Ceramic coating as well as preparation method and application thereof
Through the preparation method of ceramic coating, the problem of wear of the hollow guide shaft body of high-hard particles in air spinning technology is solved, forming a high-hard and wear-resistant coating, extending the service life and improving the yarn quality.
Patent Information
- Application Number
- CN202411086260.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-22
AI Technical Summary
In air spinning technology, the wear of high-hardness particles such as carbon atom particles on the surface of the hollow guide shaft leads to a shortening of their service life, affecting the quality of the yarn and processing efficiency.
The preparation method of ceramic coating is adopted, including cleaning of ceramic material substrates, chemical deposition of boron-doped diamond layer, magnetron sputtering diamond carbon layer and rare earth element Nd, and magnetic field heat treatment to form high hardness and wear-resistant Composite coating.
It significantly extends the service life of the hollow guide shaft body, improves the hardness and wear resistance of ceramic materials, and stably improves the comprehensive quality of the yarn.
Smart Images

Figure CN118996370A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of coating materials, and in particular to a ceramic coating and a preparation method and application thereof. Background Art
[0002] In air spinning technology, the core components of the spinning unit include a precisely designed nozzle block and a high-efficiency hollow guide shaft. Figure 1 The system cleverly uses compressed air to spray out from the nozzle to form a powerful swirling airflow field. This airflow field is like an invisible weaver, leading the end of the fiber bundle to elegantly flip and swirl around the hollow guide shaft, and finally precisely wrap around the core fiber to construct the initial shape of the yarn.
[0003] However, when high-hardness particles, especially carbon atom particles, are mixed in the yarn fibers, these "uninvited guests" become the culprits of the wear on the surface of the hollow guide shaft. Like tiny sandpaper, they constantly rub and erode the surface of the shaft, causing the smoothness of the front hollow port to drop sharply and the surface roughness to increase significantly. This phenomenon poses a severe challenge to hollow guide shafts made of traditional materials such as ordinary metals and ceramic alumina, significantly shortening their service life.
[0004] What is more serious is that as the surface of the hollow guide shaft becomes increasingly worn, its ability to finely process the yarn fibers also decreases. This not only exacerbates the damage to the yarn fibers during processing, but may also introduce more hairiness and irregularities, ultimately causing a profound impact on the quality of the finished yarn. Specifically, it manifests itself in the weakening of yarn strength, the increase of external hairiness, and the decline of hand feel. These subtle but critical changes are directly related to the market competitiveness and consumer satisfaction of the product.
[0005] Therefore, in order to solve this technical problem and improve the overall efficiency and product quality of air spinning technology, it is urgently necessary to develop hollow guide shafts made of new wear-resistant materials, or explore more effective surface protection technologies to reduce the wear of high-hardness particles on the shaft surface, ensure the smooth and efficient yarn production process, and thus steadily improve the overall quality of the finished yarn. Summary of the invention
[0006] In order to solve the above problems, the present invention provides a ceramic coating and a preparation method and application thereof.
[0007] In a first aspect, the present invention provides a method for preparing a ceramic coating, the preparation method comprising the following steps:
[0008] Cleaning the surface of the ceramic material substrate to obtain a first ceramic material substrate;
[0009] Providing a boron-doped diamond layer on the surface of the first ceramic material substrate by chemical deposition to obtain a second ceramic material substrate;
[0010] Providing a diamond-like carbon layer on the surface of the second ceramic material substrate by magnetron sputtering to obtain a third ceramic material substrate;
[0011] The rare earth element Nd is doped into the surface of the third ceramic material matrix, and then subjected to magnetic field heat treatment to obtain the ceramic coating.
[0012] Furthermore, the ceramic material matrix includes an alumina ceramic material matrix and a zirconia ceramic material matrix.
[0013] Furthermore, the cleaning method includes at least one of ultrasonic cleaning, sputtering cleaning and ion etching cleaning.
[0014] Furthermore, the step of providing a boron-doped diamond layer on the surface of the first ceramic material substrate by chemical deposition to obtain the second ceramic material substrate includes the following process:
[0015] The first ceramic material matrix is placed in a chemical deposition device, and then hydrogen, diborane and methane are introduced at a flow rate ratio of (90-95):(2-4):(2-5). Deposition is carried out for 8-10 hours at a deposition temperature of 830-860°C and a deposition pressure of 1-2 kPa to obtain the second ceramic material matrix.
