Preparation method of asphalt-based filler for seamless expansion joint

By using stone, high viscose asphalt, dry elastic enhancer and rut-resistant components to prepare seamless expansion joint asphalt-based filler, the problems of high material costs, cumbersome processes and insufficient low-temperature performance in the prior art are solved, and convenient Efficient preparation of asphalt-based filler and excellent rut resistance and oxidation resistance.

CN119019117APending Publication Date: 2024-11-26Wuhan City Ring Operation and Maintenance Construction Group Co., Ltd.
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411235229.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing seamless expansion joint filling materials are costly, cumbersome, and have poor performance stability. They are prone to flue gas and irritating odors in high-temperature construction, which is not good for construction personnel and lack of low-temperature performance.

Method used

The seamless expansion joint asphalt-based filler is prepared by stone, high-viscosity asphalt, dry elastic enhancer and rut-resistant components. By adding dry elastic enhancer and rut-resistant components, the asphalt-based filler is given excellent rut-resistant resistance. Performance, oxidation resistance and high and low temperature resistance simplify process flow and reduce processing costs.

Benefits of technology

It realizes the convenient and efficient preparation of seamless expansion joint asphalt-based fillers, reduces material costs and processing costs, improves the rut resistance, oxidation resistance and high and low temperature resistance of the fillers, and is suitable for rapid maintenance and new construction projects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005027546980000091
    Figure BDA0005027546980000091
Patent Text Reader

Abstract

The invention relates to the field of building construction, and discloses a preparation method of an asphalt-based filler for a seamless expansion joint, and the asphalt-based filler comprises the following components in parts by weight: 100 parts of stone, 7.5-11.3 parts of high-viscosity asphalt, 0.7-1.2 parts of a dry-method elasticizer, 3.7-6.5 parts of an inorganic filler, and 0.8-1.1 parts of an anti-rutting component. The dry-process elasticizer is prepared by adding an auxiliary agent component into a pre-crushed styrene-butadiene-styrene block copolymer; the anti-rut component comprises the following raw materials in parts by weight: 50-70 parts of modified polyethylene, 5-10 parts of a nano filler, 3-7 parts of a coupling agent and 2-5 parts of a lubricant, and the modified polyethylene is prepared by grafting p-phenylenediamine on the surface of a carbon oxide nanotube and further grafting maleic anhydride grafted polyethylene. Meanwhile, due to the addition of the dry-process elasticizer and the anti-rutting component, the asphalt-based filler is endowed with excellent anti-rutting performance, oxidation resistance and high and low temperature resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building construction, and in particular relates to a method for preparing an asphalt-based filling material for a seamless expansion joint. Background Art

[0002] At present, the commonly used traditional expansion joints are mainly divided into butt joint type, steel support type, plate type, and modular support type. These expansion joints all have concrete structures in the anchoring area, which are prone to vertical deformation during repeated impact loads, damage the flatness of the road surface, and cause cracks in the concrete, which poses a safety hazard. In addition, the maintenance procedures are cumbersome. Seamless expansion joints have the advantages of simple structure, convenient construction, convenient maintenance, and comfortable driving. They are suitable for the maintenance of expansion joints with smaller expansion and contraction and new construction projects.

[0003] Most of the seamless expansion joint filling materials on the current market are foreign products, which are expensive and have poor economic efficiency. Most of the similar domestic products use special asphalt, which requires the modification of common asphalt products. The process is complicated and the performance stability is poor. The processing cost is high. The admixtures used for asphalt modification also have problems such as poor environmental friendliness, which are not suitable for large-scale promotion and use.

[0004] After searching, the patent CN116396014A discloses a rubber powder epoxy asphalt binder and prefabricated structure for expansion joints, its preparation method and application, which uses epoxy resin and rubber powder to modify the base asphalt to enhance the elasticity and strength of the asphalt. However, the rubber powder modifier used in this invention patent is prone to produce smoke and irritating odor during high-temperature construction, which has an adverse effect on construction workers. More importantly, this invention requires shearing, swelling and development of asphalt during the construction of seamless expansion joints, which takes too long and is not suitable for on-site promotion and application.

