Surface coating method and semiconductor equipment

By using atomic layer deposition and plasma immersion processes to form multi-layer protective layers on the surface of semiconductor equipment, the problem of equipment surface corrosion is solved, process stability and production efficiency are improved, and equipment service life is extended.

CN118996362APending Publication Date: 2024-11-22JIANGSU LEUVEN INSTR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310566008.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-18
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The prior art cannot form a comprehensive and stable protective layer on the surface of semiconductor equipment, resulting in corrosion of internal components of the reaction chamber and affecting chip processing quality and process stability.

Method used

The surface coating method combined with atomic layer deposition process and plasma immersion process is adopted to form multiple atomic layer thin films and plasma film layers in sequence, providing a comprehensive protective layer and improving the corrosion resistance of the equipment surface.

Benefits of technology

It achieves all-round coverage of the surface of semiconductor equipment, significantly reduces particle and trace elements pollution, improves process stability and production efficiency, and extends the service life of the equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996362A_ABST
    Figure CN118996362A_ABST
Patent Text Reader

Abstract

The invention discloses a surface coating method and semiconductor equipment. The surface coating method comprises the following steps: providing an equipment body to be coated; forming a first protective layer on the surface of the equipment body; wherein the first protective layer at least comprises a first sub-protective layer formed based on an atomic layer deposition process. According to the technical scheme, the first protection layer is formed on the surface of the equipment body, the first protection layer at least comprises the first sub-protection layer formed based on the atomic layer deposition process, all-around film covering can be achieved on the surface of the equipment body, and the corrosion resistance is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of surface protection technology for enhancing the function of semiconductor equipment, and more specifically, to a surface coating method and semiconductor equipment. Background Art

[0002] Because semiconductor equipment (such as thin film deposition and plasma etcher) performs chip processing below 15nm scale on large-scale integrated circuits (such as plasma etching and thin film deposition), the reaction gases or plasmas used in most processes (such as plasma containing elements such as O, F, Cl, Br, or H) also corrode the surface of components inside the reaction chamber, changing the size and surface composition of the components, affecting the quality of chip processing and the stability of the process.

[0003] In order to enable plasma and other processes to accurately process chips at the atomic level, it is necessary to ensure that the size and composition of the reaction chamber components are highly consistent during chip preparation, such as thin film deposition or plasma etching. To achieve this goal, it is necessary to form a protective layer on the surface of the semiconductor device. In the prior art, it is impossible to form a comprehensive and stable protective layer on the surface of the semiconductor device. Summary of the invention

[0004] In view of this, the present application provides a semiconductor device and a surface coating method thereof, the scheme is as follows:

[0005] A surface coating method for semiconductor equipment, comprising:

[0006] Provide the equipment body to be coated;

[0007] A first protective layer is formed on the surface of the device body; wherein the first protective layer at least includes a first sub-protective layer formed based on an atomic layer deposition process.

[0008] Preferably, in the above surface coating method, the method of forming the first sub-protective layer includes:

[0009] An atomic layer deposition process is adopted to sequentially form an atomic layer film on the surface of the device body as the first sub-protective layer.

[0010] Preferably, in the above surface coating method, the method of forming the first sub-protective layer includes:

[0011] forming a first atomic layer film based on saturated chemical adsorption and reaction between the first precursor and the surface of the device body;

[0012] forming another atomic layer film based on saturated chemical adsorption and reaction between the second precursor and the surface of the previous atomic layer film;

[0013] Before forming a next atomic layer film, the precursor used to form the previous atomic layer film is purged and discharged.

[0014] Preferably, in the above surface coating method, before forming the first protective layer, it also includes:

[0015] The surface of the device body is pretreated to improve the adhesion stability of the first sub-protection layer on the surface of the device body.

[0016] Preferably, in the above-mentioned surface coating method, the method of pre-treating the surface of the device body comprises:

[0017] The surface of the device body is modified by a first plasma immersion process, so that a gentle transition layer with a gradual change of doping components is formed on the surface of the device body.

[0018] Preferably, in the above-mentioned surface coating method, a first plasma immersion process is used to modify the surface of the device body, including:

[0019] Under a first pulse bias, ion implantation to a first depth is performed into the surface of the device body;

[0020] Under a second pulse bias, ion implantation to a second depth is performed into the surface of the device body, and / or surface alloying of the device body is achieved;

[0021] Wherein, the second depth is smaller than the first depth.

[0022] Preferably, in the above surface coating method, the method for forming the first protective layer further comprises:

[0023] A second plasma immersion process is used to form a second sub-protecting layer on the surface of the first sub-protecting layer.

[0024] Preferably, in the above surface coating method, a second plasma immersion process is used to form a second sub-protective layer on the surface of the first sub-protective layer, comprising:

[0025] Under a negative bias voltage less than 15 kV, an all-round coating is performed on the surface of the device body formed with the first sub-protective layer to form the second sub-protective layer.

[0026] Preferably, in the above surface coating method, it also includes:

[0027] forming a second protective layer on a surface of the first protective layer;

[0028] Wherein, the thickness of the second protective layer is greater than the thickness of the first protective layer.

[0029] Preferably, in the above-mentioned surface coating method, the method of forming the second protective layer includes:

[0030] The second protective layer is formed by a plasma enhanced physical vapor deposition process.

[0031] The present application also provides a semiconductor device, comprising:

[0032] Equipment body;

[0033] A first protective layer covers the device body, wherein the first protective layer at least includes a first sub-protective layer formed based on an atomic layer deposition process.

[0034] Preferably, in the above semiconductor device, the first sub-protection layer includes a plurality of atomic layer films stacked in sequence.

[0035] Preferably, in the above-mentioned semiconductor device, the surface of the device body is modified to improve the adhesion stability of the first sub-protective layer on the surface of the device body.

[0036] Preferably, in the above semiconductor device, the first protective layer further comprises: a second sub-protective layer located on the surface of the first sub-protective layer;

[0037] Wherein, the second sub-protective layer is a film layer formed by a plasma immersion process.

[0038] Preferably, in the above semiconductor device, the first protective layer includes a ceramic film.

[0039] Preferably, in the above semiconductor device, it further comprises:

[0040] A second protective layer is located on a surface of the first protective layer.

[0041] Preferably, in the above semiconductor device, the second protective layer is a plasma enhanced physical vapor deposition film.

[0042] Preferably, in the above semiconductor device, the thickness of the first protective layer is less than 25 μm, and the thickness of the second protective layer is greater than 10 μm.

[0043] Preferably, in the above semiconductor device, the second protective layer is a ceramic film.

[0044] Preferably, in the above semiconductor device, the thickness of the second protective layer is greater than the thickness of the first protective layer.

