Low-nickel heat-resistant cast steel and preparation method thereof

Through the preparation method of low-nickel heat-resistant cast steel, combined with specific element combinations and microalloyization technology, the problems of insufficient performance and high cost of exhaust manifold materials under high temperature conditions are solved, and the high temperature mechanical properties and service life are achieved. The improvement meets the operating temperature requirements of 900℃ and reduces production costs.

CN118996257APending Publication Date: 2024-11-22JIANGYIN HONGCHUANG CASTING
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411103871.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing exhaust manifold materials have insufficient performance under high temperature conditions, especially high Ni ductile iron materials have high cost and do not meet the working requirements of exhaust manifolds. Low-nickel heat-resistant cast steels need to be developed to reduce costs and improve performance.

Method used

The preparation method of low nickel heat-resistant cast steel is adopted, and the elements are combined in a specific proportion (C: 0.2-0.5%, Si: 1.0-1.5%, Mn: 0.8-1.0%, Cr: 19-21%, Ni: 1.0-1.0- 3.0% etc.) and microalloyation technology, combined with gas carbon-nitrogen co-permeable heat treatment, new multi-alloyed heat-resistant cast steel materials such as ZG25Cr20Ni2Si2V(C) were prepared.

Benefits of technology

It achieves mechanical properties and service life exceeds vanadium cast iron (QTRSi4MoV-Q) at room temperature and high temperature, meets the mechanical properties requirements of maximum operating temperature of 900℃, and is better than the welding performance of cast iron, reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004990152020000101
    Figure BDA0004990152020000101
  • Figure BDA0004990152020000111
    Figure BDA0004990152020000111
Patent Text Reader

Abstract

The invention relates to the field of heat-resistant steel materials, and particularly discloses low-nickel heat-resistant cast steel and a preparation method thereof, and the nickel element in the low-nickel heat-resistant cast steel only accounts for 1.0-3.0% of the total substance. According to the low-nickel heat-resistant steel, intergranular strengthening, high-temperature oxidation resistance, high-temperature corrosion resistance, creep resistance and the like are achieved through a microalloying method, the effects that the normal-temperature and high-temperature mechanical properties and the service life completely exceed the performance indexes of vanadium cast iron (QTRSi4MoV-Q) are achieved, the mechanical property requirement that the highest working temperature can reach 900 DEG C is met, the low-nickel heat-resistant steel can replace the vanadium cast iron (QTRSi4MoV-Q), and the service life of the low-nickel heat-resistant steel is prolonged. The material becomes a novel material for manufacturing the high-temperature exhaust manifold.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of heat-resistant steel materials, in particular to low-nickel heat-resistant cast steel and a preparation method thereof. Background Art

[0002] The exhaust manifold is a pipe that guides the exhaust gas from each cylinder of the engine into the main pipe. It has a complex structure and harsh working conditions. Therefore, the material used to manufacture the exhaust manifold must have good high-temperature mechanical properties, thermal fatigue resistance, oxidation resistance, corrosion resistance, and growth resistance. Among them, cast exhaust manifolds have good processing and molding properties and low cost advantages and are widely used. With the advancement of technology, the materials used for casting exhaust manifolds have also experienced the development of ordinary gray iron → ordinary ductile iron → ordinary vermicular iron → SiMo ductile iron → SiMo vermicular iron → high Ni ductile iron. However, Ni is expensive, and the use of high Ni ductile iron materials will increase the production cost of enterprises. Some manufacturers use vanadium cast iron (QTRSi4MoV-Q) to cast exhaust manifolds, but the maximum operating temperature of this material is 800°C, which cannot fully meet the working performance of the exhaust manifold. Therefore, it is necessary to develop a new type of heat-resistant cast steel with low Ni content and that can meet the working performance indicators of the exhaust manifold. Summary of the invention

[0003] The purpose of the present invention is to provide a low-nickel heat-resistant cast steel and a preparation method thereof, so as to reduce the Ni content in the heat-resistant cast steel, thereby reducing the production cost of the enterprise, meeting the working performance indicators of the exhaust manifold while solving the problem of high production cost of the exhaust manifold.

[0004] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0005] The invention discloses a low-nickel heat-resistant cast steel. The mass fractions of the elements in the low-nickel heat-resistant cast steel are as follows: C: 0.2-0.5%, Si: 1.0-1.5%, Mn: 0.8-1.0%, Cr: 19-21%, Ni: 1.0-3.0%, Co: 0.14-0.20%, V: 0.15-0.20%, Nb: 0.35-0.45%, P≤0.04%, S≤0.03%, Mo≤0.5%, Te≤0.005%, rare earth elements≤0.05%, and the balance is iron.

[0006] As a limitation of the present invention, the raw materials for preparing the low-nickel heat-resistant steel include: the rare earth element contained in the low-nickel heat-resistant steel is one of Ce or Y.