[0005] Patent CN109534726A discloses a flexible seamless expansion joint material and a preparation method thereof, wherein the main bonding material is a high elastic sealant, and the high elastic sealant is a polymer modified asphalt formed by modifying a high elastic body of a non-rubber polymer on the basis of a matrix asphalt. Obviously, the high elastic sealant uses a variety of polymers to modify asphalt, and the asphalt modification process needs to be completed before construction. Not only is the material cost expensive, but also professional modification equipment is required. The modified asphalt processing also needs to go through multiple processes, such as shearing, swelling, and development, etc. The process is relatively cumbersome and the processing cost is high.

[0006] In addition, the existing technology uses high-viscosity hard asphalt binder, and adds natural asphalt or polyolefin additives to asphalt mixtures to prevent rutting. Since the addition of polyolefin additives has the advantages of simple construction process, convenient use, and significant improvement in the high-temperature performance of the mixture, its application in the base and bottom layers of highway pavements has continued to grow steadily in recent years. However, it has certain limitations, mainly manifested in: the polymer has poor thermal oxygen aging resistance, and while improving the high-temperature performance of the asphalt mixture, it reduces its low-temperature performance. Summary of the invention

[0007] In order to solve the deficiencies mentioned in the above-mentioned background technology, the purpose of the present invention is to provide a method for preparing an asphalt-based filler for seamless expansion joints. The method is convenient and efficient, has good durability, and is suitable for rapid repair and new construction of expansion joints. At the same time, by adding dry elasticizers and anti-rutting components, the asphalt-based filler is endowed with excellent anti-rutting performance, antioxidant performance, and high and low temperature resistance.

[0008] The purpose of the present invention can be achieved through the following technical solutions:

[0009] A method for preparing an asphalt-based filler for a seamless expansion joint, the asphalt-based filler comprising the following components in parts by weight: 100 parts of stone, 7.5 to 11.3 parts of high-viscosity asphalt, 0.7 to 1.2 parts of a dry elasticizer, 3.7 to 6.5 parts of an inorganic filler, and 0.8 to 1.1 parts of an anti-rutting component;

[0010] The dry elasticizer is prepared by adding a pre-crushed styrene-butadiene-styrene block copolymer to a release agent, a cosolvent, and a crosslinking agent;

[0011] The anti-rutting component comprises the following raw materials in parts by weight: 50-70 parts of modified polyethylene, 5-10 parts of nanofiller, 3-7 parts of coupling agent, and 2-5 parts of lubricant. The modified polyethylene is prepared by grafting p-phenylenediamine on the surface of oxidized carbon nanotubes by chemical reaction and further grafting with maleic anhydride grafted polyethylene;

[0012] The preparation method of the asphalt-based filler comprises the following steps:

[0013] S1. After uniformly mixing parts by weight of modified polyethylene, nanofiller, coupling agent and lubricant, the mixture is blended and extruded through an extruder and granulated to obtain an anti-rutting component;

[0014] S2, placing parts by weight of stone in a stirring pot and heating to 170-190° C., then adding parts by weight of dry elasticizer and anti-rutting component to the stone in batches and stirring well to obtain a premix;

[0015] S3, adding parts by weight of high-viscosity asphalt heated to 160-180° C. to the premix and mixing evenly to obtain a mixture;

[0016] S4, adding parts by weight of inorganic filler to the mixture and stirring well to obtain the asphalt-based filler for seamless expansion joints.

[0017] Preferably, the stone material is a mixture of basalt crushed stone, limestone crushed stone and mineral powder.

[0018] Preferably, the stone adopts a single grade, and the nominal diameter of the stone is 6 to 11 mm.

[0019] Preferably, the stone adopts discontinuous grading, and the nominal diameter of the stone is 6-11 mm, 11-16 mm.

[0020] Preferably, the inorganic filler is a mixture of one or more of stone powder, blast furnace slag, and fly ash, and the passing rate of the 0.75 mm square hole sieve is 90-100%.

