Preparation method of PVD (Physical Vapor Deposition) conductive film layer applied to carbon fibers

By combining arc discharge with magnetron sputtering, the problems of electric ignition and boundary lines of carbon fiber materials when plating conductive films are solved, and the close bonding of the conductive film layer and the substrate are achieved and excellent conductivity are achieved.

CN118996353APending Publication Date: 2024-11-22TRITREE METAL SHENZHEN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411073412.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Due to the insulation, carbon fiber materials are prone to electric ignition damage when plating conductive films, and obvious dividing lines often appear after coating, affecting the binding force.

Method used

By combining arc discharge and magnetron sputtering, first deposit the Cr layer, then deposit the pure Cr layer, CrCu or CrAg film layer and Cu or Ag film layer in turn. The combination of arc discharge and magnetron sputtering is ensured. The tight bonding and conductivity of the layers.

Benefits of technology

It effectively avoids the electric ignition damage of carbon fiber materials, realizes the close bond between the conductive film layer and the substrate, and the film layer has no obvious boundaries, which improves the conductivity and deposition speed.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996353A_ABST
    Figure CN118996353A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a PVD (Physical Vapor Deposition) conductive film layer applied to carbon fibers, and belongs to the field of PVD coating. Comprising the following steps: S1, carrying out ultrasonic cleaning on a carbon fiber substrate material; s2, putting the cleaned carbon fiber substrate material into a coating chamber, and heating and vacuumizing the coating chamber; s3, when the local vacuum degree of the coating chamber reaches 0.001 Pa or below, argon is introduced, arc discharge is started, and a Cr layer is deposited; s4, arc discharge is closed, the argon inlet amount is adjusted, a medium-frequency coating power source is started, and a pure Cr layer is deposited; s5, opening the Cr target, opening the copper target or the silver target at the same time, and depositing a CrCu or CrAg film layer; s6, closing the Cr target, continuing to open the copper target or the silver target, and depositing a Cu layer or an Ag layer; and S7, the copper target or the silver target is closed, argon is closed, and coating is finished. Compared with the prior art, arc discharge and magnetron sputtering are combined, so that the whole PVD film layer can be integrated, an obvious film layer boundary line is avoided, and the combination is tighter; and the deposition speed of the film layer is higher.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of PVD coating, and in particular relates to a method for preparing a PVD conductive film layer applied to carbon fiber. Background Art

[0002] Carbon fiber materials have excellent physical properties and excellent mechanical properties. The specific modulus and specific strength of the composite material formed with resin are about three times higher than those of conventional steel and aluminum alloy. Carbon fiber materials of the same volume are lighter and have good application prospects. However, since carbon fiber materials are not conductive, their application scenarios are greatly limited.

[0003] In order to solve this problem, a process of coating a conductive film on a carbon fiber material by magnetron sputtering has appeared in the prior art. When coating with magnetron sputtering technology, glow discharge is usually used to clean the surface of the product, but since glow discharge usually needs to last for about 30 minutes and when there are too many products, a lantern effect is easily generated. Since the carbon fiber material is insulating and the surface is not conductive, directly turning on the high bias voltage will cause the substrate fixing fixture to spark, causing damage to the carbon fiber material. Summary of the invention

[0004] In order to solve the above problems, the purpose of the present invention is to provide a method for preparing a PVD conductive film layer applied to carbon fiber, which can avoid damage to the carbon fiber material during coating;

[0005] Another object of the present invention is to provide a method for preparing a PVD conductive film layer applied to carbon fiber, so that the PVD conductive film layer is seamless, has no obvious dividing line, and has stronger bonding force.

[0006] To achieve the above object, the technical solution of the present invention is as follows:

[0007] The present invention provides a method for preparing a PVD conductive film layer applied to carbon fiber, comprising the steps of:

[0008] S1: ultrasonically cleaning the carbon fiber substrate material;

[0009] S2: placing the cleaned carbon fiber substrate material into a coating chamber, and heating and vacuuming the coating chamber;

[0010] S3: When the local vacuum degree of the coating chamber reaches below 0.001Pa, argon gas is introduced, arc discharge is started and the Cr layer is deposited;

[0011] S4: turn off the arc discharge, adjust the argon gas intake, turn on the medium frequency coating power supply, and deposit a pure Cr layer;

[0012] S5: Turn on the Cr target and turn on the copper target or silver target at the same time to deposit a CrCu or CrAg film layer;

[0013] S6: Turn off the Cr target, continue to turn on the copper target or the silver target, and deposit the Cu layer or the Ag layer;

[0014] S7: Turn off the copper target or silver target, turn off the argon gas, and end the coating.

[0015] Furthermore, in step S1, ultrasonic cleaning can remove dirt, fingerprints and other problems of the incoming carbon fiber base material, thereby ensuring the cleanliness of the carbon fiber base material before magnetron sputtering.

[0016] Furthermore, in step S2, the temperature of the coating chamber is 80-100°C.