[0007] A method for preparing low-nickel heat-resistant cast steel, the preparation method comprising:

[0008] The 304 scrap steel is heated and melted into molten steel, and after the molten steel is melted, ferrochrome, pure nickel, ferromolybdenum and ferrocobalt are added in sequence at 1700-1710°C for smelting, and a slag remover is added during smelting to remove slag. Before the molten steel is taken out of the furnace, ferroniobium, ferrovanadium and a deoxidizer are added for deoxidation. The molten steel is taken out of the furnace at 1680-1700°C, poured into a ladle, and ferrotellurium, rare earth mineralization and a deoxidizer are added, and the molten steel is allowed to stand, and the molten steel is cast and formed at 1580-1620°C, and the molten steel is naturally cooled and then polished to obtain a heat-resistant cast steel part;

[0009] The heat-resistant cast steel parts are heat treated by gas carbonitriding. The heat-resistant cast steel parts are placed in a furnace, propane, methanol, nitrogen and ammonia are added for carbonitriding, and then quenched with quenching oil after carbonitriding. After quenching, the steel parts are cleaned, cold-treated with liquid nitrogen, and then low-temperature tempering and cooling are performed to obtain low-nickel heat-resistant cast steel.

[0010] As a limitation of the present invention, the deoxidizer is SiCaBa deoxidizer and ReSiCaMn deoxidizer, wherein the SiCaBa deoxidizer is added in the furnace and the ReSiCaMn deoxidizer is added in the ladle.

[0011] As a limitation of the present invention, the time for adding ferroniobium and ferrovanadium into the furnace is 14 to 16 minutes before the molten steel is discharged from the furnace.

[0012] As a limitation of the present invention, the mass of the deoxidizer added before the furnace is 0.1-0.3% of the total mass of the molten steel in the furnace, and the time is 4-6 minutes before the furnace is taken out.

[0013] As a limitation of the present invention, the mass fraction of tellurium in the ferrotelluride added to the ladle is 0.005-0.006% of the total mass of the molten steel in the ladle, and the mass fraction of cerium in the ferrocerium is 0.015-0.017% of the total mass of the molten steel in the ladle.

[0014] As a limitation of the present invention, the carbonitriding temperature is 800-900°C, the carbonitriding potential is 1.10-1.30%, and the ammonia flow rate is 0.17-0.19 m 3 / h.

[0015] As a limitation of the present invention, the low-nickel heat-resistant cast steel can be used for casting automobile exhaust manifolds.

[0016] The beneficial effects achieved by the present invention are:

[0017] Research has found that in heat-resistant cast steel, chromium depletion is the main factor leading to its performance degradation. Carbon reacts with chromium in the alloy to form chromium carbide (Cr3C2), which makes the grain boundaries chromium-depleted (the grain boundary layer is less than 17%), thereby reducing the alloy's oxidation resistance and high-temperature strength. In a high-chromium cast iron alloy with a chromium content of 20%, when the carbon content is below 2.4%, the alloy's oxidation resistance decreases with the increase of carbon content. Therefore, appropriately reducing the carbon content is beneficial to improving the alloy's oxidation resistance, but high-chromium cast iron that only reduces carbon cannot solve the mechanical properties of the exhaust manifold under high temperature conditions. Based on this, heat-resistant cast steel becomes the only choice.

[0018] The present invention is based on adding 1.0-3.0% nickel to a heat-resistant steel alloy with a carbon content of 0.2-0.5% and a chromium content of 19.0-21.0%, and a new multi-element alloyed heat-resistant cast steel material ZG25Cr20Ni2Si2V(C) is developed by a microalloying method. The material achieves intergranular strengthening, high-temperature oxidation resistance, high-temperature corrosion resistance and creep resistance through the microalloying method, and achieves room temperature and high temperature mechanical properties, and the service life completely surpasses the performance index of vanadium cast iron (QTRSi4MoV-Q), and meets the mechanical property requirements of the maximum working temperature of 900°C. In addition, the welding type of cast steel material is completely better than that of cast iron material. Therefore, the low-nickel heat-resistant cast steel ZG25Cr20Ni2Si2V(C) of the present invention can completely replace vanadium cast iron (QTRSi4MoV-Q) (maximum working temperature 800°C), and becomes a new material for manufacturing high-temperature exhaust manifolds. DETAILED DESCRIPTION

[0019] The following is a preferred implementation of the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiment of the present invention, not all of the embodiments. For ordinary technicians in this technical field, all other embodiments obtained by ordinary technicians in this field without creative work without departing from the principle of the embodiment of the present invention are within the scope of protection of the present invention.

[0020] Quenching oil (flash point: 257°C, maximum cooling rate: 87°C / s) was provided by Shandong Lite.

[0021] Example 1: A low nickel heat-resistant cast steel

[0022] The mass fractions of each element in low nickel heat-resistant cast steel are: C: 0.2%, Si: 1.0%, Mn: 0.8%, Cr: 19%, Ni: 3.0%, Co: 0.14%, V: 0.15%, Nb: 0.35%, P: 0.04%, S: 0.03%, Mo: 0.5%, Te: 0.005%, Ce: 0.015%, and the balance is iron.