[0021] Preferably, the preparation method of the dry elasticizing agent comprises the following steps:

[0022] a. crushing the dry styrene-butadiene-styrene block copolymer into a powder having a particle size of 10 to 2000 μm at room temperature;

[0023] b. Add a release agent, a cosolvent, a crosslinking agent and a crosslinking aid to the obtained powder, and stir to obtain a basic material;

[0024] c. Place the base material in an extruder for cold granulation, and obtain a dry elasticizer after cooling.

[0025] Preferably, the release agent is diatomaceous earth, the cosolvent is furfural extracted oil, the main cross-linking agent is sulfur, and the cross-linking auxiliary agent is tetramethylthiuram monosulfide.

[0026] Preferably, the weight ratio of the release agent, the cosolvent, the main cross-linking agent, the cross-linking auxiliary agent and the styrene-butadiene-styrene block copolymer is 1-4:20-30:3-10:1-5:60-70.

[0027] Preferably, the method for preparing the modified polyethylene comprises the following steps:

[0028] (1) heating maleic anhydride in a boiling water bath to melt it, then adding it, polyethylene and initiator 2,5-dimethyl-2,5-bis-(tert-butylperoxy)hexane into a high-speed mixer and mixing them evenly for 5 to 7 minutes, then adding the obtained mixture into a twin-screw extruder for extrusion granulation, and controlling the extruder temperature at 150 to 230° C. to prepare maleic anhydride grafted polyethylene;

[0029] (2) taking carbon nanotubes in a mixture of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 3:1, placing the mixture at 75-90°C for reaction for 3-5 hours, filtering, washing and drying after the reaction, ultrasonically dispersing the obtained product in N,N-dimethylformamide, adding thionyl chloride, placing the mixture at 80-95°C for reflux reaction for 20-24 hours, filtering, washing and drying after the reaction, and preparing acyl chloride carbon nanotubes;

[0030] (3) taking p-phenylenediamine and dissolving it in N,N-dimethylformamide, adding acyl chloride carbon nanotubes, and reacting at 80-95° C. for 20-24 hours. After the reaction is completed, filtering, washing, and drying are performed to prepare amino carbon nanotubes;

[0031] (4) The maleic anhydride grafted polyethylene is dissolved in acetone, and then the amino carbon nanotubes are added and ultrasonically dispersed, and the mixture is reacted at 30-50° C. for 3-5 hours. After the reaction is completed, the polyethylene is filtered, washed, and dried to prepare the modified polyethylene.

[0032] Preferably, the nanofiller in the anti-rutting component is one or more combinations of nano calcium carbonate, nano silicon dioxide, and nano titanium dioxide; the coupling agent is one or more combinations of KH-550 silane coupling agent, KH-560 silane coupling agent, KH-570 silane coupling agent, and titanate coupling agent; the lubricant is one or more combinations of stearic acid, calcium stearate, paraffin, and polyethylene wax.

[0033] Beneficial effects of the present invention:

[0034] The present invention uses stone, high-viscosity asphalt, dry elasticizer, inorganic filler and anti-rutting component as raw materials to prepare a seamless expansion joint asphalt-based filler with simple proportion, low cost and excellent rebound performance, which can meet the normal use of bridge expansion joints with an expansion amount of less than 80 mm. At the same time, the preparation method of the seamless expansion joint asphalt-based filler provided by the present invention is convenient and efficient, and there is no need to perform shearing, swelling, development and other modification processing on the asphalt before mixing the filler, which not only reduces the processing cost but also improves the efficiency of filler preparation.

