rails are also increasing. Pearlite rails are widely used in heavy-duty railways at home and abroad because of their high strength, toughness and wear resistance. At the same time, the interlamellar spacing of pearlite groups is reduced by increasing the carbon content of pearlite rails or adjusting the heat treatment process, thereby improving the strength of pearlite steel. However, the strength and hardness of pearlite rails have almost reached their theoretical improvement limits. In this context, bainite rails have become the focus of research in the development of high-speed heavy-duty railways. Compared with traditional pearlite rails, bainite rails have high strength and toughness matching, high wear resistance and contact fatigue resistance. At the same time, due to their good welding performance, the fatigue wear problem caused by welding damage has also been effectively solved. Therefore, bainite rails have broad application prospects in heavy-duty railways.

[0003] In the production process of bainitic rails, the control of the grain size of the continuous casting billet is a key factor in ensuring its performance. The grain size affects the microstructure and macroscopic performance of the material. The fine and evenly distributed original austenite grains of the continuous casting billet can promote the transformation of bainite into fine lath bainite during the subsequent rolling and cooling process, which can improve the mechanical properties of the rail and make the bainitic rail have excellent strength and toughness. In addition, the excessive growth of the grains of the continuous casting billet may cause overheating and overburning of the material, which will reduce the overall performance of the material and even cause damage. During the hot rolling process, the fine original austenite grains help to achieve better plastic deformation, optimize the shape and size of the material, and reduce the required deformation force and energy consumption. During the cooling process, the fine grains of the rail help to achieve more uniform and effective cooling rate control, which is crucial for the formation of bainite structure. In addition, the fine original austenite grain size helps to improve the wear resistance of the rail, especially in applications subject to high friction and wear. Finally, preventing grain coarsening can avoid grain boundary segregation and other microscopic defects in the material, which may become the origin of cracks and affect the durability and reliability of the material.

[0004] Therefore, refining the original austenite grains of the continuous casting billet of the bainite rail is of great help in improving the performance of the bainite rail. However, the prior art lacks related technologies. Summary of the invention

[0005] In view of the above problems, the present invention provides a method for refining the original austenite grains of a continuous casting billet of a bainite rail.

[0006] According to one aspect of the present invention, a method for refining original austenite grains of a continuous casting billet of a bainite rail is provided, comprising the following steps: Step S1: Preliminary smelting of raw materials to obtain molten steel; Step S2: refining the molten steel, during which the titanium content is precisely controlled so that the weight proportion of titanium in the molten steel is 0.08%-0.13%, and vacuum treating the molten steel so that the weight proportion of carbon in the molten steel is 0.21%-0.25%, and the weight proportion of nitrogen in the molten steel is 0.005%-0.008%; Step S3: continuously casting the refined molten steel to obtain a continuously cast billet; Step S4: naturally cooling the continuous casting billet to remove hydrogen until the temperature reaches room temperature; Step S5: reheating the cooled continuous casting billet to austenitize the billet, so as to obtain a continuous casting billet with refined original austenite grains.

[0007] According to one embodiment of the present invention, in step S2, accurately controlling the titanium content includes: Step S2-1: before the refining, performing an initial component analysis on the molten steel to determine the current titanium content; Step S2-2: Calculate the amount of titanium alloy to be added based on the desired final chemical composition and initial composition analysis; Step S2-3: adding titanium alloy to the molten steel according to the required amount of titanium alloy.

[0008] According to one embodiment of the present invention, in step S2-3, a stirring operation is adopted when adding the titanium alloy, and the titanium alloy is a titanium-iron alloy.

[0009] According to one embodiment of the present invention, step S2 further includes: Step S2-4: After adding the titanium alloy, a secondary component analysis is performed to verify whether the titanium content reaches a predetermined target. If not, fine-tuning is performed by further adding titanium alloy or adjusting process parameters.

[0010] According to one embodiment of the present invention, in step S2, the refining temperature is controlled at 1400-1600°C.

[0011] According to one embodiment of the present invention, step S2 further includes performing a final component analysis before the refining is completed, and ensuring that the weight ratio of each component in the molten steel meets the following requirements before steel tapping: C: 0.21%~0.25%; Si: 2.0%~2.5%; Mn: 0.60%~1.00%; Cr: 0.60%~0.80%; Mo: 0.40%~0.45%; N: 0.005%~0.008%; Ti: 0.08%~0.13%; the balance is Fe and unavoidable impurities.