[0045] From the above description, it can be seen that in the surface coating method and semiconductor device provided by the technical solution of the present application, a first protective layer is formed on the surface of the device body, and the first protective layer includes at least a first sub-protective layer formed based on the atomic layer deposition process, which can achieve all-round thin film coverage on the surface of the device body to improve corrosion resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] In order to more clearly illustrate the technical solutions in the embodiments of the present application or the related technologies, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying any creative work.

[0047] The structures, proportions, sizes, etc. illustrated in the drawings of this specification are only used to match the contents disclosed in the specification so as to facilitate understanding and reading by persons familiar with this technology. They are not used to limit the conditions under which this application can be implemented, and therefore have no substantive technical significance. Any structural modification, change in proportion or adjustment of size, without affecting the effects and purposes that can be achieved by this application, should still fall within the scope of the technical contents disclosed in this application.

[0048] Figure 1 A schematic diagram of a process for coating a semiconductor device surface provided in an embodiment of the present application;

[0049] Figure 2 A flow chart of an ALD (atomic layer deposition) method for forming a first sub-protective layer provided in an embodiment of the present application;

[0050] Figure 3-Figure 6 A schematic diagram of the principle of a method for manufacturing a first sub-protective layer in different process steps provided in an embodiment of the present application;

[0051] Figure 7 A schematic flow chart of another method for coating the surface of a semiconductor device provided in an embodiment of the present application;

[0052] Figure 8 A schematic diagram of the principle of a plasma immersion process (PIIP) provided in an embodiment of the present application;

[0053] Fig. 9 A schematic diagram of the principle of modifying the surface of a device body provided in an embodiment of the present application;

[0054] Fig.10A flow chart of a method for modifying the surface of a device body provided in an embodiment of the present application;

[0055] Fig.11 A top view of the device body;

[0056] Fig.12 for Fig.11 A cross-sectional view of the device body shown;

[0057] Fig.13 for Fig.11 A partial enlarged view of the device body shown;

[0058] Fig.14 A partial enlarged view of a device body having a corrosion-resistant protective layer formed based on the coating method of an embodiment of the present application;

[0059] Fig.15 It is a partial enlarged view of another device body having a corrosion-resistant protective layer formed thereon based on the coating method of an embodiment of the present application;

[0060] Fig.16 A partial enlarged view of another device body having a corrosion-resistant protective layer formed thereon based on the coating method according to an embodiment of the present application;

[0061] Fig.17 This is another partially enlarged view of a device body having a corrosion-resistant protective layer formed thereon based on the coating method of an embodiment of the present application. DETAILED DESCRIPTION

[0062] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the embodiments in the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0063] At present, in a large number of semiconductor thin film deposition equipment such as physical vapor deposition (PVD) and chemical vapor deposition (CVD) systems, a large number of flat gas distribution plate workpieces based on 6061T aluminum alloy are still used in the reaction chamber, such as aluminum alloy shower head (SH). Aluminum alloy components without surface protection are not suitable for direct contact with reaction gas and plasma to prevent the components from being corroded and causing metal and particle pollution. The instability of the surface organization and composition of these aluminum alloy workpieces will interact with chemical reaction gases (such as O2, SiH4, TMA, TEOS, NH3, SiCl4, N2O, C2F6, SF6, SiC4, HBr, NF3, CF4, CHF3, CH2F2, Cl2, CCl4, BCl3, SiF4, etc.) and the plasma formed during the semiconductor thin film deposition process such as CVD and PVD, resulting in unnecessary chemical reaction consumption of chemical components forming thin film deposition on the surface of the chamber, resulting in uneven and unstable film deposition rate, and generating particle and trace element pollution, which seriously affects the process stability of thin film deposition. Therefore, improving the component structure and surface material stability of the semiconductor equipment reaction chamber through all-round material surface modification, such as all-round coating protection, and reducing particle contamination (particle size and number) during thin film deposition and etching processes is an important way to ensure the stability of high-quality chip processing technology and reduce production costs.

[0064] In semiconductor chip thin film deposition and plasma etching machine systems, anodic oxidation and plasma spraying (PS) yttrium oxide and other surface protection treatments are usually used for the inner wall of the reaction chamber and key components to enhance the surface resistance of the chamber components to chemical corrosion and plasma etching. Although anodic oxidation can achieve all-round oxidation protection of the surface of aluminum alloy workpieces, the stability of the anodic oxidation organization is very poor and it cannot work stably in an environment greater than 100°C, so it cannot be used for high-temperature thin film deposition processes (such as PVD, PECVD, etc.). In addition, even components with anodic protection layers are not recommended to be directly in contact with reactive gases or plasma. This is because the anodic oxidation organization contains cracks, which will produce particles and trace elements (such as Al) in the plasma environment. PS coatings (such as PS Y2O3) have loose structures and rough surfaces, and are prone to produce contaminated particles during plasma etching, making it difficult to stably carry out high-precision chip etching processes (such as below 15nm).

[0065] In recent years, the use of plasma enhanced physical vapor deposition (PEPVD) process to deposit dense thick coatings has been gradually expanded to effectively improve the surface structure stability and service life of key components such as gas shower heads and ceramic windows. However, the linear thin film deposition characteristics of PEPVD make it impossible for this process to effectively coat and protect certain key components such as the pores of the gas shower head and the inside of the gas pipeline, and it is impossible to deposit a plasma-etching-resistant protective film on the inner surface of the pores. In this way, it is impossible to avoid the metal and particle contamination of the inner surface of the pores due to corrosion by the reaction gas or plasma etching during the plasma etching process.

[0066] Most cylindrical workpieces and gas pipe workpieces used in semiconductor equipment are made of aluminum alloy or stainless steel, and have the same problems as above. Since these workpieces are usually used to transport plasma or various reactive gases, their inner surfaces will inevitably be corroded by plasma and reactive gases. Conventional coating processes (such as PS, PECVD and PVD, etc.) cannot achieve good film protection for the inner surfaces of these workpieces, and can only use anodizing methods. As mentioned above, this will cause many processes to be contaminated by metals and particles. Moreover, for stainless steel gas pipes with a small diameter (such as less than 1 cm), when they are corroded by reactive gases (such as Cl2, NF3 and HBr, etc.), especially when they are corroded at temperatures of 150°C and above, since the inner surface cannot be effectively protected by the surface coating, its surface structure is very easy to produce particles and trace elements, thereby introducing pollution of raw particles and trace elements during the chip processing process. To address this problem, generally only expensive hafnium alloys or heat-resistant alloys with high Cr and high Ni content can be used.