[0035] The present invention mixes powdered styrene-butadiene-styrene block copolymer with an isolation agent, a cosolvent and a crosslinking agent and then cold granulates the mixture into granules. When the temperature rises to the asphalt mixing temperature, the activity of the crosslinking main agent and the crosslinking auxiliary agent reaches a relatively high level. After contacting with the styrene-butadiene-styrene block copolymer powder, the -SS- free bonds can be generated to replace the C=C double bonds in the styrene-butadiene-styrene block copolymer, and a crosslinking grafting reaction occurs quickly to form a stable three-dimensional network structure, thereby improving the high and low temperature performances of the asphalt mixture. In addition, the present invention uses a twin-screw extruder to prepare maleic anhydride grafted polyethylene through a melt grafting method. At the same time, the present invention uses concentrated sulfuric acid and concentrated nitric acid to oxidize carbon nanotubes, so that the surface of the carbon nanotubes is rich in carboxyl groups, wherein the carbon nanotubes have extremely high specific surface area, excellent elastic modulus and tensile strength, excellent thermal properties and extremely low thermal expansion coefficient, and then the oxidized carbon nanotubes are chlorinated and grafted with the amino group at one end of the antioxidant p-phenylenediamine structure to prepare amino carbon nanotubes, so that the antioxidant is grafted to the surface of the carbon nanotubes, which is conducive to the dispersion of the carbon nanotubes, and can also overcome the physical loss of the antioxidant due to migration and volatilization to a certain extent, and finally the maleic anhydride group in the maleic anhydride grafted polyethylene structure reacts with the amino group on the surface of the amino carbon nanotubes to prepare modified polyethylene. The addition of modified polyethylene can give the asphalt-based filler excellent anti-rutting performance, oxidation resistance and high and low temperature resistance. DETAILED DESCRIPTION

[0036] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] The index parameters of high viscosity asphalt in the embodiments of the present invention and the comparative examples are as follows:

[0038] Needle penetration 25℃, 100g, 5s (0.01mm): ≥40,

[0039] Softening point TR&B(℃):≥80,

[0040] Elongation 5cm / min, 5℃(cm): ≥50,

[0041] 60℃ dynamic viscosity (Pa˙s): ≥20000.

[0042] Embodiment 1 A method for preparing a dry elasticizing agent comprises the following steps:

[0043] a. crushing the styrene-butadiene-styrene block copolymer in a dry state into a powder having a particle size of 500 μm at room temperature;

[0044] b. Add diatomaceous earth, furfural extracted oil, sulfur and tetramethylthiuram monosulfide to the obtained powder, stir to obtain a base material, diatomaceous earth, furfural extracted oil, sulfur, tetramethylthiuram monosulfide and styrene - butadiene - styrene block copolymer in a weight ratio of 2:23:5:1:64;

[0045] c. The base material is placed in a flat die extruder with a cutting length of 15 mm for cold granulation, cooled with cold water so that its temperature is not higher than 80°C, and then further cooled to room temperature to obtain a dry elasticizer.

[0046] Embodiment 2 A method for preparing a modified polyethylene comprises the following steps:

[0047] (1) 1.2 g of maleic anhydride was heated and melted in a boiling water bath, and then added into a high-speed mixer with 100 g of polyethylene and 0.5 g of initiator 2,5-dimethyl-2,5-bis-(tert-butylperoxy)hexane and mixed for 5 min. The obtained mixture was then added into a twin-screw extruder for extrusion granulation. The extruder temperature was controlled at 150-230° C. to prepare maleic anhydride grafted polyethylene;

[0048] (2) 3 g of carbon nanotubes were added with 81 mL of concentrated sulfuric acid and 27 mL of concentrated nitric acid, and the mixture was reacted at 85° C. for 4 h. After the reaction was completed, the mixture was filtered, washed, and dried. 1.2 g of the obtained product was ultrasonically dispersed in 100 mL of N,N-dimethylformamide, and 50 mL of dichlorothionyl was added. The mixture was refluxed at 90° C. for 24 h. After the reaction was completed, the mixture was filtered, washed, and dried to prepare chlorinated carbon nanotubes.

[0049] (3) taking 0.5 g of p-phenylenediamine and dissolving it in 100 mL of N,N-dimethylformamide, adding 0.8 g of acyl chloride carbon nanotubes, and reacting at 90° C. for 24 h. After the reaction is completed, filtering, washing, and drying are performed to prepare amino carbon nanotubes;

[0050] (4) 5.2 g of maleic anhydride grafted polyethylene was dissolved in 80 mL of acetone, and then 2 g of amino carbon nanotubes was added and ultrasonically dispersed, and the mixture was reacted at 45° C. for 3 h. After the reaction was completed, the mixture was filtered, washed, and dried to prepare modified polyethylene.