[0016] Furthermore, working condition parameters for providing a diamond-like carbon layer on the surface of the second ceramic material substrate by magnetron sputtering include: sputtering power of 260 to 350 W, sputtering temperature of 150 to 200° C., and sputtering time of 30 to 50 min.
[0017] Furthermore, the step of adding rare earth element Nd to the surface of the third ceramic material matrix and then performing magnetic field heat treatment to obtain the ceramic coating includes the following process:
[0018] The third ceramic material matrix is placed in a metal vapor vacuum arc power ion implantation device, and metal Nd is ion-doped under the condition of an ion voltage of 120-150 keV; after the rare earth element Nd is doped, it is transferred to a magnetic field sintering device, and a magnetic field heat treatment is performed for 1-2 hours under the conditions of an inert gas atmosphere, a temperature of 600-700°C, and a flux coil current of 5-8A, and the ceramic coating is obtained by natural cooling of the device.
[0019] Furthermore, the metal Nd ion doping amount is 5×10 15 ~7×10 15 ions / cm 2 .
[0020] In a second aspect, the present invention provides a ceramic coating, which is prepared by the preparation method described in any one of the first aspects.
[0021] In a third aspect, the present invention provides a use of the ceramic coating described in any one of the second aspects in the preparation of a hollow guide shaft.
[0022] In a fourth aspect, the present invention provides a hollow guide shaft body, the surface of which at least partially includes the ceramic coating described in any one of the second aspects.
[0023] The above technical solution provided by the present invention has at least the following advantages compared with the prior art:
[0024] The present invention provides a method for preparing a ceramic coating. The preparation method comprises a multi-step coating deposition and modification process such as cleaning, chemical deposition of a BDD layer, magnetron sputtering of a DLC layer, doping of a rare earth element Nd, and magnetic field heat treatment. The combination of the BDD layer and the DLC layer forms a composite coating with high hardness, wear resistance, and good chemical stability. The rare earth element Nd has a unique electronic structure and chemical properties, and can change the lattice structure and phase composition of the coating, thereby improving the hardness and wear resistance of the coating. The magnetic field heat treatment promotes the rearrangement and combination of atoms inside the coating through the action of the magnetic field to form a more compact and uniform microstructure, further optimizing the comprehensive performance of the coating, and gradually constructing a composite coating with high hardness and super wear resistance on the surface of the ceramic material substrate. When applied to a ceramic material substrate such as a hollow guide shaft, its service life can be significantly extended, and it has a wide range of practical application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0026] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0027] Figure 1 It is a schematic diagram of the structure of the hollow guide shaft.
[0028] Figure 2 A schematic flow chart of a method for preparing a ceramic coating provided by the present invention. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the drawings of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0031] In a first aspect, the present invention provides a method for preparing a ceramic coating, such as Figure 2 As shown, the preparation method comprises the following steps:
[0032] Cleaning the surface of the ceramic material substrate to obtain a first ceramic material substrate;
[0033] Providing a boron-doped diamond layer on the surface of the first ceramic material substrate by chemical deposition to obtain a second ceramic material substrate;
[0034] Providing a diamond-like carbon layer on the surface of the second ceramic material substrate by magnetron sputtering to obtain a third ceramic material substrate;
[0035] The rare earth element Nd is doped into the surface of the third ceramic material matrix, and then subjected to magnetic field heat treatment to obtain the ceramic coating.
[0036] The present invention provides a method for preparing a ceramic coating. The preparation method comprises a multi-step coating deposition and modification process such as cleaning, chemical deposition of a BDD layer, magnetron sputtering of a DLC layer, doping of a rare earth element Nd, and magnetic field heat treatment. The combination of the BDD layer and the DLC layer forms a composite coating with high hardness, wear resistance, and good chemical stability. The rare earth element Nd has a unique electronic structure and chemical properties, and can change the lattice structure and phase composition of the coating, thereby improving the hardness and wear resistance of the coating. The magnetic field heat treatment promotes the rearrangement and combination of atoms inside the coating through the action of the magnetic field to form a more compact and uniform microstructure, further optimizing the comprehensive performance of the coating, and gradually constructing a composite coating with high hardness and super wear resistance on the surface of the ceramic material substrate. When applied to a ceramic material substrate such as a hollow guide shaft, its service life can be significantly extended, and it has a wide range of practical application value.