[0017] Furthermore, in step S3, argon gas is introduced, and when the pressure of the coating chamber reaches 0.1-0.5Pa, arc discharge is performed, the arc discharge current is 80A, the discharge time is 15min, and the deposition thickness of the Cr layer is 400-600nm. In this step, the thickness of the film layer needs to be moderate. A too thin film layer cannot ensure the bonding force between the film layer and the substrate, and a too thick film layer will also cause insufficient bonding force and film fall off, so that the carbon fiber surface is metallized, which is approximately equal to an ordinary metal substrate, and a magnetron sputtering process can be used for PVD deposition.

[0018] Further, in step S4, when the gas pressure in the coating chamber reaches 0.2-0.3 Pa, the medium frequency coating power supply is turned on to deposit a pure Cr layer for 15 minutes, which is used for the connection between the magnetron sputtering Cr layer and the arc discharge Cr layer.

[0019] Furthermore, in step S5, the deposition time of the film layer is 8 minutes, which is used for the connection between the magnetron sputtered Cr layer and the magnetron sputtered Cu layer or Ag layer.

[0020] Furthermore, in step S6, the film deposition time is 75 minutes, and magnetron sputtering Cu or Ag is used as the source of conductivity of carbon fiber. A too thin film layer will result in poor conductivity. The film layer of 8A magnetron sputtering for 75 minutes can reach a thickness of about 1 micron, and the square resistance of the film layer is about 28 milliohms, which has excellent conductivity.

[0021] Furthermore, in steps S4-S6, the current of the medium frequency coating power supply is 8A, the frequency is 40KHz, and the voltage is 470-530V. Excessive current will cause the carbon fiber surface to be broken down and sparked by the current, and will also cause the temperature in the magnetron sputtering device to rise too high and too fast during the coating process; the sputtering speed of small current is too slow, affecting the coating speed.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] First, the present application combines arc discharge with magnetron sputtering. Arc discharge is performed initially to deposit a Cr layer, and then magnetron sputtering is performed to sequentially deposit a pure Cr layer as a base layer, a CrCu or CrAg film layer as a transition layer, and a Cu layer or an Ag layer as a surface layer. The arc discharge Cr layer and the magnetron sputtering pure Cr layer can be well combined, so that the arc discharge deposited Cr layer and the magnetron sputtering film layer have better bonding force; the outermost Cu or Ag film layer makes the carbon fiber have good conductivity, and the CrCu or CrAg film layer can realize the transition between the Cr layer and the Cu or Ag film layer. The entire PVD film layer is integrated, and there will be no obvious film layer boundary, and the combination is tighter;

[0024] At the same time, the characteristics of arc discharge are utilized to allow the high-density electron flow in the arc plasma to deposit on the substrate. Compared with simple magnetron sputtering, the sputtering amount per unit time is larger, and the film particle ionization rate is higher, which can reach 60-90%, and the deposition speed is faster. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a flowchart of the preparation method of this embodiment.

[0026] Figure 2 This is an SEM enlarged image of the cross section of the PVD conductive film layer of this embodiment.

[0027] Figure 3 This is a diagram of the square resistance measurement interface of the PVD conductive film layer of this embodiment. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0029] To achieve the above object, the technical solution of the present invention is as follows:

[0030] See also Figure 1 As shown, this embodiment provides a method for preparing a PVD conductive film layer applied to carbon fiber, comprising the steps of:

[0031] S1: ultrasonically cleaning the carbon fiber substrate material;

[0032] S2: placing the cleaned carbon fiber substrate material into a coating chamber, and heating and vacuuming the coating chamber;

[0033] S3: When the local vacuum degree of the coating chamber reaches below 0.001Pa, argon gas is introduced, arc discharge is started and the Cr layer is deposited;

[0034] S4: turn off the arc discharge, adjust the argon gas intake, turn on the medium frequency coating power supply, and deposit a pure Cr layer;

[0035] S5: Turn on the Cr target and turn on the copper target or silver target at the same time to deposit a CrCu or CrAg film layer;

[0036] S6: Turn off the Cr target, continue to turn on the copper target or the silver target, and deposit the Cu layer or the Ag layer;

[0037] S7: Turn off the copper target or silver target, turn off the argon gas, and end the coating.

[0038] Furthermore, in step S1, ultrasonic cleaning can remove dirt, fingerprints and other problems of the incoming carbon fiber base material, thereby ensuring the cleanliness of the carbon fiber base material before magnetron sputtering.

[0039] Furthermore, in step S2, the temperature of the coating chamber is 80°C.

[0040] Furthermore, in step S3, argon gas is introduced, and when the pressure of the coating chamber reaches 0.1-0.5Pa, arc discharge is performed, the arc discharge current is 80A, the discharge time is 15min, and the deposition thickness of the Cr layer is 500nm. In this step, the thickness of the film layer needs to be moderate. A too thin film layer cannot ensure the bonding force between the film layer and the substrate, and a too thick film layer will also cause insufficient bonding force and film fall off, so that the carbon fiber surface is metallized, which is approximately equal to an ordinary metal substrate, and a magnetron sputtering process can be used for PVD deposition.

[0041] Furthermore, in step S4, when the gas pressure in the coating chamber reaches 0.28 Pa, the medium frequency coating power supply is turned on to deposit a pure Cr layer for 15 minutes, which is used for the connection between the magnetron sputtering Cr layer and the arc discharge Cr layer.