[0023] A method for preparing low-nickel heat-resistant cast steel, the preparation method comprising:

[0024] Weigh the raw materials according to the mass fraction of each element in the above low-nickel heat-resistant cast steel for batching, heat up and melt 304 scrap steel into molten steel, add ferrochrome and pure nickel in sequence at 1705°C after the molten steel is clear, add 1% perlite of the total weight of the raw materials to remove slag after the ferrochrome and pure nickel are melted, add ferromolybdenum and ferrocobalt in sequence after the slag removal, add 1% perlite of the total weight of the raw materials to remove slag again after the ferromolybdenum and ferrocobalt are melted, and continue to smelt the molten steel after the slag removal;

[0025] 15 minutes before the molten steel is discharged from the furnace, ferroniobium and ferrovanadium are added in sequence. After the ferroniobium and ferrovanadium are melted, 1% of the total weight of the raw materials are added again to remove the slag. 5 minutes before the molten steel is discharged from the furnace, 0.2% of the total weight of the molten steel in the furnace is added as a SiCaBa deoxidizer for deoxidation. The molten steel is discharged from the furnace at 1690°C and poured into a ladle.

[0026] Adding ferrotelluride with a tellurium element mass fraction of 0.005% of the total mass of the molten steel in the ladle, ferrocerium with a cerium element mass fraction of 0.015% of the total mass of the molten steel in the ladle, and a ReSiCaMn deoxidizer with a total mass of 0.15% of the total mass of the molten steel in the ladle to the molten steel in the ladle, leaving it to stand, casting the molten steel at 1600° C., and grinding it after natural cooling to obtain a heat-resistant cast steel part;

[0027] The heat-resistant steel castings were heat treated by gas carbonitriding. The heat-resistant steel castings were placed in a furnace and propane, methanol, nitrogen and ammonia were added. Carbonitriding was performed at 820°C. The carburizing potential was 1.18% and the ammonia flow rate was 0.18m 3 / h. After carbonitriding, the steel parts are isothermally quenched with quenching oil at 110°C. After quenching, the steel parts are cleaned, and the steel parts are cold treated at -78°C for 1h with liquid nitrogen, and then low-temperature tempering is performed at 180°C for 3h. After cooling, low-nickel heat-resistant cast steel is obtained.

[0028] Example 2: A low nickel heat resistant cast steel

[0029] The mass fractions of each element in low nickel heat-resistant cast steel are: C: 0.3%, Si: 1.2%, Mn: 0.8%, Cr: 20%, Ni: 2.0%, Co: 0.15%, V: 0.17%, Nb: 0.38%, P: 0.03%, S: 0.025%, Mo: 0.4%, Te: 0.005%, Ce: 0.015%, and the balance is iron.

[0030] A method for preparing low-nickel heat-resistant cast steel, the preparation method comprising:

[0031] Weigh the raw materials according to the mass fraction of each element in the above low-nickel heat-resistant cast steel for batching, heat up and melt 304 scrap steel into molten steel, add ferrochrome and pure nickel in sequence at 1705°C after the molten steel is clear, add 1% perlite of the total weight of the raw materials to remove slag after the ferrochrome and pure nickel are melted, add ferromolybdenum and ferrocobalt in sequence after the slag removal, add 1% perlite of the total weight of the raw materials to remove slag again after the ferromolybdenum and ferrocobalt are melted, and continue to smelt the molten steel after the slag removal;

[0032] 15 minutes before the molten steel is discharged from the furnace, ferroniobium and ferrovanadium are added in sequence. After the ferroniobium and ferrovanadium are melted, 1% of the total weight of the raw materials are added again to remove the slag. 5 minutes before the molten steel is discharged from the furnace, 0.2% of the total weight of the molten steel in the furnace is added as a SiCaBa deoxidizer for deoxidation. The molten steel is discharged from the furnace at 1690°C and poured into a ladle.

[0033] Adding ferrotelluride with a tellurium element mass fraction of 0.005% of the total mass of the molten steel in the ladle, ferrocerium with a cerium element mass fraction of 0.015% of the total mass of the molten steel in the ladle, and a ReSiCaMn deoxidizer with a total mass of 0.15% of the total mass of the molten steel in the ladle to the molten steel in the ladle, leaving it to stand, casting the molten steel at 1600° C., and grinding it after natural cooling to obtain a heat-resistant cast steel part;

[0034] The heat-resistant steel castings were heat treated by gas carbonitriding. The heat-resistant steel castings were placed in a furnace and propane, methanol, nitrogen and ammonia were added. Carbonitriding was performed at 820°C. The carburizing potential was 1.18% and the ammonia flow rate was 0.18m 3 / h. After carbonitriding, the steel parts are isothermally quenched with quenching oil at 110°C. After quenching, the steel parts are cleaned, and the steel parts are cold treated at -78°C for 1h with liquid nitrogen, and then low-temperature tempering is performed at 180°C for 3h. After cooling, low-nickel heat-resistant cast steel is obtained.