[0037] In some specific embodiments, the ceramic material matrix includes an alumina ceramic material matrix and a zirconia ceramic material matrix.
[0038] In some specific embodiments, the cleaning method includes at least one of ultrasonic cleaning, sputtering cleaning and ion etching cleaning.
[0039] In some specific embodiments, the step of providing a boron-doped diamond layer on the surface of the first ceramic material substrate by chemical deposition to obtain the second ceramic material substrate includes the following process:
[0040] The first ceramic material matrix is placed in a chemical deposition device, and then hydrogen, diborane and methane are introduced at a flow rate ratio of (90-95):(2-4):(2-5). Deposition is carried out for 8-10 hours at a deposition temperature of 830-860°C and a deposition pressure of 1-2 kPa to obtain the second ceramic material matrix.
[0041] In some specific embodiments, the working condition parameters for forming a diamond-like carbon layer on the surface of the second ceramic material substrate by magnetron sputtering include: a sputtering power of 260 to 350 W, a sputtering temperature of 150 to 200° C., and a sputtering time of 30 to 50 min.
[0042] In some specific embodiments, the step of adding rare earth element Nd to the surface of the third ceramic material matrix and then performing magnetic field heat treatment to obtain the ceramic coating includes the following process:
[0043] The third ceramic material matrix is placed in a metal vapor vacuum arc power ion implantation device, and metal Nd is ion-doped under the condition of an ion voltage of 120-150 keV; after the rare earth element Nd is doped, it is transferred to a magnetic field sintering device, and a magnetic field heat treatment is performed for 1-2 hours under the conditions of an inert gas atmosphere, a temperature of 600-700°C, and a flux coil current of 5-8A, and the ceramic coating is obtained by natural cooling of the device.
[0044] In some specific embodiments, the amount of metal Nd ions doped is 5×10 15 ~7×10 15 ions / cm 2 .
[0045] In a second aspect, based on the same inventive concept, the present invention provides a ceramic coating, which is prepared by the preparation method described in any one of the first aspects.
[0046] In a third aspect, based on the same inventive concept, the present invention provides an application of the ceramic coating described in any one of the second aspects in the preparation of a hollow guide shaft.
[0047] In a fourth aspect, based on the same inventive concept, the present invention provides a hollow guide shaft body, the surface of which at least partially includes the ceramic coating described in any one of the second aspects.
[0048] It should be noted that the ceramic coating and its preparation method and application provided by the present invention can be directly commercially available unless otherwise specified or described, and the present invention document will not elaborate on it in detail. At the same time, the steps involved in the preparation method can be carried out using existing ceramic coating preparation processes or existing equipment unless otherwise specified or described, and will not be elaborated on one by one here.
[0049] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are intended only to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0050] Example 1
[0051] This example provides a ceramic coating, with a hollow guide shaft as a ceramic material matrix, and the preparation method of the ceramic coating includes the following steps:
[0052] Step (1): subjecting the surface of the ceramic material substrate to ultrasonic cleaning treatment, with an ultrasonic power of 300 W and a cleaning time of 30 minutes, and then vacuum drying in a vacuum drying oven to obtain a first ceramic material substrate;
[0053] Step (2): placing the first ceramic material matrix obtained in step (1) in a chemical deposition device, and then introducing hydrogen, diborane and methane at flow rate ratios of 93 sccm, 3 sccm and 5 sccm, respectively, and performing deposition for 9 hours at a deposition temperature of 845° C. and a deposition pressure of 1.5 kPa to obtain the second ceramic material matrix;
[0054] Step (3): placing the second ceramic material substrate obtained in step (2) in a magnetron sputtering coating device, using a graphite target as a sputtering source and argon gas with a flow rate of 60 sccm as a working gas, performing magnetron sputtering for 38 minutes at a sputtering power of 300 W and a sputtering temperature of 170° C., to obtain a third ceramic material substrate;
[0055] Step (4): Place the third ceramic material matrix obtained in step (3) in a metal vapor vacuum arc power ion implantation device, and dope metal Nd at an ion voltage of 130 keV. The doping amount of Nd ions is 6×10 15 ions / cm 2 After the rare earth element Nd is doped, it is transferred to a magnetic field sintering device, and subjected to magnetic field heat treatment for 1.5 hours under a nitrogen gas atmosphere, a temperature of 650°C and a flux coil current of 6A, and the device is naturally cooled to obtain the ceramic coating.