[0051] Example 3 An asphalt-based filler for seamless expansion joints comprises the following components in parts by weight: 100 parts of stone, 7.5 parts of high-viscosity asphalt, 0.7 parts of dry elasticizer prepared in Example 1, 3.7 parts of stone powder, and 0.8 parts of anti-rutting component; wherein the anti-rutting component comprises the following raw materials in parts by weight: 50 parts of modified polyethylene prepared in Example 2, 5 parts of nano-calcium carbonate, 3 parts of KH-550 silane coupling agent, and 2 parts of stearic acid; the stone is selected from basalt crushed stone with a particle size of 10 to 15 mm, basalt crushed stone with a particle size of 6 to 11 mm, limestone crushed stone with a particle size of 5 to 10 mm, and mineral powder, which are mixed in a mass ratio of 39:35:16:10.

[0052] The preparation method of the asphalt-based filler comprises the following steps:

[0053] S1. After uniformly mixing parts by weight of modified polyethylene, nanofiller, coupling agent and lubricant, the mixture is blended and extruded through an extruder and granulated to obtain an anti-rutting component;

[0054] S2, placing parts by weight of stone in a stirring pot and heating to 180° C., then adding parts by weight of dry elasticizer and anti-rutting component to the stone in batches and stirring well to obtain a premix;

[0055] S3, adding parts by weight of high-viscosity asphalt heated to 175° C. to the premix and mixing evenly to obtain a mixture;

[0056] S4, adding parts by weight of inorganic filler to the mixture and stirring well to obtain the asphalt-based filler for seamless expansion joints.

[0057] Example 4 An asphalt-based filler for seamless expansion joints comprises the following components in parts by weight: 100 parts of stone, 10.2 parts of high-viscosity asphalt, 1.0 parts of the dry elasticizer prepared in Example 1, 5.3 parts of blast furnace slag, and 0.9 parts of an anti-rutting component; wherein the anti-rutting component comprises the following raw materials in parts by weight: 65 parts of modified polyethylene prepared in Example 2, 7 parts of nano-silicon dioxide, 5 parts of KH-560 silane coupling agent, and 3 parts of paraffin; the stone is selected from basalt crushed stone with a particle size of 10 to 15 mm, basalt crushed stone with a particle size of 6 to 11 mm, limestone crushed stone with a particle size of 5 to 10 mm, and mineral powder, which are mixed in a mass ratio of 39:35:16:10.

[0058] The preparation method of the above-mentioned asphalt-based filler is the same as that of Example 3.

[0059] Example 5 An asphalt-based filler for seamless expansion joints comprises the following components in parts by weight: 100 parts of stone, 11.3 parts of high-viscosity asphalt, 1.2 parts of dry elasticizer prepared in Example 1, 6.3 parts of fly ash, and 1.1 parts of anti-rutting component; wherein the anti-rutting component comprises the following raw materials in parts by weight: 68 parts of modified polyethylene prepared in Example 2, 10 parts of nano-titanium dioxide, 7 parts of KH-570 silane coupling agent, and 5 parts of polyethylene wax; the stone is selected from basalt crushed stone with a particle size of 10 to 15 mm, basalt crushed stone with a particle size of 6 to 11 mm, limestone crushed stone with a particle size of 5 to 10 mm, and mineral powder, which are mixed in a mass ratio of 39:35:16:10.

[0060] The preparation method of the above-mentioned asphalt-based filler is the same as that of Example 3.

[0061] Comparative Example 1 An asphalt-based filler for seamless expansion joints comprises the following components in parts by weight: 100 parts of stone, 11.3 parts of high-viscosity asphalt, 1.2 parts of styrene-butadiene-styrene block copolymer powder, 6.3 parts of fly ash, and 1.1 parts of anti-rutting components; wherein the anti-rutting components comprise the following raw materials in parts by weight: 68 parts of modified polyethylene prepared in Example 2, 10 parts of nano-titanium dioxide, 7 parts of KH-570 silane coupling agent, and 5 parts of polyethylene wax; the stone is selected from basalt crushed stone with a particle size of 10 to 15 mm, basalt crushed stone with a particle size of 6 to 11 mm, limestone crushed stone with a particle size of 5 to 10 mm, and mineral powder, which are mixed in a mass ratio of 39:35:16:10.