[0012] According to one embodiment of the present invention, the titanium, carbon and nitrogen in the molten steel satisfy the following chemical equivalent ratio when tapping: Ti / C is 3.95-4.00, and Ti / N≤3.42.

[0013] According to one embodiment of the present invention, in step S3, the cooling rate during the continuous casting process is controlled to be 200-300° C. / s.

[0014] According to one embodiment of the present invention, in step S4, the cooling time is not less than 24 hours.

[0015] According to an embodiment of the present invention, in step S5, the heating temperature is 1200-1300°C.

[0016] Due to the adoption of the above technical scheme, the method provided by the present invention promotes the formation of nano-scale fine and dispersed MX-type precipitation phases through precise chemical composition design and continuous casting process control, especially the comprehensive regulation of titanium (Ti), carbon (C), nitrogen (N), and preferred molybdenum (Mo) and chromium (Cr) elements. These nano-scale fine and dispersed precipitation phases form a pinning effect at the grain boundary, effectively limiting the growth of the original austenite grains. In addition, the hot continuous casting billet forms bainite or martensite during natural cooling, and many fine subgrains may be formed inside the austenite grains during the bainite or martensite phase transformation process. These subgrains can serve as new nuclei in the subsequent heating process to promote the formation of fine austenite grains. In the process of reheating to the austenitizing temperature, the microstructure (such as dislocations and twins) in the bainite or martensite will recover and recrystallize to form fine austenite grains. Through the above technical scheme, the present invention can not only avoid the risk of cracks during processing and improve the production efficiency of subsequent bainite rails, but also significantly improve their mechanical properties, meeting the demand for high-performance rails in the rail transit field. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 The present invention is a flowchart of a method for refining original austenite grains of a continuous casting billet of a bainite rail according to an embodiment of the present invention. DETAILED DESCRIPTION

[0018] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0019] like Figure 1 As shown, the method for refining the original austenite grains of the continuous casting billet of bainite rail provided by the present invention generally comprises the following steps: Step S1: Preliminary smelting of raw materials to obtain molten steel; Step S2: refining the molten steel, during the refining process, accurately controlling the titanium content so that the weight proportion of titanium in the molten steel is 0.08%-0.13%, vacuum treating the molten steel so that the weight proportion of carbon in the molten steel is 0.21%-0.25%, and the weight proportion of nitrogen in the molten steel is 0.005%-0.008%; Step S3: continuously casting the refined molten steel to obtain a continuously cast billet; Step S4: Cooling the continuous casting billet naturally to remove hydrogen until the temperature reaches room temperature; Step S5: reheating the cooled continuous casting billet to austenitize the billet, so as to obtain a continuous casting billet with refined original austenite grains.

[0020] The operation of each step of the method is described in detail below, but the present invention is not limited to the specific parameters given.

[0021] In step S1, the raw materials are preliminarily smelted to obtain molten steel. For example, an electric arc furnace (EAF), a converter or other smelting equipment can be used to melt molten iron, scrap steel and necessary alloying elements to form primary molten steel. During the smelting process, impurities such as sulfur (S) and phosphorus (P) need to be removed to improve the purity of the molten steel.

[0022] In step S2, the molten steel is refined. For example, the molten steel after the initial refining can be transferred to a refining furnace, such as a vacuum degassing furnace (VD furnace) or an external refining station (LF furnace). In this process, gases and inclusions are further removed, and the chemical composition is adjusted to ensure that the molten steel meets the required quality standards. During the refining process of steelmaking, the titanium (Ti) content is accurately controlled so that the weight proportion of titanium in the molten steel is 0.08% to 0.13%. In some embodiments, the control of the Ti content can be performed by, for example, the following operations: Step S2-1: Before refining, the molten steel is subjected to an initial chemical analysis to determine the current titanium content, and the content of other alloying elements can also be determined; Step S2-2: Calculate the amount of titanium alloy to be added based on the desired final chemical composition and initial composition analysis; Step S2-3: adding titanium alloy to the molten steel according to the required amount of titanium alloy.