[0056] Example 2
[0057] This example provides a ceramic coating, with a hollow guide shaft as a ceramic material matrix, and the preparation method of the ceramic coating includes the following steps:
[0058] Step (1): subjecting the surface of the ceramic material substrate to ultrasonic cleaning treatment, with an ultrasonic power of 300 W and a cleaning time of 30 minutes, and then vacuum drying in a vacuum drying oven to obtain a first ceramic material substrate;
[0059] Step (2): placing the first ceramic material matrix obtained in step (1) in a chemical deposition device, and then introducing hydrogen, diborane and methane at flow rate ratios of 90 sccm, 2 sccm and 3 sccm, respectively, and performing deposition for 10 hours at a deposition temperature of 830° C. and a deposition pressure of 1.5 kPa to obtain the second ceramic material matrix;
[0060] Step (3): placing the second ceramic material substrate obtained in step (2) in a magnetron sputtering coating device, using a graphite target as a sputtering source and argon gas with a flow rate of 60 sccm as a working gas, performing magnetron sputtering for 50 minutes at a sputtering power of 260 W and a sputtering temperature of 150° C., to obtain a third ceramic material substrate;
[0061] Step (4): Place the third ceramic material matrix obtained in step (3) in a metal vapor vacuum arc power ion implantation device, and dope metal Nd at an ion voltage of 130 keV. The doping amount of Nd ions is 5×10 15 ions / cm 2 After the rare earth element Nd is doped, it is transferred to a magnetic field sintering device, and subjected to magnetic field heat treatment for 1.5 hours under a nitrogen gas atmosphere, a temperature of 650°C and a flux coil current of 6A, and the device is naturally cooled to obtain the ceramic coating.
[0062] Example 3
[0063] This example provides a ceramic coating, with a hollow guide shaft as a ceramic material matrix, and the preparation method of the ceramic coating includes the following steps:
[0064] Step (1): subjecting the surface of the ceramic material substrate to ultrasonic cleaning treatment, with an ultrasonic power of 300 W and a cleaning time of 30 minutes, and then vacuum drying in a vacuum drying oven to obtain a first ceramic material substrate;
[0065] Step (2): placing the first ceramic material matrix obtained in step (1) in a chemical deposition device, and then introducing hydrogen, diborane and methane at flow rate ratios of 95 sccm, 2 sccm and 4 sccm, respectively, and performing deposition for 8 hours at a deposition temperature of 860° C. and a deposition pressure of 1 kPa to obtain the second ceramic material matrix;
[0066] Step (3): placing the second ceramic material substrate obtained in step (2) in a magnetron sputtering coating device, using a graphite target as a sputtering source and argon gas with a flow rate of 60 sccm as a working gas, performing magnetron sputtering for 30 minutes at a sputtering power of 350 W and a sputtering temperature of 200° C., to obtain a third ceramic material substrate;
[0067] Step (4): Place the third ceramic material matrix obtained in step (3) in a metal vapor vacuum arc power ion implantation device, and dope metal Nd at an ion voltage of 130 keV. The doping amount of Nd ions is 7×10 15 ions / cm 2 After the rare earth element Nd is doped, it is transferred to a magnetic field sintering device, and subjected to magnetic field heat treatment for 1.5 hours under a nitrogen gas atmosphere, a temperature of 650°C and a flux coil current of 6A, and the device is naturally cooled to obtain the ceramic coating.
[0068] Comparative Example 1
[0069] This example provides a ceramic coating and a preparation method thereof, which differs from Example 1 only in that the metal Nd in step (4) is adjusted to metal La; the remaining steps and parameters are the same.
