Method for producing combustible gas and simultaneously preparing high-performance hydrogen evolution electrode through molten salt electrochemical oxidation of carbon fiber composite material

By employing a molten salt electrochemical oxidation method to carry out thermo-electrochemical coupling conversion under intermediate temperature conditions, the problems of high energy consumption and low product quality in the recycling of carbon fiber composite materials have been solved, enabling the preparation of high-performance hydrogen evolution electrodes and the value-added utilization of carbon fibers.

CN118996444AActive Publication Date: 2024-11-22CHANGJIANG RIVER SCI RES INST CHANGJIANG WATER RESOURCES COMMISSION

Patent Information

Application Number
CN202411121681.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-22
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

Existing carbon fiber composite material recycling technologies suffer from high energy consumption due to high-temperature pyrolysis, low product quality, and reduced mechanical properties of carbon fibers, making it difficult to achieve efficient resource utilization.

Method used

A high-performance hydrogen evolution electrode was prepared by constructing a molten salt electrochemical oxidation method. By utilizing the enhanced heat transfer and catalytic effect of molten salt, thermo-electrochemical coupling conversion was carried out under intermediate temperature conditions. This method controls the degree of oxidation on the carbon fiber surface and constructs a porous structure and defective active sites.

Benefits of technology

This study achieved efficient conversion of carbon fiber composite materials into combustible gas and high-performance hydrogen evolution electrodes under intermediate temperature conditions, reducing energy consumption, increasing combustible gas concentration, and enhancing the catalytic activity and mechanical properties of carbon fibers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996444A_ABST
    Figure CN118996444A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of carbon fiber recovery and value-added utilization, and relates to a method for producing combustible gas and simultaneously preparing a high-performance hydrogen evolution electrode through molten salt electrochemical oxidation of a carbon fiber composite material. The method comprises the following steps: constructing a two-electrode system consisting of a cathode and an anode by taking fused salt as an electrolyte, and carrying out electrolytic conversion on the anode to prepare combustible gas and a hydrogen evolution electrode; the working temperature of the fused salt is 400-600 DEG C; and the anode is a carbon fiber composite material. By utilizing the characteristics of heat transfer enhancement, catalytic conversion and electrochemical conversion of a molten salt medium, a carbon fiber composite material is efficiently converted into combustible gas on an anode side and the carbon fiber material is recycled by constructing a molten salt thermoelectric chemical coupling conversion system.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of carbon fiber recovery and value-added utilization, and in particular to a method for producing combustible gas and simultaneously preparing a high-performance hydrogen evolution electrode by electrochemically oxidizing a carbon fiber composite material with molten salt. Background Art

[0002] Carbon fiber composites are usually made of carbon fiber and resin. Due to their excellent mechanical properties and lightweight characteristics, they are widely used in aerospace, automobile, construction and other fields. However, with the increase in the use of carbon fiber composites, the treatment and resource utilization of their waste has become an urgent problem to be solved. At present, the latest technologies for recycling and resource utilization of carbon fiber composites mainly include high-temperature pyrolysis, supercritical fluid method, chemical recycling method and physical recycling method.

[0003] Traditional chemical or physical recycling methods often have problems of low recycling efficiency and high cost. Chemical reagents or physical crushing can damage the fibers, making it difficult to maintain their original strength and modulus. The use of organic chemical reagents is potentially toxic and poses safety risks. The technology of high-temperature pyrolysis of carbon fiber composites to recover carbon fibers is of great significance in the field of carbon fiber recycling because it is currently the only recycling method that has been commercialized. However, this technology also faces some problems and challenges: high temperature conditions are required and energy consumption is high; the high-temperature pyrolysis process requires precise control of temperature, atmosphere and other conditions to ensure the pyrolysis effect and product quality, but the control of thermochemical operating conditions is difficult, especially in the case of large-scale production; in the pyrolysis process, in addition to obtaining carbon fibers, the resin pyrolysis conversion will produce some gas-liquid-solid three-phase products, such as combustible gas and solid carbon, but the product quality is low and difficult to use, and solid carbon is often easy to adhere to the surface of carbon fibers, affecting the subsequent use of carbon fibers; in the high-temperature pyrolysis process, carbon fibers may be affected by high temperature (>800°C) and surface oxidation, resulting in a large reduction in their mechanical properties. Therefore, how to make carbon fibers more valuable is a difficult problem. Summary of the invention