[0067] In view of this, the embodiment of the present application provides a semiconductor device and a surface coating method thereof, which can be used for thin film deposition (such as PVD, CVD, etc.) equipment and important components of plasma etcher (Plasma Etcher), such as flat plate-type key workpieces (such as SH, etc.) and hollow cylindrical workpieces (such as cylinders and air pipes, etc.). The surface coating method is a comprehensive surface coating protection method for the surface of a material that can effectively enhance the working stability. Even when the diameter and depth of the circular hole reach 1:200, an effective protective layer can be prepared on the inner surface of the cylindrical workpiece to extend the service life of the workpiece. The technical solution of the present application can effectively enhance the process stability of semiconductor equipment (such as thin film deposition and plasma etching equipment), significantly reduce the risk of particle pollution and trace element pollution in the process of different semiconductor equipment, thereby improving the process stability of integrated circuit chip production, improving production efficiency, and reducing the production cost of semiconductor equipment.

[0068] In order to make the above-mentioned objects, features and advantages of the present application more obvious and easy to understand, the present application is further described in detail below in conjunction with the accompanying drawings and specific implementation methods.

[0069] refer to Figure 1 , Figure 1 A schematic flow chart of a method for coating a semiconductor device surface provided in an embodiment of the present application, the method for coating a semiconductor device surface comprising:

[0070] Step S11: providing a device body to be coated;

[0071] In the embodiments of the present application, the semiconductor equipment includes thin film deposition equipment and plasma etc. The equipment body includes any workpiece in the semiconductor equipment that needs to be in contact with the reaction gas or plasma, such as a shower head, a gas pipeline, and a reaction chamber. The embodiments of the present application do not limit the specific methods of the semiconductor equipment and the equipment body.

[0072] Step S12: forming a first protective layer on the surface of the device body; wherein the first protective layer at least includes a first sub-protective layer formed based on an atomic layer deposition process.

[0073] The atomic layer deposition process is a special chemical vapor deposition process that grows a single layer of atoms. The film growth process can be carried out at a low temperature and low pressure environment of 450°C. Unlike ordinary CVD, the chemical reaction precursor in the atomic layer deposition process does not decompose before it contacts the surface of the device body to be coated. Instead, after being adsorbed on the surface of the device body, a chemical decomposition reaction occurs on the surface of the device body, and the chemical components formed by the decomposition are evenly covered on the entire surface of the device body to form an atomic layer film. Therefore, as long as the distribution of the reaction gas is controlled during the atomic layer deposition process so that the chemical reaction precursor can fully diffuse and contact the surface of the component, and the remaining precursor is purged for a sufficient time to remove the remaining precursor, the atomic layer deposition process can form a uniform multi-atomic layer stacked film on the device body with a complex surface (such as a device body with a complex geometric surface, the inner and outer walls of a cylindrical tube, and the inner surface of a small pore). Since the atomic layer growth film is formed by the decomposition of the precursor, the film structure formed by the atomic layer deposition process is very dense, which can form a full-range surface coverage of the device body, and the film has good interface bonding and thermal stability.

[0074] Optionally, in an embodiment of the present application, the method for forming the first sub-protective layer includes: using an atomic layer deposition process to sequentially form multiple layers of atomic layer films on the surface of the device body as the first sub-protective layer. The thickness of the first sub-protective layer can be precisely controlled by controlling the number of cycles of depositing the atomic layer films.

[0075] refer to Figure 2 As shown, Figure 2 A flow chart of a method for forming a first sub-protective layer provided in an embodiment of the present application, wherein the first sub-protective layer includes a multi-layer atomic layer film, and the method for forming the first sub-protective layer includes:

[0076] Step S21: forming a first atomic layer film based on saturated chemical adsorption and reaction between the first precursor and the surface of the device body;

[0077] Step S22: forming another atomic layer film based on the saturated chemical adsorption and reaction between the second precursor and the surface of the previous atomic layer film.

[0078] Before forming a next atomic layer film, the precursor used to form the previous atomic layer film is purged and discharged.

[0079] The number of cycles for depositing the atomic layer film is set based on demand, so that the thickness of the first sub-protective layer can be accurately controlled.

[0080] refer to Figure 3-Figure 6 As shown, Figure 3-Figure 6 A schematic diagram of the principle of a method for manufacturing a first sub-protective layer in different process steps provided in an embodiment of the present application, the manufacturing method includes:

[0081] First, if Figure 3 As shown, the first precursor 11 is introduced, and the first atomic layer film 12 is formed based on the saturated chemical adsorption and reaction between the first precursor 11 and the surface of the device body 13.

[0082] Then, if Figure 4 As shown, the first precursor 11 is exhausted by purging.

[0083] For example Figure 5 As shown, the second precursor 14 is introduced, and the second atomic layer film 15 is formed based on the saturated chemical adsorption and reaction between the second precursor 14 and the surface of the first atomic layer film 12 .

[0084] For example Figure 6 As shown, the second precursor 14 is exhausted by purging.

[0085] exist Figure 3-Figure 6 In the method shown, the formation method of the first sub-protective layer is illustrated by taking the formation of two layers of atomic layer films as an example. As mentioned above, in the embodiment of the present application, the number of cycles of depositing the atomic layer film can be set based on demand, and the thickness of the first sub-protective layer can be accurately controlled. Among them, the precursors used in different atomic layer films can be the same or different, and the precursor components are set based on the reaction requirements, which is not limited in the embodiment of the present application.

[0086] In the embodiment of the present application, the first protective layer at least includes a first sub-protective layer formed based on the atomic layer deposition process, which is used to protect the surface of the equipment body and prevent the surface of the equipment body from being corroded by the reaction gas and plasma. Compared with conventional limited coating methods such as CVD and PVD, the first sub-protective layer formed by the atomic layer deposition process includes the following advantages: the first sub-protective layer is a dense thin film without pinholes formed by low-temperature deposition, which can effectively avoid the erosion of reaction gases and plasma; it can form a large-area film on the surface of various equipment bodies with complex shapes in all directions; it can accurately control the composition and thickness of the film, and the thickness variation range can be increased from 1nm to more than 10μm; the film penetration is excellent, and the width-to-depth ratio of the film can reach more than 1:200, which is convenient for film formation on the inner surface of deep holes and pipes; the film has good bonding with the equipment body and good high temperature resistance.

[0087] In order to improve the interfacial bonding force of the first sub-protective layer on the device body, before forming the first protective layer, the surface of the device body is pretreated so that the surface of the device body is modified to improve the adhesion stability of the first sub-protective layer on the surface of the device body.