[0035] Example 3: A low nickel heat-resistant cast steel

[0036] The mass fractions of each element in low nickel heat-resistant cast steel are: C: 0.3%, Si: 1.2%, Mn: 0.9%, Cr: 21%, Ni: 1.0%, Co: 0.16%, V: 0.17%, Nb: 0.39%, P: 0.035%, S: 0.02%, Mo: 0.3%, Te: 0.005%, Ce: 0.016%, and the balance is iron.

[0037] A method for preparing low-nickel heat-resistant cast steel, the preparation method comprising:

[0038] Weigh the raw materials according to the mass fraction of each element in the above low-nickel heat-resistant cast steel for batching, heat up and melt 304 scrap steel into molten steel, add ferrochrome and pure nickel in sequence at 1705°C after the molten steel is clear, add 1% perlite of the total weight of the raw materials to remove slag after the ferrochrome and pure nickel are melted, add ferromolybdenum and ferrocobalt in sequence after the slag removal, add 1% perlite of the total weight of the raw materials to remove slag again after the ferromolybdenum and ferrocobalt are melted, and continue to smelt the molten steel after the slag removal;

[0039] 15 minutes before the molten steel is discharged from the furnace, ferroniobium and ferrovanadium are added in sequence. After the ferroniobium and ferrovanadium are melted, 1% of the total weight of the raw materials are added again to remove the slag. 5 minutes before the molten steel is discharged from the furnace, 0.2% of the total weight of the molten steel in the furnace is added as a SiCaBa deoxidizer for deoxidation. The molten steel is discharged from the furnace at 1690°C and poured into a ladle.

[0040] Adding ferrotelluride with a tellurium element mass fraction of 0.005% of the total mass of the molten steel in the ladle, ferrocerium with a cerium element mass fraction of 0.016% of the total mass of the molten steel in the ladle, and a ReSiCaMn deoxidizer with a total mass of 0.15% of the total mass of the molten steel in the ladle to the molten steel in the ladle, leaving it to stand, casting the molten steel at 1600° C., and grinding it after natural cooling to obtain a heat-resistant cast steel part;

[0041] The heat-resistant steel castings were heat treated by gas carbonitriding. The heat-resistant steel castings were placed in a furnace and propane, methanol, nitrogen and ammonia were added. Carbonitriding was performed at 820°C. The carburizing potential was 1.18% and the ammonia flow rate was 0.18m 3 / h. After carbonitriding, the steel parts are isothermally quenched with quenching oil at 110°C. After quenching, the steel parts are cleaned, and the steel parts are cold treated at -78°C for 1h with liquid nitrogen, and then low-temperature tempering is performed at 180°C for 3h. After cooling, low-nickel heat-resistant cast steel is obtained.

[0042] Example 4: A low nickel heat-resistant cast steel

[0043] The mass fractions of each element in low nickel heat-resistant cast steel are: C: 0.4%, Si: 1.0%, Mn: 0.9%, Cr: 19%, Ni: 3.0%, Co: 0.18%, V: 1.15%, Nb: 0.4%, P: 0.02%, S: 0.02%, Mo: 0.5%, Te: 0.005%, Ce: 0.016%, and the balance is iron.

[0044] A method for preparing low-nickel heat-resistant cast steel, the preparation method comprising:

[0045] Weigh the raw materials according to the mass fraction of each element in the above low-nickel heat-resistant cast steel for batching, heat up and melt 304 scrap steel into molten steel, add ferrochrome and pure nickel in sequence at 1705°C after the molten steel is clear, add 1% perlite of the total weight of the raw materials to remove slag after the ferrochrome and pure nickel are melted, add ferromolybdenum and ferrocobalt in sequence after the slag removal, add 1% perlite of the total weight of the raw materials to remove slag again after the ferromolybdenum and ferrocobalt are melted, and continue to smelt the molten steel after the slag removal;

[0046] 15 minutes before the molten steel is discharged from the furnace, ferroniobium and ferrovanadium are added in sequence. After the ferroniobium and ferrovanadium are melted, 1% of the total weight of the raw materials are added again to remove the slag. 5 minutes before the molten steel is discharged from the furnace, 0.2% of the total weight of the molten steel in the furnace is added as a SiCaBa deoxidizer for deoxidation. The molten steel is discharged from the furnace at 1690°C and poured into a ladle.

[0047] Adding ferrotelluride with a tellurium element mass fraction of 0.005% of the total mass of the molten steel in the ladle, ferrocerium with a cerium element mass fraction of 0.016% of the total mass of the molten steel in the ladle, and a ReSiCaMn deoxidizer with a total mass of 0.15% of the total mass of the molten steel in the ladle to the molten steel in the ladle, leaving it to stand, casting the molten steel at 1600° C., and grinding it after natural cooling to obtain a heat-resistant cast steel part;

[0048] The heat-resistant steel castings were heat treated by gas carbonitriding. The heat-resistant steel castings were placed in a furnace and propane, methanol, nitrogen and ammonia were added. Carbonitriding was performed at 820°C. The carburizing potential was 1.18% and the ammonia flow rate was 0.18m 3 / h. After carbonitriding, the steel parts are isothermally quenched with quenching oil at 110°C. After quenching, the steel parts are cleaned, and the steel parts are cold treated at -78°C for 1h with liquid nitrogen, and then low-temperature tempering is performed at 180°C for 3h. After cooling, low-nickel heat-resistant cast steel is obtained.