[0070] The preparation method of the ceramic coating comprises the following steps:
[0071] Step (1): subjecting the surface of the ceramic material substrate to ultrasonic cleaning treatment, with an ultrasonic power of 300 W and a cleaning time of 30 minutes, and then vacuum drying in a vacuum drying oven to obtain a first ceramic material substrate;
[0072] Step (2): placing the first ceramic material matrix obtained in step (1) in a chemical deposition device, and then introducing hydrogen, diborane and methane at flow rate ratios of 93 sccm, 3 sccm and 5 sccm, respectively, and performing deposition for 9 hours at a deposition temperature of 845° C. and a deposition pressure of 1.5 kPa to obtain the second ceramic material matrix;
[0073] Step (3): placing the second ceramic material substrate obtained in step (2) in a magnetron sputtering coating device, using a graphite target as a sputtering source and argon gas with a flow rate of 60 sccm as a working gas, performing magnetron sputtering for 38 minutes at a sputtering power of 300 W and a sputtering temperature of 170° C., to obtain a third ceramic material substrate;
[0074] Step (4): Place the third ceramic material matrix obtained in step (3) in a metal vapor vacuum arc power ion implantation device, and dope metal La at an ion voltage of 130 keV. The La ion doping amount is 6×10 15 ions / cm 2 After the rare earth element Nd is doped, it is transferred to a magnetic field sintering device, and subjected to magnetic field heat treatment for 1.5 hours under a nitrogen gas atmosphere, a temperature of 650°C and a flux coil current of 6A, and the device is naturally cooled to obtain the ceramic coating.
[0075] Comparative Example 2
[0076] This example provides a ceramic coating and a preparation method thereof, which is different from Example 1 only in that no BDD layer is provided on the surface of the ceramic material substrate; the remaining steps and parameters are the same.
[0077] The preparation method of the ceramic coating comprises the following steps:
[0078] Step (1): subjecting the surface of the ceramic material substrate to ultrasonic cleaning treatment, with an ultrasonic power of 300 W and a cleaning time of 30 minutes, and then vacuum drying in a vacuum drying oven to obtain a first ceramic material substrate;
[0079] Step (2): placing the first ceramic material substrate obtained in step (1) in a magnetron sputtering coating device, using a graphite target as a sputtering source and argon gas with a flow rate of 60 sccm as a working gas, performing magnetron sputtering for 38 minutes at a sputtering power of 300 W and a sputtering temperature of 170° C., to obtain a second ceramic material substrate;
[0080] Step (3): The second ceramic material matrix obtained in step (2) is placed in a metal vapor vacuum arc power ion implantation device, and metal Nd is ion-doped at an ion voltage of 130 keV. The amount of Nd ion doped is 6×10 15 ions / cm 2 After the rare earth element Nd is doped, it is transferred to a magnetic field sintering device, and subjected to magnetic field heat treatment for 1.5 hours under a nitrogen gas atmosphere, a temperature of 650°C and a flux coil current of 6A, and the device is naturally cooled to obtain the ceramic coating.
[0081] Test Case
[0082] In this example, the hollow guide shaft bodies with ceramic coatings on the surfaces obtained in the above-mentioned embodiments and comparative examples were subjected to performance tests, and hollow guide shaft bodies without coatings were used as basic control groups.
[0083] Test method: 1) Use HXD-1000TM / LCD digital display microhardness tester to test the surface Vickers hardness; 2) According to the requirements of GB / T 2523-2008 standard, use Japan Mitutoyo SJ410 roughness tester to measure the surface roughness.
[0084] The test results are shown in Table 1.
[0085] Table 1
[0086]
[0087]
[0088] It can be seen from Table 1 that although Comparative Examples 1 to 2 can improve the performance of the hollow guide shaft to a certain extent, the improvement effect is far worse than that of Example 1 of the present application; at the same time, according to the requirements of ISO 27874:2008 (E) standard, the sample obtained in Example 1 of the present invention is bent into 90° and then bent back to the original position, reciprocating 3 times, and then the sample is visually tested with a 4x magnifying glass under a lighting lamp. There is no wrinkling, blistering, peeling, cracking or other undesirable phenomena on the surface of the coating / plating layer at the bending part, indicating that the coating has good bonding strength.