[0088] In order to improve the interfacial bonding strength of the first sub-protective layer on the surface of the equipment body, before forming the first sub-protective layer, the surface of the equipment body is pretreated so that the thickness of part of the side of the equipment body to be coated is converted into a gentle transition layer. The first sub-protective layer has better adhesion stability in the gentle transition layer to improve the adhesion stability of the first sub-protective layer on the surface of the equipment body.

[0089] refer to Figure 7 As shown, Figure 7 A schematic flow chart of another semiconductor device surface coating method provided in an embodiment of the present application, the surface coating method comprising:

[0090] Step S31: providing a device body to be coated.

[0091] Step S32: pre-treating the surface of the device body to improve the adhesion stability of the first sub-protective layer on the surface of the device body.

[0092] Step S33: forming a first protective layer on the surface of the device body; wherein the first protective layer at least includes a first sub-protective layer formed based on an atomic layer deposition process (ALD).

[0093] based on Figure 1 The method shown, Figure 7 In the method shown, the surface of the device body is pretreated before forming the first protective layer, which can improve the adhesion stability of the first sub-protective layer on the surface of the device body.

[0094] Optionally, the method for pre-treating the surface of the device body includes: using a first plasma immersion process to modify the surface of the device body so that a gentle transition layer with a gradual change in doping components is formed on the surface of the device body.

[0095] The first plasma immersion process is adopted to place the device body in a plasma immersion environment, and the surface of the device body is modified, which can achieve all-round surface modification. It can be applicable to the surface modification of the device body with complex geometric surfaces, inner and outer walls of cylindrical tubes, and inner surfaces of fine pores, so as to improve the surface bonding force of the first protective layer.

[0096] Compared with the method of directly forming a protective layer on the surface of the device body based on the atomic layer deposition process, Figure 7 The method shown combines plasma immersion process and atomic layer deposition process, and can perform high-quality all-round coating on the surface of the device body. The first protective layer formed on the surface of the device body has better interface bonding strength and controllable density with the surface of the device body within a certain thickness.

[0097] Plasma immersion process, its process principle is as follows Figure 8 shown.

[0098] refer to Figure 8 As shown, Figure 8 A schematic diagram of the principle of a plasma immersion process provided in an embodiment of the present application is provided, wherein the device body 13 to be processed is placed in the reaction chamber 21 of the plasma immersion device, and after evacuation through the vacuum port 211, the reaction gas is input into the reaction chamber 21 through the reaction gas supply device 23. The reaction chamber 21 is connected to one or more external plasma generating power supplies 22, and the reaction gas in the reaction chamber 21 is excited or ignited by the external plasma generating power supply 22 to form a plasma. The device body 13 will be immersed and surrounded by the formed plasma. The device body 13 is placed on a tray, and the device body 13 has a pulse bias based on the external signal source 24 connected to the tray, and as the density and bias of the plasma change, the charged ions and active chemical components in the plasma surrounding the device body 13 interact with the surface of the device body in all directions.

[0099] The inventors found that in the plasma immersion process, different process effects can be achieved by adjusting the pulse bias voltage. Under ultra-high pulse bias voltage (>30kV), ion implantation (Plasma immersion ion implantation, referred to as PIII) can be performed on the surface of the workpiece in all directions; within the appropriate bias voltage range (5kV-35kV), workpiece surface alloying (Plasma immersion ion alloying, referred to as PIIA) or surface doping (Plasma immersion ion doping, referred to as PIID) can be achieved; under a relatively low negative bias voltage (<15kV), omnidirectional coating (Plasma immersion ion deposition, referred to as PIID) can be achieved on the surface of the workpiece; under a lower bias voltage (<1kV), energetic ion bombardment cleaning (Plasma immersion ion cleaning, referred to as PIIC) can be performed on the surface of the workpiece. In addition, since PIID uses energetic ions to perform all-round coating on the workpiece surface under a relatively low bias voltage, PIID also has the function of ion beam assisted deposition (IBAD) and forms a dense thin film structure, and can form a film on the workpiece surface at a low temperature (<300°C).

[0100] Due to the numerous functions mentioned above, PIIP can perform all-round surface treatment on the surfaces of many different materials (such as metals, plastics and ceramics, etc.), and the film formed on the surface of the equipment body has very good interface bonding force. This is because PIIP can form an interface transition layer with a gentle chemical composition on the surface of the workpiece.

[0101] Although for some non-penetrating blind holes with smaller diameters (<1 mm), PIIP is not easy to form a uniform modified layer on the inner surface of the deep hole due to the limitations of gas diffusion and the formation of plasma electric field distribution, the technical solution of this application combines it with the atomic layer deposition process, and the first sub-protection prepared by the atomic layer process can achieve all-round thin film protection. The surface pretreatment based on PIIP can further improve the interface bonding force of the first sub-protection layer on the surface of the equipment body to a certain extent. Moreover, in semiconductor equipment, the equipment body used to accommodate reaction gases and plasma generally does not have a small diameter blind hole.

[0102] refer to Fig. 9 As shown, Fig. 9The schematic diagram of the principle of modifying the surface of the device body provided in the embodiment of the present application, wherein the plasma 10 is controlled by the pulse bias voltage to modify the device body 13. Based on the above description, by adjusting the pulse bias voltage during the PIIP process, different modification treatments can be achieved on the surface of the device body, from the inside of the device body 13 to the surface to be coated (i.e. Fig. 9 In the direction from right to left), the device body 13 includes: a first injection zone, a second injection zone and a surface film. The doping components in the first injection zone, the second injection zone and the surface film increase successively. Among them, the first injection zone is the above-mentioned PIII doping process, the second injection zone is the above-mentioned PIIA doping process or surface alloying process, and the surface film is the above-mentioned PIID coating process. Among them, the doping depths of the first injection zone and the second injection zone in this direction decrease successively, and the concentrations of the doping components increase successively, so that the surface of the device body 13 has a gentle transition layer with increasing doping components, which can improve the interface bonding force of the first sub-protective layer formed subsequently on the surface of the device body.

[0103] Based on the above description, in the surface coating method provided in the embodiment of the present application, the method of modifying the surface of the device body by using the first plasma immersion process is as follows: Fig.10 shown.

[0104] refer to Fig.10 As shown, Fig.10 A flow chart of a method for modifying the surface of a device body provided in an embodiment of the present application, the method comprising:

[0105] Step S41: performing ion implantation to a first depth into the surface of the device body under a first pulse bias voltage;

[0106] Step S42: Under a second pulse bias voltage, ion implantation to a second depth is performed into the surface of the device body, and / or surface alloying of the device body is achieved;

[0107] The second depth is smaller than the first depth.