[0049] Example 5: A low nickel heat-resistant cast steel

[0050] The mass fractions of each element in low nickel heat-resistant cast steel are: C: 0.2%, Si: 1.0-1.5%, Mn: 1.0%, Cr: 20%, Ni: 2.0%, Co: 0.20%, V: 0.15%, Nb: 0.42%, P: 0.01%, S: 0.03%, Mo: 0.4%, Te: 0.005%, Ce: 0.0017%, and the balance is iron.

[0051] A method for preparing low-nickel heat-resistant cast steel, the preparation method comprising:

[0052] Weigh the raw materials according to the mass fraction of each element in the above low-nickel heat-resistant cast steel for batching, heat up and melt 304 scrap steel into molten steel, add ferrochrome and pure nickel in sequence at 1705°C after the molten steel is clear, add 1% perlite of the total weight of the raw materials to remove slag after the ferrochrome and pure nickel are melted, add ferromolybdenum and ferrocobalt in sequence after the slag removal, add 1% perlite of the total weight of the raw materials to remove slag again after the ferromolybdenum and ferrocobalt are melted, and continue to smelt the molten steel after the slag removal;

[0053] 15 minutes before the molten steel is discharged from the furnace, ferroniobium and ferrovanadium are added in sequence. After the ferroniobium and ferrovanadium are melted, 1% of the total weight of the raw materials are added again to remove the slag. 5 minutes before the molten steel is discharged from the furnace, 0.2% of the total weight of the molten steel in the furnace is added as a SiCaBa deoxidizer for deoxidation. The molten steel is discharged from the furnace at 1690°C and poured into a ladle.

[0054] Adding ferrotelluride with a tellurium element mass fraction of 0.005% of the total mass of the molten steel in the ladle, ferrocerium with a cerium element mass fraction of 0.017% of the total mass of the molten steel in the ladle, and a ReSiCaMn deoxidizer with a total mass of 0.15% of the total mass of the molten steel in the ladle to the molten steel in the ladle, leaving it to stand, casting the molten steel at 1600° C., and grinding it after natural cooling to obtain a heat-resistant cast steel part;

[0055] The heat-resistant steel castings were heat treated by gas carbonitriding. The heat-resistant steel castings were placed in a furnace and propane, methanol, nitrogen and ammonia were added. Carbonitriding was performed at 820°C. The carburizing potential was 1.18% and the ammonia flow rate was 0.18m 3 / h. After carbonitriding, the steel parts are isothermally quenched with quenching oil at 110°C. After quenching, the steel parts are cleaned, and the steel parts are cold treated at -78°C for 1h with liquid nitrogen, and then low-temperature tempering is performed at 180°C for 3h. After cooling, low-nickel heat-resistant cast steel is obtained.

[0056] Example 6: A low nickel heat-resistant cast steel

[0057] The mass fractions of each element in low nickel heat-resistant cast steel are: C: 0.5%, Si: 1.0%, Mn: 1.0%, Cr: 21%, Ni: 1.0%, Co: 0.18%, V: 0.20%, Nb: 0.35%, P: 0.015%, S: 0.025%, Mo: 0.3%, Te: 0.006%, Ce: 0.017%, and the balance is iron.

[0058] A method for preparing low-nickel heat-resistant cast steel, the preparation method comprising:

[0059] Weigh the raw materials according to the mass fraction of each element in the above low-nickel heat-resistant cast steel for batching, heat up and melt 304 scrap steel into molten steel, add ferrochrome and pure nickel in sequence at 1705°C after the molten steel is clear, add 1% perlite of the total weight of the raw materials to remove slag after the ferrochrome and pure nickel are melted, add ferromolybdenum and ferrocobalt in sequence after the slag removal, add 1% perlite of the total weight of the raw materials to remove slag again after the ferromolybdenum and ferrocobalt are melted, and continue to smelt the molten steel after the slag removal;

[0060] 15 minutes before the molten steel is discharged from the furnace, ferroniobium and ferrovanadium are added in sequence. After the ferroniobium and ferrovanadium are melted, 1% of the total weight of the raw materials are added again to remove the slag. 5 minutes before the molten steel is discharged from the furnace, 0.2% of the total weight of the molten steel in the furnace is added as a SiCaBa deoxidizer for deoxidation. The molten steel is discharged from the furnace at 1690°C and poured into a ladle.