[0023] The microstructure and macroscopic properties of steel can be improved by adding Ti, a microalloying element. The carbides and nitrides formed by Ti in steel can inhibit grain growth, making it an effective means to refine grains and improve material properties. However, the titanium microalloying process requires precise control, including the amount of titanium added, the ratio with other elements, and the subsequent manufacturing process. Improper control may cause adverse aggregation or precipitation of titanium, thereby affecting material properties. In addition, grain size control of titanium microalloyed steel during continuous casting and hot rolling is also a technical challenge, which requires comprehensive consideration of factors such as cooling rate, chemical composition uniformity, and microstructural transformation.

[0024] In some embodiments, stirring is performed when adding the titanium alloy, and sufficient stirring is performed to ensure uniform distribution of the titanium alloy to avoid local enrichment. The titanium alloy may be a titanium-iron alloy, such as but not limited to FeTi30, FeTi40, FeTi50, etc.

[0025] In some embodiments, a secondary component analysis is performed after adding the titanium alloy to verify whether the titanium content reaches the predetermined target. If the predetermined target is not reached, fine-tuning is performed by further adding titanium alloy or adjusting process parameters.

[0026] In this step, a vacuum degassing furnace (VD furnace) is used for vacuum treatment to remove dissolved gases (such as hydrogen and nitrogen) in the molten steel and promote the dissolution of titanium in the steel. After vacuum treatment, the weight proportion of carbon in the molten steel is 0.21%~0.25%, and the weight proportion of nitrogen is 0.005%~0.008%.

[0027] In some embodiments, the refining temperature is controlled at 1400-1600°C. The solubility of Ti is significantly affected by temperature. Too high a temperature may cause burning of Ti, while too low a temperature may cause insufficient dissolution of Ti. Further, argon stirring is used during the refining process to improve the dissolution efficiency and uniformity of titanium.

[0028] Before the end of refining, the final chemical composition analysis is carried out to confirm whether the content of Ti and other elements meets the standards. After confirming that the composition is correct, the refined molten steel is tapped and prepared for continuous casting. Before tapping, ensure that the weight ratio of each component in the molten steel meets the following requirements: C: 0.21%~0.25%; Si: 2.0%~2.5%; Mn: 0.60%~1.00%; Cr: 0.60%~0.80%; Mo: 0.40%~0.45%; N: 0.005%~0.008%; Ti: 0.08%~0.13%; the balance is Fe and unavoidable impurities.

[0029] Ti exists in the form of carbides and nitrides in steel. Nanoscale fine dispersed precipitates can be formed at grain boundaries and dislocations, hindering the migration of grain boundaries through the pinning effect. Affecting the recrystallization behavior of austenite. During hot rolling, the Ti element can affect the recrystallization behavior of austenite. The precipitation of TiN or Ti (C, N) can inhibit the growth of austenite grains at high temperatures, thereby forming finer grains during the phase transformation process. Moreover, the Ti element can form heterogeneous precipitation at the phase interface between austenite and ferrite. This precipitation can hinder the movement of the phase interface, thereby affecting the grain size and distribution. Further, the addition of Ti can increase the recrystallization temperature of cold-rolled steel, which means that a higher temperature is required to start the recrystallization process, which helps to maintain a fine grain structure at a lower temperature.

[0030] Ti is usually added to steel in trace amounts, with the content generally not exceeding 0.13wt%, which helps to form a large number of nano-scale fine dispersed MX-type precipitation phases (TiC and TiN) during the cooling process. The mass fraction of C and N needs to achieve the initial content control of Ti and C / N. The ratio of Ti to C and Ti to N is crucial for the formation of nano-scale fine TiC and TiN precipitation phases. To this end, the titanium, carbon and nitrogen in the molten steel meet the following chemical equivalent ratios when tapping: Ti / C is 3.95~4.00, and Ti / N≤3.42.