[0062] The preparation method of the above-mentioned asphalt-based filler is the same as that of Example 3.

[0063] Comparative Example 2: An asphalt-based filler for seamless expansion joints comprises the following components in parts by weight: 100 parts of stone, 11.3 parts of high-viscosity asphalt, 1.2 parts of the dry elasticizer prepared in Example 1, 6.3 parts of fly ash, and 1.1 parts of an anti-rutting component; wherein the anti-rutting component comprises the following raw materials in parts by weight: 68 parts of polyethylene, 10 parts of nano-titanium dioxide, 7 parts of KH-570 silane coupling agent, and 5 parts of polyethylene wax; the stone is selected from basalt crushed stone with a particle size of 10 to 15 mm, basalt crushed stone with a particle size of 6 to 11 mm, limestone crushed stone with a particle size of 5 to 10 mm, and mineral powder, which are mixed in a mass ratio of 39:35:16:10.

[0064] The preparation method of the above-mentioned asphalt-based filler is the same as that of Example 3.

[0065] Performance Testing

[0066] The asphalt-based fillers prepared in Examples 3-5 and Comparative Examples 1-2 were subjected to performance tests:

[0067] The dynamic stability and low temperature bending tests were tested and detected according to JTG-E20-2011 "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering"; for the aging performance test, the asphalt-based filler was first aged for 4 hours in a forced ventilation oven at 135°C, and then the test pieces were made into forced ventilation ovens at 85°C and aged for 120 hours. The data results are shown in Table 1.

[0068] Table 1 Test results of sample performance

[0069]

[0070] From the data in Table 1, it can be seen that the asphalt-based fillers prepared in Examples 3-5 of the present invention have excellent anti-rutting performance, oxidation resistance, and high and low temperature resistance. In Comparative Example 1, the dry elasticizer is replaced with styrene-butadiene-styrene block copolymer powder in equal amounts, and the high and low temperature resistance measured is worse than that of Examples 3-5, indicating that the addition of auxiliary agents such as release agents and cross-linking agents can improve the dynamic stability and low-temperature bending failure strain value of the asphalt-based filler. In Comparative Example 2, the polyethylene in the anti-rutting component is not modified, and the oxidation resistance and high and low temperature resistance measured are worse than those of Examples 3-5, because the polyethylene is not modified by the carbon nanotubes grafted with antioxidants.

[0071] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0072] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.

Claims

1. A method for preparing an asphalt-based filler for a seamless expansion joint, characterized in that: The asphalt-based filler comprises the following components by weight: 100 parts of stone, 7.5-11.3 parts of high-viscosity asphalt, 0.7-1.2 parts of dry elasticizer, 3.7-6.5 parts of inorganic filler, and 0.8-1.1 parts of anti-rutting component; The dry elasticizer is prepared by adding a pre-crushed styrene-butadiene-styrene block copolymer to a release agent, a cosolvent, and a crosslinking agent; The anti-rutting component comprises the following raw materials in parts by weight: 50-70 parts of modified polyethylene, 5-10 parts of nanofiller, 3-7 parts of coupling agent, and 2-5 parts of lubricant. The modified polyethylene is prepared by grafting p-phenylenediamine on the surface of oxidized carbon nanotubes by chemical reaction and further grafting with maleic anhydride grafted polyethylene; The preparation method of the asphalt-based filler comprises the following steps: S1. After uniformly mixing parts by weight of modified polyethylene, nanofiller, coupling agent and lubricant, the mixture is blended and extruded through an extruder and granulated to obtain an anti-rutting component; S2, placing parts by weight of stone in a stirring pot and heating to 170-190° C., then adding parts by weight of dry elasticizer and anti-rutting component to the stone in batches and stirring well to obtain a premix; S3, adding parts by weight of high-viscosity asphalt heated to 160-180° C. to the premix and mixing evenly to obtain a mixture; S4, adding parts by weight of inorganic filler to the mixture and stirring well to obtain the asphalt-based filler for seamless expansion joints.