[0061] Adding ferrotelluride with a tellurium element mass fraction of 0.005% of the total mass of the molten steel in the ladle, ferrocerium with a cerium element mass fraction of 0.017% of the total mass of the molten steel in the ladle, and a ReSiCaMn deoxidizer with a total mass of 0.15% of the total mass of the molten steel in the ladle to the molten steel in the ladle, leaving it to stand, casting the molten steel at 1600° C., and grinding it after natural cooling to obtain a heat-resistant cast steel part;

[0062] The heat-resistant steel castings were heat treated by gas carbonitriding. The heat-resistant steel castings were placed in a furnace and propane, methanol, nitrogen and ammonia were added. Carbonitriding was performed at 820°C. The carburizing potential was 1.18% and the ammonia flow rate was 0.18m 3 / h. After carbonitriding, the steel parts are isothermally quenched with quenching oil at 110°C. After quenching, the steel parts are cleaned, and the steel parts are cold treated at -78°C for 1h with liquid nitrogen, and then low-temperature tempering is performed at 180°C for 3h. After cooling, low-nickel heat-resistant cast steel is obtained.

[0063] Based on Example 1, control experiments were carried out, specifically Comparative Example 1, Comparative Example 2, and Comparative Example 3, as described below:

[0064] Comparative Example 1: Ferrotellurium and ferrocerium were added into the furnace instead, and the other conditions were the same as those in Example 1, specifically:

[0065] A low nickel heat-resistant cast steel

[0066] The mass fractions of each element in low nickel heat-resistant cast steel are: C: 0.2%, Si: 1.0%, Mn: 0.8%, Cr: 19%, Ni: 3.0%, Co: 0.14%, V: 0.15%, Nb: 0.35%, P: 0.04%, S: 0.03%, Mo: 0.5%, Te: 0.005%, Ce: 0.015%, and the balance is iron.

[0067] A method for preparing low-nickel heat-resistant cast steel, the preparation method comprising:

[0068] Weigh the raw materials according to the mass fraction of each element in the above low-nickel heat-resistant cast steel for batching, heat up and melt 304 scrap steel into molten steel, add ferrochrome and pure nickel in sequence at 1705°C after the molten steel is clear, add 1% perlite of the total weight of the raw materials to remove slag after the ferrochrome and pure nickel are melted, add ferromolybdenum and ferrocobalt in sequence after the slag removal, add 1% perlite of the total weight of the raw materials to remove slag again after the ferromolybdenum and ferrocobalt are melted, and continue to smelt the molten steel after the slag removal;

[0069] 15 minutes before the molten steel is discharged from the furnace, ferroniobium and ferrovanadium are added in sequence. After the ferroniobium and ferrovanadium are melted, 1% of the total mass of the raw materials perlite is added again to remove the slag. After the slag is removed, ferrotelluride with a tellurium element mass fraction of 0.005% of the total mass of the molten steel and ferrocerium with a cerium element mass fraction of 0.015% of the total mass of the molten steel are added. 5 minutes before the molten steel is discharged from the furnace, 0.2% of the total mass of the molten steel in the furnace is added as a SiCaBa deoxidizer for deoxidation. The molten steel is discharged from the furnace at 1690°C and poured into a ladle.

[0070] Adding 0.15% of the total mass of the molten steel in the ladle to the molten steel in the ladle is a ReSiCaMn deoxidizer, and the molten steel is allowed to stand, and the molten steel is cast at 1600° C. After natural cooling, the molten steel is polished to obtain a heat-resistant steel casting;

[0071] The heat-resistant steel castings were heat treated by gas carbonitriding. The heat-resistant steel castings were placed in a furnace and propane, methanol, nitrogen and ammonia were added. Carbonitriding was performed at 820°C. The carburizing potential was 1.18% and the ammonia flow rate was 0.18m 3 / h. After carbonitriding, the steel parts are isothermally quenched with quenching oil at 110°C. After quenching, the steel parts are cleaned, and the steel parts are cold treated at -78°C for 1h with liquid nitrogen, and then low-temperature tempering is performed at 180°C for 3h. After cooling, low-nickel heat-resistant cast steel is obtained.

[0072] Comparative Example 2: No ferrotelluride was added to the ladle, and the remaining conditions were the same as those in Example 1, specifically:

[0073] A low nickel heat-resistant cast steel

[0074] The mass fractions of each element in low nickel heat-resistant cast steel are: C: 0.2%, Si: 1.0%, Mn: 0.8%, Cr: 19%, Ni: 3.0%, Co: 0.14%, V: 0.15%, Nb: 0.35%, P: 0.04%, S: 0.03%, Mo: 0.5%, Ce: 0.015%, and the balance is iron.

[0075] A method for preparing low-nickel heat-resistant cast steel, the preparation method comprising:

[0076] Weigh the raw materials according to the mass fraction of each element in the above low-nickel heat-resistant cast steel for batching, heat up and melt 304 scrap steel into molten steel, add ferrochrome and pure nickel in sequence at 1705°C after the molten steel is clear, add 1% perlite of the total weight of the raw materials to remove slag after the ferrochrome and pure nickel are melted, add ferromolybdenum and ferrocobalt in sequence after the slag removal, add 1% perlite of the total weight of the raw materials to remove slag again after the ferromolybdenum and ferrocobalt are melted, and continue to smelt the molten steel after the slag removal;

[0077] 15 minutes before the molten steel is discharged from the furnace, ferroniobium and ferrovanadium are added in sequence. After the ferroniobium and ferrovanadium are melted, 1% of the total weight of the raw materials are added again to remove the slag. 5 minutes before the molten steel is discharged from the furnace, 0.2% of the total weight of the molten steel in the furnace is added as a SiCaBa deoxidizer for deoxidation. The molten steel is discharged from the furnace at 1690°C and poured into a ladle.