[0031] In addition to the alloy composition design of Ti, the method of the present invention also optimizes the alloy content of alloy elements Mo (molybdenum) and Cr (chromium). Mo and Cr affect the nucleation and growth of Ti (C, N). Mo can replace part of the Ti atoms in Ti (C, N) to form a (Ti, Mo)X solid solution. The atomic radius of Mo is different from that of Ti, and this difference can cause lattice distortion, thereby inhibiting the growth of particles and achieving the effect of reducing the size of Ti (C, N) particles. The addition of Cr will cause lattice distortion of the steel matrix, which can affect the nucleation and growth process of MX-type precipitation phases. Lattice distortion can increase the difficulty of particle nucleation, but it can also hinder the growth of particles, resulting in a reduction in the size of Ti (C, N) particles, which is conducive to the formation of fine and dispersed MX-type precipitation phases and pinning at more locations.

[0032] In step S3, the refined molten steel is continuously cast to obtain a continuously cast billet. In some embodiments, the refined high-quality molten steel is continuously cast through a continuous casting machine, and the liquid molten steel is transformed into a continuous solid billet. When the molten steel solidifies, the cooling rate is controlled to be 200-300°C / s. Rapid cooling can reduce the segregation of elements and promote the formation of fine equiaxed crystals, thereby helping to obtain a fine original austenite grain size.

[0033] In step S4, the continuous casting billet is naturally cooled to remove hydrogen until room temperature. After the molten steel solidifies into a billet, the billet is slowly cooled in a natural environment to reduce internal stress and remove hydrogen dissolved in the steel. The dehydrogenation process is crucial to avoid white spot defects in the rail and avoid hydrogen embrittlement in the subsequent service of the rail, and to improve the plasticity and toughness of the rail. The duration of the cooling process is not less than 24 hours. During the natural cooling stage of the continuous casting billet, the precipitation phase of Ti precipitates below 400°C to obtain fine dispersed TiC and TiN. The grain size of the continuous casting billet after slow cooling: 50μm~90μm. Bainite or martensite is formed during the cooling process of the billet, and many fine subgrains may be formed inside the austenite grains during the phase transformation of bainite or martensite. These subgrains can serve as new nuclei in the subsequent heating process to promote the formation of fine austenite grains.

[0034] In step S5, the cooled continuous casting billet is reheated for austenitization to obtain a continuous casting billet with refined original austenite grains. The billet obtained by continuous casting is heated to above the austenitization temperature, between 1200 and 1300°C, in preparation for hot rolling. During the heating process, the chemical composition and temperature inside the billet need to be homogenized to reduce the internal stress and chemical composition inhomogeneity. During the reheating to the austenitization temperature, the microstructure (such as dislocations and twins) in the bainite or martensite will recover and recrystallize, which helps to form fine austenite grains.

[0035] The present invention is further described below by means of specific examples, but the protection scope of the present invention is not limited thereto.

[0036] Example 1 Molten iron, scrap steel and necessary alloying elements are melted in a converter for preliminary smelting to obtain molten steel. The molten steel is refined. During the refining process, the molten steel is subjected to a preliminary chemical composition analysis, and it is determined that the initial titanium content is 0.03%, which does not meet the requirements. Add FeTi30 (ferrotitanium alloy) to the refining furnace in the form of fine powder and stir it thoroughly to ensure that the titanium alloy is evenly distributed. The refining temperature is controlled at 1400°C. After argon stirring and vacuum treatment, the sample is taken again for analysis to confirm that the titanium content has been adjusted to 0.09%. The molten steel is vacuum treated so that the weight proportion of carbon in the molten steel is 0.21% and the weight proportion of nitrogen is 0.005%. Before tapping, the final composition analysis is carried out to ensure that the weight proportion of each component in the molten steel meets the following requirements: C: 0.21%; Si: 2.0%; Mn: 0.60%; Cr: 0.60%; Mo: 0.40%; N: 0.005%; Ti: 0.09%; the remainder is Fe and unavoidable impurities. The refined molten steel is continuously cast to obtain a continuous casting billet. During the continuous casting process, the flow rate of cooling water and the nozzle layout are adjusted to control the cooling rate at 200℃ / s to promote the formation of fine equiaxed crystals. The pulling speed and cooling system of the continuous casting machine are accurately controlled to ensure that the grain size of the continuous casting billet is uniform and small, and rapid cooling is achieved. The continuously cast billet is slowly cooled in a natural environment to ensure that the cooling time to room temperature exceeds 24 hours, effectively removing hydrogen from the billet and reducing internal stress. The naturally cooled billet is heated to 1200℃ and maintained for 40 minutes for austenitization to ensure the uniformity of the internal temperature and chemical composition of the billet. Control the heating speed not to exceed 300℃ / h to avoid overheating or overburning.