[0089] In summary, the present invention provides a ceramic coating and its preparation method and application. Through multiple steps of coating deposition and modification such as cleaning, chemical deposition of BDD layer, magnetron sputtering of DLC layer, incorporation of rare earth element Nd and magnetic field heat treatment, the combination of BDD layer and DLC layer forms a composite coating with high hardness, wear resistance and good chemical stability; the rare earth element Nd has a unique electronic structure and chemical properties, which can change the lattice structure and phase composition of the coating, thereby improving the hardness and wear resistance of the coating. Magnetic field heat treatment promotes the rearrangement and combination of atoms inside the coating through the action of the magnetic field to form a more dense and uniform microstructure, which further optimizes the comprehensive performance of the coating and gradually constructs a composite coating with high hardness and super wear resistance on the surface of the ceramic material substrate. When applied to ceramic material substrates such as hollow guide shafts, it can significantly extend its service life and has a wide range of practical application value.
[0090] Various embodiments of the present invention may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present invention; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0091] In the description of the specification of the present invention, the terms "including", "comprising", etc. mean "including but not limited to". In this article, relational terms such as "first" and "second", etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. Wherein A and B can be singular or plural. In this article, "at least one" means one or more, and "plurality" means two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single or plural items. For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b, c can be single or plural, respectively.
[0092] The foregoing is merely a specific embodiment of the present invention, which enables those skilled in the art to understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features claimed herein.
Claims
1. A method for preparing a ceramic coating, characterized in that: The preparation method comprises the following steps: Cleaning the surface of the ceramic material substrate to obtain a first ceramic material substrate; Providing a boron-doped diamond layer on the surface of the first ceramic material substrate by chemical deposition to obtain a second ceramic material substrate; Providing a diamond-like carbon layer on the surface of the second ceramic material substrate by magnetron sputtering to obtain a third ceramic material substrate; The rare earth element Nd is doped into the surface of the third ceramic material matrix, and then subjected to magnetic field heat treatment to obtain the ceramic coating.
2. The method for preparing a ceramic coating according to claim 1, characterized in that: The ceramic material matrix includes an alumina ceramic material matrix and a zirconia ceramic material matrix.
3. The method for preparing a ceramic coating according to claim 1, characterized in that: The cleaning method includes at least one of ultrasonic cleaning, sputtering cleaning and ion etching cleaning.
4. The method for preparing a ceramic coating according to claim 1, characterized in that: The step of providing a boron-doped diamond layer on the surface of the first ceramic material substrate by chemical deposition to obtain the second ceramic material substrate comprises the following process: The first ceramic material matrix is placed in a chemical deposition device, and then hydrogen, diborane and methane are introduced at a flow rate ratio of (90-95):(2-4):(2-5). Deposition is carried out for 8-10 hours at a deposition temperature of 830-860°C and a deposition pressure of 1-2 kPa to obtain the second ceramic material matrix.
5. The method for preparing a ceramic coating according to claim 1, characterized in that: The working condition parameters for setting the diamond-like carbon layer on the surface of the second ceramic material substrate by magnetron sputtering include: sputtering power of 260-350W, sputtering temperature of 150-200°C, and sputtering time of 30-50min.
6. The method for preparing a ceramic coating according to claim 1, characterized in that: The step of adding rare earth element Nd to the surface of the third ceramic material matrix and then performing magnetic field heat treatment to obtain the ceramic coating includes the following process: The third ceramic material matrix is placed in a metal vapor vacuum arc power ion implantation device, and metal Nd is ion-doped under the condition of an ion voltage of 120-150 keV; after the rare earth element Nd is doped, it is transferred to a magnetic field sintering device, and a magnetic field heat treatment is performed for 1-2 hours under the conditions of an inert gas atmosphere, a temperature of 600-700°C, and a flux coil current of 5-8A, and the ceramic coating is obtained by natural cooling of the device.
7. The method for preparing a ceramic coating according to claim 1, characterized in that: The amount of metal Nd ions doped is 5×10 15 ~7×10 15 ions / cm 2 .
8. A ceramic coating, characterized in that: The ceramic coating is prepared by the preparation method described in any one of claims 1 to 7.
9. Use of the ceramic coating according to claim 8 in the preparation of a hollow guide shaft.
10. A hollow guide shaft, characterized in that: The surface of the hollow guide shaft body at least partially includes the ceramic coating according to claim 8.
Citation Information
Cited By
CVD (Chemical Vapor Deposition) modified coating as well as preparation method and application thereof
CN119956155A
A cvd modified coating and method of making and use thereof
CN119956155B