[0078] Adding ferrocerium whose total mass of cerium element is 0.015% of the total mass of molten steel in the ladle and ReSiCaMn deoxidizer whose total mass of molten steel in the ladle is 0.15% of the total mass of molten steel in the ladle to the molten steel in the ladle, leaving it to stand, casting the molten steel at 1600° C., and grinding it after natural cooling to obtain a heat-resistant cast steel part;

[0079] The heat-resistant steel castings were heat treated by gas carbonitriding. The heat-resistant steel castings were placed in a furnace and propane, methanol, nitrogen and ammonia were added. Carbonitriding was performed at 820°C. The carburizing potential was 1.18% and the ammonia flow rate was 0.18m 3 / h. After carbonitriding, the steel parts are isothermally quenched with quenching oil at 110°C. After quenching, the steel parts are cleaned, and the steel parts are cold treated at -78°C for 1h with liquid nitrogen, and then low-temperature tempering is performed at 180°C for 3h. After cooling, low-nickel heat-resistant cast steel is obtained.

[0080] Comparative Example 3: No ferrocerium was added to the ladle, and the remaining conditions were the same as those in Example 1, specifically:

[0081] A low nickel heat-resistant cast steel

[0082] The mass fractions of each element in low nickel heat-resistant cast steel are: C: 0.2%, Si: 1.0%, Mn: 0.8%, Cr: 19%, Ni: 3.0%, Co: 0.14%, V: 0.15%, Nb: 0.35%, P: 0.04%, S: 0.03%, Mo: 0.5%, Te: 0.005%, and the balance is iron.

[0083] A method for preparing low-nickel heat-resistant cast steel, the preparation method comprising:

[0084] Weigh the raw materials according to the mass fraction of each element in the above low-nickel heat-resistant cast steel for batching, heat up and melt 304 scrap steel into molten steel, add ferrochrome and pure nickel in sequence at 1705°C after the molten steel is clear, add 1% perlite of the total weight of the raw materials to remove slag after the ferrochrome and pure nickel are melted, add ferromolybdenum and ferrocobalt in sequence after the slag removal, add 1% perlite of the total weight of the raw materials to remove slag again after the ferromolybdenum and ferrocobalt are melted, and continue to smelt the molten steel after the slag removal;

[0085] 15 minutes before the molten steel is discharged from the furnace, ferroniobium and ferrovanadium are added in sequence. After the ferroniobium and ferrovanadium are melted, 1% of the total weight of the raw materials are added again to remove the slag. 5 minutes before the molten steel is discharged from the furnace, 0.2% of the total weight of the molten steel in the furnace is added as a SiCaBa deoxidizer for deoxidation. The molten steel is discharged from the furnace at 1690°C and poured into a ladle.

[0086] Adding tellurium iron with a tellurium element mass fraction of 0.005% of the total mass of the molten steel in the ladle and ReSiCaMn deoxidizer with a mass fraction of 0.15% of the total mass of the molten steel in the ladle to the molten steel in the ladle, leaving it to stand, casting the molten steel at 1600° C., and grinding it after natural cooling to obtain a heat-resistant cast steel part;

[0087] The heat-resistant steel castings were heat treated by gas carbonitriding. The heat-resistant steel castings were placed in a furnace and propane, methanol, nitrogen and ammonia were added. Carbonitriding was performed at 820°C. The carburizing potential was 1.18% and the ammonia flow rate was 0.18m 3 / h. After carbonitriding, the steel parts are isothermally quenched with quenching oil at 110°C. After quenching, the steel parts are cleaned, and the steel parts are cold treated at -78°C for 1h with liquid nitrogen, and then low-temperature tempering is performed at 180°C for 3h. After cooling, low-nickel heat-resistant cast steel is obtained.

[0088] Detection experiment:

[0089] Preparation of samples: The samples required for each test were prepared according to the preparation method of low-nickel heat-resistant steel provided in Examples 1-6 and Comparative Examples 1-3. At the same time, a sample was prepared using vanadium cast iron (QTRSi4MoV-Q), which was recorded as Comparative Example 4.

[0090] Room temperature mechanical properties: The test was carried out in accordance with the "Room temperature tensile test method for metallic materials" (GB / T 228-2002). Each sample was clamped on the chuck of the universal testing machine. After adjusting the force measuring pointer to zero, the testing machine was turned on to measure the tensile strength, yield strength and elongation at break of each sample.