[0037] The results show that the final continuous casting billet has a small and uniform grain size, with an average grain size of 80 μm.

[0038] Example 2 Molten iron, scrap steel and necessary alloying elements are melted in a converter for preliminary smelting to obtain molten steel. The molten steel is refined. During the refining process, the molten steel is subjected to a preliminary chemical composition analysis, and it is determined that the initial titanium content is 0.02%, which does not meet the requirements. Add FeTi40 (ferrotitanium alloy) to the refining furnace in the form of fine powder and stir it thoroughly to ensure that the titanium alloy is evenly distributed. The refining temperature is controlled at 1500°C. After argon stirring and vacuum treatment, the sample is taken again for analysis to confirm that the titanium content has been adjusted to 0.11%. The molten steel is vacuum treated so that the weight proportion of carbon in the molten steel is 0.23% and the weight proportion of nitrogen is 0.007%. Before tapping, the final composition analysis is carried out to ensure that the weight proportion of each component in the molten steel meets the following requirements: C: 0.23%; Si: 2.3%; Mn: 0.80%; Cr: 0.70%; Mo: 0.43%; N: 0.007%; Ti: 0.11%; the remainder is Fe and unavoidable impurities. The refined molten steel is continuously cast to obtain a continuous casting billet. During the continuous casting process, the flow rate of cooling water and the nozzle layout are adjusted to control the cooling rate at 250℃ / s to promote the formation of fine equiaxed crystals. The pulling speed and cooling system of the continuous casting machine are accurately controlled to ensure that the grain size of the continuous casting billet is uniform and small, and rapid cooling is achieved. The continuously cast billet is slowly cooled in a natural environment to ensure that the cooling time to room temperature exceeds 24 hours, effectively removing hydrogen from the billet and reducing internal stress. The naturally cooled billet is heated to 1250℃ and maintained for 45 minutes for austenitization to ensure the uniformity of the internal temperature and chemical composition of the billet. Control the heating speed not to exceed 350℃ / h to avoid overheating or overburning.

[0039] The results show that the final continuous casting billet has a fine and uniform grain size, with an average grain size of 85 μm.

[0040] Example 3 Molten iron, scrap steel and necessary alloying elements are melted in a converter for preliminary smelting to obtain molten steel. The molten steel is refined. During the refining process, the molten steel is subjected to a preliminary chemical composition analysis, and it is determined that the initial titanium content is 0.05%, which does not meet the requirements. Add FeTi50 (ferrotitanium alloy) to the refining furnace in the form of fine powder and stir it thoroughly to ensure that the titanium alloy is evenly distributed. The refining temperature is controlled at 1600°C. After argon stirring and vacuum treatment, the sample is taken again for analysis to confirm that the titanium content has been adjusted to 0.13%. The molten steel is vacuum treated so that the weight proportion of carbon in the molten steel is 0.25% and the weight proportion of nitrogen in the molten steel is 0.008%. Before tapping, the final composition analysis is carried out to ensure that the weight proportion of each component in the molten steel meets the following requirements: C: 0.25%; Si: 2.5%; Mn: 1.00%; Cr: 0.80%; Mo: 0.45%; N: 0.008%; Ti: 0.13%; the remainder is Fe and unavoidable impurities. The refined molten steel is continuously cast to obtain a continuous casting billet. During the continuous casting process, the flow rate of cooling water and the nozzle layout are adjusted to control the cooling rate at 300℃ / s to promote the formation of fine equiaxed crystals. The pulling speed and cooling system of the continuous casting machine are accurately controlled to ensure that the grain size of the continuous casting billet is uniform and small, and rapid cooling is achieved. The continuously cast billet is slowly cooled in a natural environment to ensure that the cooling time to room temperature exceeds 24 hours, effectively removing hydrogen from the billet and reducing internal stress. The naturally cooled billet is heated to 1300℃ and maintained for 35 minutes for austenitization to ensure the uniformity of the internal temperature and chemical composition of the billet. Control the heating speed not to exceed 330℃ / h to avoid overheating or overburning.