2. The method for preparing an asphalt-based filler for a seamless expansion joint according to claim 1, characterized in that: The stone material is a mixture of basalt crushed stone, limestone crushed stone and mineral powder.

3. The method for preparing an asphalt-based filler for a seamless expansion joint according to claim 2, characterized in that: The stone adopts a single grade, and the nominal diameter of the stone is 6 to 11 mm.

4. The method for preparing an asphalt-based filler for a seamless expansion joint according to claim 2, characterized in that: The stones are discontinuously graded, and the nominal diameters of the stones are 6-11 mm and 11-16 mm.

5. The method for preparing an asphalt-based filler for a seamless expansion joint according to claim 1, characterized in that: The inorganic filler is a mixture of one or more of stone powder, blast furnace slag and fly ash, and the passing rate of the 0.75 mm square hole sieve is 90-100%.

6. The method for preparing an asphalt-based filler for a seamless expansion joint according to claim 1, characterized in that: The preparation method of the dry elasticizing agent comprises the following steps: a. crushing the dry styrene-butadiene-styrene block copolymer into a powder having a particle size of 10 to 2000 μm at room temperature; b. Add a release agent, a cosolvent, a crosslinking agent and a crosslinking aid to the obtained powder, and stir to obtain a basic material; c. Place the base material in an extruder for cold granulation, and obtain a dry elasticizer after cooling.

7. The method for preparing an asphalt-based filler for a seamless expansion joint according to claim 6, characterized in that: The release agent is diatomaceous earth, the cosolvent is furfural extracted oil, the main cross-linking agent is sulfur, and the cross-linking auxiliary agent is tetramethylthiuram monosulfide.

8. The method for preparing an asphalt-based filler for a seamless expansion joint according to claim 6, characterized in that: The weight ratio of the isolating agent, the cosolvent, the main crosslinking agent, the crosslinking auxiliary agent and the styrene-butadiene-styrene block copolymer is 1-4:20-30:3-10:1-5:60-70.

9. The method for preparing an asphalt-based filler for a seamless expansion joint according to claim 1, characterized in that: The preparation method of the modified polyethylene comprises the following steps: (1) heating maleic anhydride in a boiling water bath to melt it, then adding it, polyethylene and initiator 2,5-dimethyl-2,5-bis-(tert-butylperoxy)hexane into a high-speed mixer and mixing them evenly for 5 to 7 minutes, then adding the obtained mixture into a twin-screw extruder for extrusion granulation, and controlling the extruder temperature at 150 to 230° C. to prepare maleic anhydride grafted polyethylene; (2) taking carbon nanotubes in a mixture of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 3:1, placing the mixture at 75-90°C for reaction for 3-5 hours, filtering, washing and drying after the reaction, ultrasonically dispersing the obtained product in N,N-dimethylformamide, adding thionyl chloride, placing the mixture at 80-95°C for reflux reaction for 20-24 hours, filtering, washing and drying after the reaction, and preparing acyl chloride carbon nanotubes; (3) taking p-phenylenediamine and dissolving it in N,N-dimethylformamide, adding acyl chloride carbon nanotubes, and reacting at 80-95° C. for 20-24 hours. After the reaction is completed, filtering, washing, and drying are performed to prepare amino carbon nanotubes; (4) The maleic anhydride grafted polyethylene is dissolved in acetone, and then the amino carbon nanotubes are added and ultrasonically dispersed, and the mixture is reacted at 30-50° C. for 3-5 hours. After the reaction is completed, the polyethylene is filtered, washed, and dried to prepare the modified polyethylene.

10. The method for preparing asphalt-based filler for seamless expansion joints according to claim 1, characterized in that: The nanofiller in the anti-rutting component is one or more combinations of nano calcium carbonate, nano silicon dioxide, and nano titanium dioxide; the coupling agent is one or more combinations of KH-550 silane coupling agent, KH-560 silane coupling agent, KH-570 silane coupling agent, and titanate coupling agent; the lubricant is one or more combinations of stearic acid, calcium stearate, paraffin, and polyethylene wax.