[0004] In view of the shortcomings of the existing high-temperature pyrolysis and recovery technology of carbon fiber composite materials, the present invention provides a method for producing combustible gas by electrochemically oxidizing carbon fiber composite materials with molten salt and preparing a high-performance hydrogen evolution electrode at the same time. With the help of the enhanced heat transfer and electrolyte properties of molten salt, the carbon fiber composite material undergoes a thermo-electrochemical coupled conversion reaction on the anode side of a molten salt electrolytic cell. The strong heat transfer properties and catalytic reaction ability of the molten salt can reduce the conversion temperature of the carbon fiber composite material to a medium temperature range, while catalytically improving the quality of the resin thermally converted into combustible gas. The electrochemical oxidation process can accurately control the degree of oxidation on the carbon fiber surface. By constructing a porous structure and defective active sites, the catalytic activity of the recycled carbon fiber as a hydrogen evolution electrode is enhanced.

[0005] To achieve the above object, the present invention provides the following solutions:

[0006] One of the technical solutions of the present invention is to provide a method for producing combustible gas and preparing a high-performance hydrogen evolution electrode by electrochemically oxidizing carbon fiber composite materials with molten salt, the steps comprising:

[0007] A two-electrode system consisting of a cathode and an anode is constructed using molten salt as an electrolyte, and the anode is converted by electrolysis to prepare a combustible gas and a hydrogen evolution electrode;

[0008] The working temperature of the molten salt is 400-600°C;

[0009] The anode is made of carbon fiber composite material.

[0010] Furthermore, the molten salt is at least one of carbonate, chloride, sulfate, fluoride and hydroxide.

[0011] Preferably, the carbonate is at least one of Li2CO3, Na2CO3, K2CO3 and CaCO3.

[0012] Preferably, the chloride salt is at least one of LiCl, NaCl, KCl and CaCl2.

[0013] Preferably, the sulfate is at least one of Li2SO4, Na2SO4, K2SO4 and CaSO4.

[0014] Preferably, the fluoride is at least one of LiF, NaF, KF and CaF2.

[0015] Preferably, the hydroxide is at least one of LiOH, NaOH, KOH and Ca(OH)2.

[0016] The molten salts are carbonates, chlorides, sulfates, fluorides and hydroxides having a melting point or eutectic point of about 400-600° C. and chemically stable and non-decomposable properties.

[0017] Furthermore, the cathode is one of Au, Ag, Pt, Ni, Cu, Mo, NiFe alloy, NiFeCu alloy and graphite.

[0018] Furthermore, the electrolysis step is: heating the molten salt electrolyte to 400-600° C., then immersing the anode and cathode in the molten salt electrolyte, and performing electrolysis in a constant current or constant voltage manner for 0.5-3 h.

[0019] Preferably, the constant voltage is 1.5-5V; the constant current is 50mA-2A.

[0020] Furthermore, the combustible gas includes at least one of H2, CO and CH4.

[0021] Furthermore, the method further comprises the step of washing the anode with water after electrolysis.

[0022] Furthermore, the carbon fiber composite material is a sheet structure with a thickness of less than 0.5 cm.

[0023] After the electrolysis is completed, the carbon fiber material is recovered from the liquid molten salt, and then the residual molten salt on the surface is removed by water washing to obtain a carbon fiber-based electrode for electrochemical hydrogen evolution.

[0024] Using molten salt electrochemical means, carbon fiber composites are subjected to molten salt thermal / electrochemical coupled conversion to produce high-value combustible gas and recycled carbon fiber. The recycled carbon fiber can be used as a hydrogen evolution electrode.

[0025] Molten salt is a good heat medium, and its thermal conductivity is 10 times that of nitrogen. Molten salt also has the ability to catalyze pyrolysis and convert organic matter to produce high-value combustible gas. Therefore, the conversion of carbon fiber composites in a molten salt environment can be carried out under medium temperature conditions (400-600°C), which can avoid high energy consumption and damage to the quality of carbon fiber at high temperatures, while catalyzing the conversion of resin matrix into high-value combustible gas. The unique liquid phase reaction environment of molten salt can promote the separation of resin solid phase products and carbon fibers through surface tension and interface interactions.

[0026] Molten salt in a molten state is also an ionic liquid that can be used as an electrolyte. Carbon fiber itself has the ability to conduct electricity, so carbon fiber composites can be used as the anode of a molten salt electrolytic cell, using both thermochemical and electrochemical conversion processes simultaneously. The electrochemical process can precisely control the kinetics of the chemical reaction by adjusting the electrode potential. Compared with simple thermal reaction conditions, the electrochemical parameters can be more precisely controlled.