[0041] The results show that the final continuous casting billet has a fine and uniform grain size, with an average grain size of 70 μm.

[0042] Comparative Example 1 Molten iron, scrap steel and necessary alloying elements (excluding titanium) are melted in a converter for preliminary smelting to obtain molten steel. The molten steel is refined and fully stirred to ensure uniform distribution of the alloy. The refining temperature is controlled at 1600℃. After argon stirring and vacuum treatment, the sample is analyzed again, so that the weight proportion of carbon in the molten steel is 0.25% and the weight proportion of nitrogen is 0.008%. The final component analysis is carried out before steelmaking to ensure that the weight proportion of each component in the molten steel meets the following requirements: C: 0.25%; Si: 2.5%; Mn: 1.00%; Cr: 0.80%; Mo: 0.45%; N: 0.008%; the remainder is Fe and unavoidable impurities. The refined molten steel is continuously cast to obtain a continuous casting billet. During the continuous casting process, the flow rate of cooling water and the nozzle layout are adjusted to control the cooling rate at 300℃ / s to promote the formation of fine equiaxed crystals. Precisely control the casting speed and cooling system of the continuous casting machine to ensure that the grain size of the continuous casting billet is uniform and small, and achieve rapid cooling. Slowly cool the billet after continuous casting in a natural environment to ensure that the cooling time to room temperature exceeds 24 hours, effectively remove the hydrogen in the billet and reduce internal stress. Heat the naturally cooled billet to 1300℃ and keep it for 35 minutes for austenitization to ensure the uniformity of the internal temperature and chemical composition of the billet. Control the heating rate not to exceed 330℃ / h to avoid overheating or overburning.

[0043] After testing, it was found that the average grain size of the continuous casting billet finally obtained in this comparative example was 250 μm, and the structure was uneven.

[0044] Comparative Example 2 Molten iron, scrap steel and necessary alloying elements are melted in a converter for preliminary smelting to obtain molten steel. The molten steel is refined. During the refining process, the molten steel is subjected to preliminary chemical composition analysis to determine that the initial titanium content is 0.03%, the Ti content is low, and it is fully stirred to ensure uniform distribution of the alloy. The refining temperature is controlled at 1600℃. The molten steel is vacuum treated so that the weight proportion of carbon in the molten steel is 0.25% and the weight proportion of nitrogen in the molten steel is 0.008%. The final component analysis is performed before steelmaking to ensure that the weight proportion of each component in the molten steel meets the following requirements: C: 0.25%; Si: 2.5%; Mn: 1.00%; Cr: 0.80%; Mo: 0.45%; N: 0.008%; Ti: 0.05%; the remainder is Fe and unavoidable impurities. The refined molten steel is continuously cast to obtain a continuous casting billet. During the continuous casting process, the flow rate of cooling water and the nozzle layout are adjusted to control the cooling rate at 300℃ / s to promote the formation of fine equiaxed crystals. Precisely control the casting speed and cooling system of the continuous casting machine to ensure that the grain size of the continuous casting billet is uniform and small, and achieve rapid cooling. Slowly cool the billet after continuous casting in a natural environment to ensure that the cooling time to room temperature exceeds 24 hours, effectively remove the hydrogen in the billet and reduce internal stress. Heat the naturally cooled billet to 1300℃ and keep it for 35 minutes for austenitization to ensure the uniformity of the internal temperature and chemical composition of the billet. Control the heating rate not to exceed 330℃ / h to avoid overheating or overburning.

[0045] After testing, the average grain size of the continuous casting billet finally obtained in this comparative example is 150 μm, and the grain size is coarse.