[0091] Hardness: The test is carried out in accordance with the Instrumented Indentation Test for Hardness and Material Parameters of Metallic Materials (GB / T 21238-2008). The sample is fixed on the sample table of the testing machine and the hardness of each sample is measured using a regular square pyramid diamond indenter (Vickers indenter) with an angle of 136° between the two opposite faces at the top.

[0092]

[0093] Mechanical properties at high temperature: According to the “Method for High Temperature Tensile Test of Metallic Materials” (GB / T 4338-2006), each sample was heated to the specified temperature (780℃ and 871℃) and kept at the specified temperature for 10 minutes. After adjusting the zero point of the extensometer, the tensile strength, yield strength and elongation of each sample were measured using an extensometer.

[0094]

[0095] Conclusion: It can be seen from the experiment that the various indicators of Example 1 at room temperature and high temperature are better than those of Comparative Examples 1-3, and the various indicators of each embodiment at room temperature and high temperature are better than those of Comparative Example 4 (vanadium cast iron), achieving the effect of completely surpassing the performance indicators of vanadium cast iron (QTRSi4MoV-Q) in terms of room temperature and high temperature mechanical properties and service life, meeting the mechanical performance requirements of up to 900°C at the highest working temperature, and completely superior to cast iron in the welding type of cast steel. Therefore, it can completely replace vanadium cast iron (QTRSi4MoV-Q) (maximum working temperature 800°C) and become a new material for manufacturing high-temperature exhaust manifolds.

[0096] Finally, it should be noted that the above is only a preferred embodiment of the present invention, but the protection scope of this application is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the spirit and principle of the present invention and within the technical scope disclosed in this application should be included in the protection scope of this application; in the absence of conflict, the embodiments of this application and the features in the embodiments can be combined with each other. Therefore, the protection scope of this application shall be based on the protection scope of the claims.

Claims

1. A low nickel heat-resistant cast steel, characterized in that: The mass fractions of each element in the low nickel heat-resistant cast steel are: C: 0.2-0.5%, Si: 1.0-1.5%, Mn: 0.8-1.0%, Cr: 19-21%, Ni: 1.0-3.0%, Co: 0.14-0.20%, V: 0.15-0.20%, Nb: 0.35-0.45%, P≤0.04%, S≤0.03%, Mo≤0.5%, Te≤0.005%, rare earth elements≤0.05%, and the balance is iron.

2. A low nickel heat-resistant cast steel according to claim 1, characterized in that: The rare earth element contained in low nickel heat-resistant steel is one of Ce or Y.

3. A method for preparing low-nickel heat-resistant cast steel, characterized in that: The preparation method is: The 304 scrap steel is heated and melted into molten steel, and after the molten steel is clear, ferrochrome, pure nickel, ferromolybdenum and ferrocobalt are added in sequence at 1700-1710°C for smelting, and a slag remover is added during smelting to remove slag, and ferroniobium, ferrovanadium and a deoxidizer are added before the molten steel is taken out of the furnace for deoxidation, the molten steel is taken out of the furnace at 1680-1700°C, poured into a ladle, ferrotellurium, ferrocerium and a deoxidizer are added, and the molten steel is allowed to stand, and the molten steel is cast and formed at 1580-1620°C, and the molten steel is naturally cooled and then polished to obtain a heat-resistant steel casting; The heat-resistant cast steel parts are heat treated by gas carbonitriding. The heat-resistant cast steel parts are placed in a furnace, propane, methanol, nitrogen and ammonia are added for carbonitriding, and then quenched with quenching oil after carbonitriding. After quenching, the steel parts are cleaned, cold-treated with liquid nitrogen, and then low-temperature tempering and cooling are performed to obtain low-nickel heat-resistant cast steel.

4. The method for preparing a low-nickel heat-resistant cast steel according to claim 3, characterized in that: The deoxidizers are SiCaBa deoxidizer and ReSiCaMn deoxidizer, wherein the SiCaBa deoxidizer is added in the furnace and the ReSiCaMn deoxidizer is added in the ladle.

5. The method for preparing a low-nickel heat-resistant cast steel according to claim 3, characterized in that: The time for adding ferroniobium and ferrovanadium into the furnace is 14 to 16 minutes before the molten steel is discharged from the furnace.

6. The method for preparing a low-nickel heat-resistant cast steel according to claim 3, characterized in that: The mass of deoxidizer added before taking out of the furnace is 0.1-0.3% of the total mass of molten steel in the furnace, and the time is 4-6 minutes before taking out of the furnace.

7. The method for preparing a low-nickel heat-resistant cast steel according to claim 3, characterized in that: The mass fraction of tellurium element in ferrotelluride added to the ladle is 0.005-0.006% of the total mass of molten steel in the ladle, and the mass fraction of cerium element in ferrocerium is 0.015-0.017% of the total mass of molten steel in the ladle.

8. The method for preparing a low-nickel heat-resistant cast steel according to claim 3, characterized in that: The temperature during carbonitriding is 800-900°C, the carburizing potential is 1.10-1.30%, and the ammonia flow rate is 0.17-0.19m 3 / h.