[0042] Furthermore, in step S5, the deposition time of the film layer is 8 minutes, which is used for the connection between the magnetron sputtered Cr layer and the magnetron sputtered Cu layer or Ag layer.

[0043] Further, in step S6, the film deposition time is 75 minutes, and magnetron sputtering Cu or Ag is used as the source of carbon fiber conductivity. Too thin a film layer will result in poor conductivity. The film layer of 75 minutes 8A magnetron sputtering can reach a thickness of about 1 micron, such as Figure 3 Measurements show that the sheet resistance of the film layer is about 28 milliohms, which means it has excellent conductivity.

[0044] Furthermore, in steps S4-S6, the current of the medium frequency coating power supply is 8A, the frequency is 40KHz, and the voltage is 470V. Excessive current will cause the carbon fiber surface to be broken down and sparked by the current, and will also cause the temperature in the magnetron sputtering device to rise too high and too fast during the coating process; the sputtering speed of small current is too slow, affecting the coating speed.

[0045] Compared with the prior art, the beneficial effects of this embodiment are:

[0046] This embodiment combines arc discharge with magnetron sputtering. Arc discharge is performed initially to deposit a Cr layer, and then magnetron sputtering is performed to deposit a pure Cr layer as a base layer, a CrCu or CrAg film layer as a transition layer, and a Cu layer or an Ag layer as a surface layer. The arc discharge Cr layer and the magnetron sputtering pure Cr layer can be well combined, so that the arc discharge deposited Cr layer and the magnetron sputtering film layer have better bonding strength; the outermost Cu or Ag film layer makes the carbon fiber have good conductivity, and the CrCu or CrAg film layer can achieve the transition between the Cr layer and the Cu or Ag film layer. See Figure 2 , SEM magnified image of the cross section of the PVD conductive film layer, the lower layer is the substrate, the upper layer is the PVD conductive film layer, the thickness of the entire PVD conductive film layer is 3.84μm, the PVD film layer is integrated, there is no obvious film layer boundary, and the combination is tighter;

[0047] At the same time, the characteristics of arc discharge are utilized to allow the high-density electron flow in the arc plasma to deposit on the substrate. Compared with simple magnetron sputtering, the sputtering amount per unit time is larger, and the film particle ionization rate is higher, which can reach 60-90%, and the deposition speed is faster.

[0048] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a PVD conductive film layer applied to carbon fiber, characterized in that: Includes steps: S1: ultrasonically cleaning the carbon fiber substrate material; S2: placing the cleaned carbon fiber substrate material into a coating chamber, and heating and vacuuming the coating chamber; S3: When the local vacuum degree of the coating chamber reaches below 0.001Pa, argon gas is introduced, arc discharge is started and the Cr layer is deposited; S4: turn off the arc discharge, adjust the argon gas intake, turn on the medium frequency coating power supply, and deposit a pure Cr layer; S5: Turn on the Cr target and turn on the copper target or silver target at the same time to deposit a CrCu or CrAg film layer; S6: Turn off the Cr target, continue to turn on the copper target or the silver target, and deposit the Cu layer or the Ag layer; S7: Turn off the copper target or silver target, turn off the argon gas, and end the coating.

2. The method for preparing a PVD conductive film layer applied to carbon fiber according to claim 1, characterized in that: In step S1, ultrasonic cleaning is performed to remove dirt and fingerprints on the incoming carbon fiber base material, thereby ensuring the cleanliness of the carbon fiber base material before magnetron sputtering.

3. The method for preparing a PVD conductive film layer applied to carbon fiber according to claim 1, characterized in that: In step S2, the temperature of the coating chamber is 80-100°C.

4. The method for preparing a PVD conductive film layer applied to carbon fiber according to claim 1, characterized in that: In step S3, argon gas is introduced, and when the gas pressure in the coating chamber reaches 0.1-0.5 Pa, arc discharge is performed, the arc discharge current is 80A, the discharge time is 15 minutes, and the deposition thickness of the Cr layer is 400-600nm.

5. The method for preparing a PVD conductive film layer applied to carbon fiber according to claim 1, characterized in that: In step S4, when the gas pressure in the coating chamber reaches 0.2-0.3 Pa, the medium frequency coating power supply is turned on to deposit a pure Cr layer for 15 minutes, which is used for the connection between the magnetron sputtering Cr layer and the arc discharge Cr layer.

6. The method for preparing a PVD conductive film layer applied to carbon fiber according to claim 1, characterized in that: In step S5, the deposition time of the film layer is 8 minutes, which is used for the connection between the magnetron sputtered Cr layer and the magnetron sputtered Cu layer or Ag layer.

7. The method for preparing a PVD conductive film layer applied to carbon fiber according to claim 1, characterized in that: In step S6, the film deposition time is 75 minutes.

8. The method for preparing a PVD conductive film layer applied to carbon fiber according to claim 1, characterized in that: In steps S4-S6, the current of the medium frequency coating power supply is 8A, the frequency is 40KHz, and the voltage is 470-530V.