[0046] Comparative Example 3 Molten iron, scrap steel and necessary alloying elements are melted in a converter for preliminary smelting to obtain molten steel. The molten steel is refined. During the refining process, the molten steel is subjected to preliminary chemical composition analysis to determine that the initial titanium content is 0.05%. Titanium-iron alloy (FeTi50) is added to the refining furnace in the form of fine powder, so that the titanium content after refining is 0.20%. It is fully stirred to ensure uniform distribution of the alloy. The refining temperature is controlled at 1600℃. The molten steel is vacuum treated so that the weight proportion of carbon in the molten steel is 0.25% and the weight proportion of nitrogen is 0.008%. The final component analysis is performed before steelmaking to ensure that the weight proportion of each component in the molten steel meets the following requirements: C: 0.25%; Si: 2.5%; Mn: 1.00%; Cr: 0.80%; Mo: 0.45%; N: 0.008%; Ti: 0.20%; the remainder is Fe and unavoidable impurities. The refined molten steel is continuously cast to obtain a continuous casting billet. During the continuous casting process, adjust the cooling water flow and nozzle layout, and control the cooling rate at 300℃ / s to promote the formation of fine equiaxed crystals. Accurately control the casting speed and cooling system of the continuous casting machine to ensure that the grain size of the continuous casting billet is uniform and small, and achieve rapid cooling. Slowly cool the billet after continuous casting in a natural environment, and ensure that the cooling time to room temperature exceeds 24 hours, effectively remove the hydrogen in the billet and reduce internal stress. Heat the naturally cooled billet to 1300℃ and keep it for 35 minutes for austenitization to ensure the uniformity of the internal temperature and chemical composition of the billet. Control the heating rate not to exceed 330℃ / h to avoid overheating or overburning.

[0047] After testing, the average grain size of the continuous casting billet finally obtained in this comparative example is 220 μm. The excessive addition of titanium leads to the precipitation of coarse titanium carbides / nitrides, and the grain boundary pinning effect is significantly reduced.

[0048] Comparative Example 4 Molten iron, scrap steel and necessary alloying elements (excluding Mo and Cr) are melted in a converter for preliminary smelting to obtain molten steel. The molten steel is refined. During the refining process, the molten steel is subjected to preliminary chemical composition analysis, and it is determined that the initial titanium content is 0.05%, which does not meet the requirements. Ferro-titanium alloy (FeTi50) is added to the refining furnace in the form of fine powder, and FeTi50 is fully stirred to ensure uniform distribution of the titanium alloy. The refining temperature is controlled to be 1600℃. After argon stirring and vacuum treatment, the sample is taken again for analysis to confirm that the titanium content has been adjusted to 0.13%. The molten steel is vacuum treated so that the weight proportion of carbon in the molten steel is 0.25% and the weight proportion of nitrogen is 0.008%. The final component analysis is performed before steelmaking to ensure that the weight proportion of each component in the molten steel meets the following requirements: C: 0.25%; Si: 2.5%; Mn: 1.00%; N: 0.008%; Ti: 0.13%; the remainder is Fe and unavoidable impurities. The refined molten steel is continuously cast to obtain continuous casting billets. During the continuous casting process, the flow rate of cooling water and the nozzle layout are adjusted to control the cooling rate at 300℃ / s to promote the formation of fine equiaxed crystals. The pulling speed and cooling system of the continuous casting machine are accurately controlled to ensure that the grain size of the continuous casting billet is uniform and small, and rapid cooling is achieved. The billet after continuous casting is slowly cooled in a natural environment to ensure that the cooling time to room temperature exceeds 24 hours, effectively removing hydrogen from the billet and reducing internal stress. The naturally cooled billet is heated to 1300℃ and maintained for 35 minutes for austenitization to ensure the uniformity of the internal temperature and chemical composition of the billet. The heating rate is controlled not to exceed 330℃ / h to avoid overheating or overburning.

[0049] After testing, the average grain size of the continuous casting billet finally obtained in this comparative example is 130 μm, lacking the strengthening effect of Mo and Cr alloy elements, and its grain refining effect is weakened.