[0108] Based on the first pulse bias, a first injection region can be formed on the surface of the device body, and based on the second pulse bias, a second injection region or surface metallization can be formed on the surface of the device body, thereby forming a gentle transition layer with increasing doping components on the surface of the device body to improve the interface bonding force of the first sub-protective layer formed subsequently on the surface of the device body. Moreover, the gentle transition layer can not only improve the interface bonding force of the first sub-protective layer on the device body, but also further increase the corrosion resistance and high temperature resistance of the surface of the device body.

[0109] In other methods, the surface of the equipment body is modified, and a doping layer can also be formed on the surface of the equipment body based on the plasma immersion process. The doping layer can be a doping area with uniform doping components formed based on a constant pulse bias, such as a doping area formed based on a PIII process, or a doping area formed based on a PIIA process, or it can include the above-mentioned first doping area and the second doping area at the same time, and the doping components of the two doping areas are gradually changed. Among them, the gradual change of the doping component refers to the gradual change of the concentration of the doping element. In this way, the interfacial bonding force of the first sub-protective layer can also be improved to a certain extent.

[0110] In the embodiment of the present application, compared with the solution of forming the first protective layer on the surface of the device body based on a single atomic layer deposition process, the solution of forming the first protective layer on the surface of the device body by combining the plasma immersion process and the atomic layer deposition process can improve the interface bonding force between the first protective layer and the device body based on the gentle transition layer formed on the surface of the device body by the plasma immersion process. Moreover, compared with the plasma immersion process, the atomic layer deposition process has a higher film coverage width-to-depth ratio, and it is easier to form a uniform film coverage on the surface of the device body with a complex structure and inner holes, and the film thickness control accuracy is very high (the thickness change is generally less than 5%).

[0111] Optionally, based on any of the above methods, in the surface coating method provided in the embodiment of the present application, the method for forming the first protective layer also includes: using a second plasma immersion process to form a second sub-protective layer on the surface of the first sub-protective layer. The protective layer is provided to include a first sub-protective layer and a second sub-protective layer, and the device body can be protected against corrosion by the protective layer when a first sub-protective layer of smaller thickness is used. The thickness of the second sub-protective layer can be 50nm-15μm. Furthermore, when the thickness of the second sub-protective layer can be set to 500nm-1μm, the first protective layer can achieve better corrosion protection.

[0112] Since the atomic layer deposition process forms thin films slowly, and the cost rises rapidly with the increase of film thickness, the thickness of the first sub-protective layer formed based on the atomic layer deposition process is generally thin, and the thickness of the first sub-protective layer is less than 2000nm. In some cases, the thickness of the first sub-protective layer is less than or equal to 500nm. If the thickness of the first sub-protective layer is too large, it will not only lead to a significant increase in production costs, but also cause the film grains to become coarse and the surface structure to coarsen. In order to improve the quality of the all-round protective layer on the surface of the equipment body and expand the application scope of the all-round protective layer, the embodiment of the present application is provided on the first sub-protective layer. A second sub-protective layer prepared based on a plasma immersion process is used to increase the thickness of the first protective layer. In this way, a thinner first sub-protective layer can be formed based on the atomic layer deposition process to achieve better corrosion protection effect.

[0113] Optionally, a second plasma immersion process is used to form a second sub-protective layer on the surface of the first sub-protective layer, including: performing omnidirectional coating on the surface of the device body formed with the first sub-protective layer under a negative bias voltage of less than 15 kV to form the second sub-protective layer. At this time, a surface film layer can be formed on the surface of the device body based on the above-mentioned PIID process.

[0114] In order to further improve the corrosion resistance of the equipment body, the surface coating method also includes: forming a second protective layer on the surface of the first protective layer; wherein the thickness of the second protective layer may be greater than the thickness of the first protective layer.

[0115] Optionally, the method for forming the second protective layer includes: forming the second protective layer by a plasma enhanced physical vapor deposition process. For a device body having a pore with a smaller diameter, the thinner first protective layer covers the surface of the device body in all directions, including the inner wall of the pore, and the thicker second protective layer covers the surface outside the pore and the inner wall near the pore mouth.

[0116] The plasma enhanced physical vapor deposition process is essentially a surface thin film deposition process that combines the physical vapor deposition process with the plasma enhanced process. Among them, the PVD process can be carried out through vacuum evaporation, ion bombardment sputtering, magnetron sputtering and other process methods, while the plasma enhancement function can be achieved through ion bombardment in the plasma and ion beam bombardment. Due to the bombardment effect of ions, the weak atomic bonds in the film growth process can be broken, prompting the surface diffusion of atoms to form a dense crystalline or amorphous structure with consistent orientation. Therefore, compared with the films prepared by other thin film deposition processes such as evaporation and plasma spraying, the film structure formed by the plasma enhanced physical vapor deposition process is dense, and the plasma etching resistance is greatly enhanced. In addition, because it is a combination of physical vapor deposition and plasma processes, the plasma enhanced physical vapor deposition process can be carried out on the surface of the equipment body at a lower temperature (<200℃), and the film thickness can reach more than 150μm, which is very suitable for depositing ceramic films of sufficient thickness (>20um) such as Y2O3 on the surface of the equipment body made of aluminum alloy.

[0117] The surface coating method described in the embodiment of the present application is further described below by taking the device body as a shower head as an example.

[0118] refer to Figure 11-13 As shown, Fig.11 This is a top view of the device body. Fig.12 for Fig.11 The cross-sectional view of the device body is shown. Fig.13 for Fig.11 The enlarged partial view of the device body is shown. Figure 11-13In the illustrated embodiment, the device body 13 is a shower head having air holes 131 , and no protective layer is provided on the surface of the device body 13 , which makes the surface of the device body 13 susceptible to corrosion by the reaction gas and plasma.

[0119] The thickness of the shower head is generally 3 mm to 100 mm, and the diameter of the air hole 131 can be from 0.04 mm to 100 mm. The diameter of the air hole 131 of some shower heads can be greater than 100 mm. In the embodiment of the present application, the uniform diameter of the air hole 131 is used as an example for illustration. In other embodiments, the air hole 131 can also be composed of pipes of different diameters.

[0120] refer to Fig.14 As shown, Fig.14 This is a partial enlarged view of a device body having a corrosion-resistant protective layer formed by the coating method according to an embodiment of the present application. Figure 11-13 Based on the method shown, Fig.14 In the shown manner, a first protective layer 31 is formed on the surface of the device body 13, and the first protective layer 31 includes a first sub-protective layer 311. The first sub-protective layer 311 formed based on the atomic layer deposition process has excellent film penetration, and the width-to-depth ratio of the thin film can reach 1:200 or more, so it can form a full-range thin film coverage on the surface of the device body 13 to form a good corrosion-resistant protective layer.

[0121] refer to Fig.15 As shown, Fig.15 FIG. 1 is a partial enlarged view of another device body having a corrosion-resistant protective layer formed thereon based on the coating method of an embodiment of the present application. Fig.14 Based on the method shown, Fig.15 In the illustrated embodiment, before forming the first protective layer 31 , the surface of the device body 13 is pretreated to form a modified layer 32 to improve the interface bonding force of the first protective layer 31 on the device body 13 .

[0122] refer to Fig.16 As shown, Fig.16 FIG. 1 is a partial enlarged view of another device body having a corrosion-resistant protective layer formed thereon based on the coating method of an embodiment of the present application. Fig.15 Based on the method shown, Fig.16 In the illustrated method, a second sub-protective layer 312 is also formed on the surface of the first sub-protective layer 311. As mentioned above, the first sub-protective layer 311 is limited by the atomic layer deposition process, the film forming speed is slow, and a thick film cannot be formed. In this method, the second sub-protective layer 312 is also formed on the surface of the first sub-protective layer 311, which can achieve better corrosion resistance based on the thinner first sub-protective layer 311.

[0123] refer to Fig.17 As shown, Fig.17FIG. 1 is a partial enlarged view of another device body having a corrosion-resistant protective layer formed thereon based on the coating method of an embodiment of the present application. Fig.16 Based on the method shown, Fig.17 In the illustrated embodiment, a second protective layer 33 prepared based on the PEPVD process is also formed on the surface of the first protective layer 31 .

[0124] It can be seen from the above description that the surface coating method described in the technical solution of the present application is based on the modified layer 32 formed on the surface of the device body 13 by the plasma immersion process. The modified layer 32 is a gentle transition layer with a gradual change in doping components, which is used to enhance the interface bonding force of the first sub-protective layer 311 formed subsequently. It is convenient to form a dense first sub-protective layer 311 on the modified layer 32 formed by the plasma immersion process. Compared with the plasma immersion process, the first sub-protective layer 311 formed by the atomic layer deposition process has a very high film coverage width-to-depth ratio. Therefore, the surface coating method provided by the technical solution of the present application uses an atomic layer deposition process to form a first sub-protective layer 311 with uniform thickness and composition on the modified layer 32 formed by the plasma immersion process, which can cover the entire outer surface of the device body 13 and the inner surface of the pore 131. In order to ensure that the surface protective layer with all-round coverage finally formed has a fine and dense organizational structure, a second sub-protective layer 312 is prepared on the first sub-protective layer 311 based on the plasma immersion process to further increase the thickness of the first protective layer 31. The surface protection layer prepared in this way is very suitable for the surface protection of flat workpieces used in semiconductor coating equipment such as PVD and CVD, such as a shower head made of aluminum alloy.

[0125] In the embodiment of the present application, the first protective layer 31 includes a ceramic film to form a ceramic protective film that covers the surface of the device body 13 in all directions. The first sub-protective layer 311 is a ceramic film. When the first protective layer 31 also includes a second sub-protective layer 312, the second sub-protective layer 312 is a ceramic film.

[0126] In order to enhance the structural stability of the first protective layer 31 formed on the surface of the equipment body 13 and meet the working requirements of the use environment, it is preferred to use a plasma corrosion-resistant film with a chemical composition and a structural structure similar to that of the equipment body 13 as the first sub-protective layer 311 combined with the equipment body 13 and deposited on the surface of the equipment body 13. When the first sub-protective layer 311 is a ceramic film, the alloy elements in the ceramic film are the same as the material of the equipment body 13. When the ceramic film is deposited on the surface of the equipment body 13, it has a smaller interface deformation stress, which is conducive to improving the structural stability of the formed ceramic film. For example, when an aluminum alloy equipment body 13 is used, an Al2O3 film is deposited on its surface as the first sub-protective layer 311; when a silicon-based equipment body 13 is used, a SiC film is deposited on its surface as the first sub-protective layer 311; when a yttrium alloy equipment body 13 is used, a Y2O3, YF3 or YOF film is deposited on its surface as the first sub-protective layer 311.

[0127] When the first sub-protective layer 311 is a ceramic film, the alloy elements in the ceramic film are the same as the material of the device body 13, and the interface bonding force between the ceramic film and the device body 13 can be improved. The amorphous structure characteristics of the ceramic film can effectively prevent the trace elements in the device body 13 from diffusing to the surface of the ceramic film, thereby reducing the trace element contamination caused by the device body 13 during the use of the semiconductor device. For shower heads made of aluminum alloy that are often used under high temperature conditions, such as shower heads used in PVD equipment and CVD equipment, the operating temperature may be above 150°C or even 300°C. The amorphous all-round covering ceramic film as the first sub-protective layer 311 can play a good role in reducing trace element contamination.

[0128] In the semiconductor device improved by the embodiment of the present application, the first sub-protective layer 311 is a multi-layer thin film structure, and by setting the thin film properties and the order of formation, the required protection device body 13 has a very excellent performance combination in different use environments.

[0129] Taking the device body 13 made of aluminum alloy as an example, the first sub-protective layer 311 includes an aluminum oxide ceramic film. A doping layer can be formed by implanting oxygen ions into the surface of the device body 13, and the doping layer serves as a modified layer 32 to enhance the interfacial bonding force of the aluminum oxide film subsequently formed. After the modified layer 32 is formed on the surface of the device body 13, an amorphous aluminum oxide ceramic film is formed on the surface of the modified layer 32, which can not only enhance the surface corrosion resistance of the aluminum alloy device body 13, but also prevent the alloy elements in the aluminum alloy from diffusing to the surface, enhance the surface tissue stability of the device body 13, and reduce the pollution of trace elements.

[0130] The first sub-protection layer 311 at least includes a first ALD film located on the surface of the device body 13 and a second ALD film located on the surface of the first ALD film, and the first ALD film is in contact with the surface of the device body.

[0131] The corrosion resistance of the second ALD film is stronger than that of the first ALD film, and the two have similar thermal expansion coefficients. In this way, the corrosion resistance of the first sub-protection layer 311 can be further enhanced by the second ALD film. Taking the first ALD film as aluminum oxide and the second ALD film as yttrium oxide as an example, the material properties of the two are shown in Table 1 below.

[0132] Table 1

[0133]

[0134] Table 1 shows the thermal expansion coefficient of the material at 200-1000°C and the thermal conductivity coefficient at 20°C. As shown in Table 1, the thermal expansion coefficients of aluminum oxide and yttrium oxide are very close, and the plasma corrosion resistance of yttrium oxide in different plasma environments (such as those containing O2, F, Cl, and HBr, etc.) is much higher than that of aluminum oxide. Therefore, depositing an yttrium oxide film on the surface of the aluminum oxide film can further enhance the corrosion resistance of the first protective layer 31, improve the process stability of the device body 13 (such as a shower head) and the application range in different semiconductor devices.