[0050] Comparative Example 5 Molten iron, scrap steel and necessary alloying elements are melted in a converter for preliminary smelting to obtain molten steel. The molten steel is refined. During the refining process, the molten steel is subjected to a preliminary chemical composition analysis, and it is determined that the initial titanium content is 0.05%, which does not meet the requirements. Add FeTi50 (ferrotitanium alloy) to the refining furnace in the form of fine powder and stir it thoroughly to ensure that the titanium alloy is evenly distributed. The refining temperature is controlled at 1600°C. After argon stirring and vacuum treatment, the sample is taken again for analysis to confirm that the titanium content has been adjusted to 0.13%. The molten steel is vacuum treated so that the weight proportion of carbon in the molten steel is 0.25% and the weight proportion of nitrogen in the molten steel is 0.008%. Before tapping, the final composition analysis is carried out to ensure that the weight proportion of each component in the molten steel meets the following requirements: C: 0.25%; Si: 2.5%; Mn: 1.00%; Cr: 0.80%; Mo: 0.45%; N: 0.008%; Ti: 0.13%; the remainder is Fe and unavoidable impurities. The refined molten steel is continuously cast to obtain a continuous casting billet. During the continuous casting process, the flow rate of cooling water and the nozzle layout are adjusted to control the cooling rate at 300℃ / s to promote the formation of fine equiaxed crystals. The pulling speed and cooling system of the continuous casting machine are accurately controlled to ensure that the grain size of the continuous casting billet is uniform and small, and rapid cooling is achieved. The continuously cast billet is slowly cooled in a natural environment to ensure that the cooling time to room temperature exceeds 24 hours, effectively removing hydrogen from the billet and reducing internal stress. The naturally cooled billet is heated to 1300℃ and maintained for 150 minutes for austenitization. The heating rate is controlled not to exceed 330℃ / h to avoid overheating or overburning.

[0051] After testing, the average grain size of the continuous casting billet finally obtained in this comparative example is 300 μm, and the grain size is coarse.

[0052] The above-mentioned embodiments only express the implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A method for refining the original austenite grains of a continuous casting billet of a bainite rail, It is characterized in that The following steps are involved: Step S1: Preliminary smelting of raw materials to obtain molten steel; Step S2: refining the molten steel, during which the titanium content is precisely controlled so that the weight proportion of titanium in the molten steel is 0.08%-0.13%, and vacuum treating the molten steel so that the weight proportion of carbon in the molten steel is 0.21%-0.25%, and the weight proportion of nitrogen in the molten steel is 0.005%-0.008%; Step S3: continuously casting the refined molten steel to obtain a continuously cast billet; Step S4: naturally cooling the continuous casting billet to remove hydrogen until the temperature reaches room temperature; Step S5: reheating the cooled continuous casting billet for austenitization to obtain a continuous casting billet with refined original austenite grains.

2. The method according to claim 1, It is characterized in that In step S2, the precise control of the titanium content includes: Step S2-1: before the refining, performing an initial component analysis on the molten steel to determine the current titanium content; Step S2-2: Calculate the amount of titanium alloy to be added based on the desired final chemical composition and initial composition analysis; Step S2-3: adding titanium alloy to the molten steel according to the required amount of titanium alloy.

3. The method according to claim 2, It is characterized in that In step S2-3, stirring operation is adopted when adding the titanium alloy, and the titanium alloy is ferrotitanium alloy.

4. The method according to claim 2, It is characterized in that Step S2 also includes: Step S2-4: After adding the titanium alloy, a secondary component analysis is performed to verify whether the titanium content reaches a predetermined target. If not, fine-tuning is performed by further adding titanium alloy or adjusting process parameters.

5. The method according to claim 1, It is characterized in that In step S2, the refining temperature is controlled at 1400-1600°C.

6. The method according to claim 1, It is characterized in that Step S2 also includes performing a final component analysis before the refining is completed, and ensuring that the weight ratio of each component in the molten steel meets the following requirements before steel is tapped: C: 0.21%~0.25%; Si: 2.0%~2.5%; Mn: 0.60%~1.00%; Cr: 0.60%~0.80%; Mo: 0.40%~0.45%; N: 0.005%~0.008%; Ti: 0.08%~0.13%; the balance is Fe and unavoidable impurities.

7. The method according to claim 6, It is characterized in that When tapping, the titanium, carbon and nitrogen in the molten steel satisfy the following chemical equivalent ratio: Ti / C is 3.95-4.00, and Ti / N≤3.

42.

8. The method according to claim 1, It is characterized in that In step S3, the cooling rate is controlled to be 200-300°C / s during the continuous casting process.

9. The method according to claim 1, It is characterized in that In step S4, the cooling time is not less than 24 hours.

10. The method according to claim 9, It is characterized in that In step S5, the heating temperature is 1200-1300°C.