[0135] In order to further improve the bonding strength between the second ALD film and the first ALD film, a transition layer may be formed between the two. Taking the case where the first ALD film is amorphous aluminum oxide and the second ALD film is crystalline yttrium oxide as an example, the transition layer between the two may be a crystalline aluminum oxide film. In this case, the multilayer film structure of the first sub-protective layer 311 includes: amorphous aluminum oxide / crystalline aluminum oxide / crystalline yttrium oxide.

[0136] In order to improve other properties of the first sub-protective layer 311, such as thermal conductivity and electrical conductivity, a thermally conductive / conductive film can be added to the first sub-protective layer 311, so that the first sub-protective layer 311 has good thermal and electrical conductivity while achieving corrosion resistance, thereby forming a multifunctional first sub-protective layer 311. Ions can also be implanted into the single-element film in the first sub-protective layer 311 to change the film properties. The thickness of the first sub-protective layer 311 and the combination of the thickness of different films can be set according to different process conditions and the properties of the film material, and the embodiments of the present application do not limit this.

[0137] From the above description, it can be seen that the surface coating method provided by the technical solution of the present application is capable of performing surface coating on workpieces with complex structural surfaces in semiconductor equipment, such as surface coating on shower heads, cylindrical workpieces, and gas pipe workpieces. Combining the atomic layer deposition process and the plasma immersion process can achieve all-round coating on the surface of the equipment body, effectively solving the surface protection problem of workpieces with complex structural surfaces in semiconductor equipment.

[0138] This surface coating method exploits the versatility of the plasma immersion process and improves the bonding strength and surface density of all-round thin films based on PIII and PIID. It can effectively improve the quality of thin films formed by single ALD, enhance the organizational stability of all-round thin films, reduce the particles and trace element contamination generated by the corrosion of the surface of workpieces such as the protected cavity workpiece by reaction gas or plasma, and improve the process stability of semiconductor equipment.

[0139] Moreover, the surface coating method can prepare multi-layer atomic layer films on the surface of the device body according to the working environment requirements of the semiconductor device and the mutual matching compatibility of the organizational structure and performance of different thin film materials, using the stability and process controllability of the ALD process to prepare thin films; through the design of thin film materials, an interface layer with strong bonding force, a ceramic film with surface resistance to plasma corrosion, and a multi-layer structure with special functions (heat resistance / thermal conductivity / electrical conductivity, etc.) are formed on the surface of the device body to meet the working requirements of different semiconductor devices.

[0140] Furthermore, according to the plasma etching characteristics of the semiconductor device, combined with the PEPVD process, a second protective layer with a larger thickness can be deposited on the surface of the prepared first protective layer with all-round coverage, so as to further improve the plasma corrosion resistance, improve the critical service life and process stability of plasma etching.

[0141] Based on the above surface coating method embodiment, another embodiment of the present application further provides a semiconductor device, such as the above semiconductor device including but not limited to thin film deposition equipment and plasma etcher. The semiconductor device includes: a device body, which can be a flat workpiece in the semiconductor device, such as a shower head, or other transmission pipelines, or a reaction chamber, etc.

[0142] Combination Fig.14 In the illustrated embodiment, the semiconductor device includes: a device body 13, and a first protective layer 31 covering the device body 13, wherein the first protective layer 31 includes at least a first sub-protective layer 311 formed based on an atomic layer deposition process.

[0143] Optionally, in the embodiment of the present application, the first protective sublayer 311 includes a plurality of atomic layer films stacked in sequence. Based on the number of atomic layer depositions, the thickness of the first protective sublayer 311 can be precisely controlled.

[0144] Combination Fig.15 In the illustrated embodiment, the surface of the device body is modified so that a certain thickness portion of the surface of the device body serves as a modified layer 32 to improve the adhesion stability of the first sub-protective layer 311 on the surface of the device body 13 .

[0145] Combination Fig.16 In the illustrated embodiment, the first protective layer 31 further includes: a second sub-protective layer 312 located on the surface of the first sub-protective layer 311; wherein the second sub-protective layer 312 is a film layer formed by a plasma immersion process.

[0146] In the embodiment of the present application, the first protective layer 31 includes a ceramic film, thereby forming a ceramic protective film that covers the surface of the device body 13 in all directions. The first sub-protective layer 311 can be a ceramic film. When the first protective layer 31 also includes a second sub-protective layer 312, the second sub-protective layer 312 is a ceramic film.

[0147] Among them, the materials of ceramic films include: Al2O3, Y2O3, YF3, YOF (such as Y5O4F7), ZrO2, Er2O3, SiC, SiO2, HfO2, Si3N4, AlN, B2O3, Nd2O3, Nb2O5, CeO2, Sm2O3, Yb2O3, Y3Al5O 12 (YAG), Er3Al5O 12 One or more of Y4Al2O9 (EAG), Y4Al2O9 (YAM), YAlO3 (YAP), Er4Al2O9 (EAM) and ErAlO3 (EAP), or composite ceramic films based on these ceramic materials, have the common characteristics of being resistant to plasma corrosion, stable performance, and their corrosion resistance and stability are far superior to aluminum alloy workpiece materials.

[0148] Combination Fig.17 In the illustrated embodiment, the semiconductor device further includes: a second protective layer 33 located on the surface of the first protective layer 31; optionally, the second protective layer 33 is a plasma enhanced physical vapor deposition film.

[0149] The thickness of the second protective layer 33 may be greater than that of the first protective layer 31. Alternatively, the thickness of the second protective layer 33 may be less than that of the first protective layer 31 by setting the coating time of the coating process.

[0150] The thickness of the first protective layer 31 is less than 25 μm, and the thickness of the second protective layer 33 is greater than 10 μm.

[0151] Optionally, the second protective layer 33 is a ceramic film, and the material of the ceramic film can be as described above, which will not be described in detail here.

[0152] The thickness of the first protective layer 31 prepared based on the atomic layer deposition process and the plasma immersion process is generally thin, less than 10 μm in some cases, or even less than 2 μm. Therefore, in the plasma etching process, the first protective layer 31 may be corroded by the plasma due to its thin thickness. This problem can be solved by adding a second protective layer 33 with a larger thickness on the surface of the first protective layer 31.

[0153] The second protective layer 33 is a dense plasma corrosion resistant film prepared by PEPVD process, with a thickness greater than 10 μm, such as 20 μm-150 μm. The second protective layer 33 prepared by PEPVD process has good density, no defects, and is resistant to plasma corrosion.

[0154] exist Fig.17 In the figure, the device body 13 is taken as a shower head as an example for illustration. The shower head is made of aluminum alloy. After the first protective layer 31 is formed on its surface, a thick second protective layer 33 is deposited by the PEPVD process. The material 32 of the second protective layer 33 can be Y2O3 or YF3. The surface film structure of the shower head may include: a modified layer 32 prepared based on the PIIP process, amorphous aluminum oxide (amorphous Al2O3, or a-Al2O3) and crystalline yttrium oxide (Y2O3) prepared based on the ALD process, and a Y2O3 thick film prepared based on the PEVD process, so that the surface of the shower head in contact with the plasma has a thicker, dense, plasma-resistant corrosion-resistant protective layer to ensure the service life of the shower head. The inner wall of the shower head pore can be protected by the thin first protective layer 31 that covers all directions to avoid corrosion by the reaction gas, thereby ensuring that no metal and particle pollution is generated during the operation of the shower head. Therefore, when the technical solution of the present application is used for a shower head, it can significantly improve the long-term process stability of semiconductor equipment using the shower head, thereby achieving the purpose of improving production efficiency.

[0155] In this specification, each embodiment is described in a progressive, parallel, or progressive and parallel manner. Each embodiment focuses on the differences from other embodiments, and the same or similar parts between the embodiments can be referred to each other. For the semiconductor device disclosed in the embodiment, since it corresponds to the surface coating method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the relevant part of the surface coating method.

[0156] It should be noted that in the description of the present application, it should be understood that the description of the drawings and embodiments is illustrative rather than restrictive. The same drawings throughout the embodiments of the specification mark the same structure. In addition, for the sake of understanding and ease of description, the drawings may exaggerate the thickness of some layers, films, panels, regions, etc. It is also understood that when an element such as a layer, film, region or substrate is referred to as "on" another element, the element may be directly on the other element or there may be an intermediate element. In addition, "on" refers to positioning an element on or below another element, but does not essentially mean positioning on the upper side of another element according to the direction of gravity.

[0157] The terms "upper", "lower", "top", "bottom", "inner", "outer", etc. indicate positions or positional relationships based on the positions or positional relationships shown in the drawings, and are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present application. When a component is considered to be "connected" to another component, it may be directly connected to the other component or there may be a centrally arranged component at the same time.

[0158] It should also be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "comprises", "comprising" or any other variants thereof are intended to cover non-exclusive inclusion, so that an article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such article or device. In the absence of further restrictions, the elements defined by the sentence "comprising a ..." do not exclude the existence of other identical elements in the article or device including the above elements.

[0159] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A surface coating method for semiconductor equipment, It is characterized in that include: Provide the equipment body to be coated; A first protective layer is formed on the surface of the device body; wherein the first protective layer at least includes a first sub-protective layer formed based on an atomic layer deposition process.

2. The surface coating method according to claim 1, It is characterized in that The method of forming the first sub-protection layer includes: An atomic layer deposition process is adopted to sequentially form multiple layers of atomic layer films on the surface of the device body as the first sub-protective layer.

3. The surface coating method according to claim 2, It is characterized in that The method of forming the first sub-protection layer includes: forming a first atomic layer film based on saturated chemical adsorption and reaction between the first precursor and the surface of the device body; forming another atomic layer film based on saturated chemical adsorption and reaction between the second precursor and the surface of the previous atomic layer film; Before forming a next atomic layer film, the precursor used to form the previous atomic layer film is purged and discharged.

4. The surface coating method according to claim 1, It is characterized in that Before forming the first protective layer, the method further includes: The surface of the device body is pretreated to improve the adhesion stability of the first sub-protection layer on the surface of the device body.

5. The surface coating method according to claim 4, It is characterized in that The method for pre-treating the surface of the device body comprises: The surface of the device body is modified by a first plasma immersion process, so that a gentle transition layer with a gradual change of doping components is formed on the surface of the device body.

6. The surface coating method according to claim 5, It is characterized in that The surface of the device body is modified by a first plasma immersion process, including: Under a first pulse bias, ion implantation to a first depth is performed into the surface of the device body; Under a second pulse bias, ion implantation to a second depth is performed into the surface of the device body, and / or surface alloying of the device body is achieved; Wherein, the second depth is smaller than the first depth.

7. The surface coating method according to claim 2, It is characterized in that The method of forming the first protective layer further includes: A second plasma immersion process is used to form a second sub-protecting layer on the surface of the first sub-protecting layer.

8. The surface coating method according to claim 7, It is characterized in that Using a second plasma immersion process to form a second sub-protective layer on the surface of the first sub-protective layer includes: Under a negative bias voltage less than 15 kV, an all-round coating is performed on the surface of the device body formed with the first sub-protective layer to form the second sub-protective layer.

9. The surface coating method according to any one of claims 1 to 8, It is characterized in that Also includes: forming a second protective layer on a surface of the first protective layer; Wherein, the thickness of the second protective layer is greater than the thickness of the first protective layer.

10. The surface coating method according to claim 9, It is characterized in that The method of forming the second protective layer includes: The second protective layer is formed by a plasma enhanced physical vapor deposition process.

11. A semiconductor device, It is characterized in that include: Equipment body; A first protective layer covers the device body, wherein the first protective layer at least includes a first sub-protective layer formed based on an atomic layer deposition process.

12. The semiconductor device according to claim 11, It is characterized in that The first sub-protection layer includes a plurality of atomic layer films stacked in sequence.

13. The semiconductor device according to claim 11, It is characterized in that The surface of the device body is modified to improve the adhesion stability of the first sub-protective layer on the surface of the device body.

14. The semiconductor device according to claim 11, It is characterized in that The first protective layer further includes: a second sub-protective layer located on the surface of the first sub-protective layer; Wherein, the second sub-protective layer is a film layer formed by a plasma immersion process.

15. The semiconductor device according to claim 11, It is characterized in that The first protection layer includes a ceramic film.

16. The semiconductor device according to claim 11, It is characterized in that Also includes: A second protective layer is located on a surface of the first protective layer.

17. The semiconductor device according to claim 16, It is characterized in that The second protective layer is a plasma enhanced physical vapor deposition film.

18. The semiconductor device according to claim 16, It is characterized in that The thickness of the first protective layer is less than 25 μm, and the thickness of the second protective layer is greater than 10 μm.

19. The semiconductor device according to claim 16, It is characterized in that The second protective layer is a ceramic film.

20. The semiconductor device according to claim 16, It is characterized in that The thickness of the second protective layer is greater than that of the first protective layer.