[0027] Considering that carbon fiber itself has good electrical conductivity, it is possible to consider using recycled carbon fiber in the field of electrochemical hydrogen evolution as a hydrogen evolution electrode to achieve value-added utilization of carbon fiber. The molten salt thermoelectrochemical coupling can accurately control the degree of oxidation on the carbon fiber surface, thereby constructing a porous structure and defective active hydrogen evolution sites on the carbon fiber surface, and enhancing the catalytic ability of the carbon fiber-based hydrogen evolution electrode.

[0028] The second technical solution of the present invention is to provide a hydrogen evolution electrode prepared by the above method.

[0029] The third technical solution of the present invention is to provide a method for recycling carbon fiber composite materials, the steps comprising:

[0030] A two-electrode system consisting of a cathode and an anode is constructed using a carbon fiber composite material as an anode and a molten salt as an electrolyte. The carbon fiber composite material is converted into a combustible gas and a hydrogen evolution electrode through electrolysis;

[0031] The working temperature of the molten salt is 400-600°C.

[0032] Furthermore, the molten salt is at least one of carbonate, chloride, sulfate, fluoride and hydroxide.

[0033] Preferably, the carbonate is at least one of Li2CO3, Na2CO3, K2CO3 and CaCO3.

[0034] Preferably, the chloride salt is at least one of LiCl, NaCl, KCl and CaCl2.

[0035] Preferably, the sulfate is at least one of Li2SO4, Na2SO4, K2SO4 and CaSO4.

[0036] Preferably, the fluoride is at least one of LiF, NaF, KF and CaF2.

[0037] Preferably, the hydroxide is at least one of LiOH, NaOH, KOH and Ca(OH)2.

[0038] Furthermore, the cathode is one of Au, Ag, Pt, Ni, Cu, Mo, NiFe alloy, NiFeCu alloy and graphite.

[0039] Furthermore, the electrolysis step is: heating the molten salt electrolyte to 400-600° C., then immersing the anode and cathode in the molten salt electrolyte, and performing electrolysis in a constant current or constant voltage manner for 0.5-3 h.

[0040] Preferably, the constant voltage is 1.5-5V; the constant current is 50mA-2A.

[0041] Furthermore, the combustible gas includes at least one of H2, CO and CH4.

[0042] Furthermore, the method further comprises the step of washing the anode with water after electrolysis.

[0043] The present invention discloses the following technical effects:

[0044] The present invention utilizes the characteristics of molten salt medium that simultaneously enhances heat transfer, catalytic conversion and electrochemical conversion, and constructs a molten salt thermo-electrochemical coupling conversion system to achieve efficient conversion of carbon fiber composite materials into combustible gas and recycling of carbon fiber materials on the anode side. The heat transfer characteristics of molten salt are used to reduce the thermal conversion temperature, thereby reducing energy consumption; the catalytic effect of molten salt is used to increase the concentration of combustible gas; by precisely controlling the electrochemical operating conditions, the degree of oxidation on the carbon fiber surface is finely controlled, and a pore structure and defective active sites suitable for hydrogen evolution reaction are constructed on the carbon fiber surface, thereby improving the carbon fiber hydrogen evolution reaction ability, thereby realizing the value-added utilization of recycled carbon fiber. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0046] Figure 1 This is a scanning electron microscope image of the hydrogen evolution electrode prepared in Example 1;

[0047] Figure 2 This is a scanning electron microscope image of the carbon fiber-based electrode for electrochemical hydrogen evolution prepared in Comparative Example 1;

[0048] Figure 3 is the concentration change of combustible gas in Example 1 and Comparative Example 1;

[0049] Figure 4 The linear voltammetric scanning diagram of the hydrogen evolution electrode prepared in Example 1 and the carbon fiber-based electrode for electrochemical hydrogen evolution prepared in Comparative Example 1 used as electrochemical hydrogen evolution electrodes in 1M KOH solution;

[0050] Figure 5 XRD diagrams of the carbon fiber-based electrodes in Example 1 and Comparative Example 2;

[0051] Figure 6 is the concentration change of combustible gas in Example 2. DETAILED DESCRIPTION

[0052] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0053] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0054] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0055] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0056] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0057] Example 1

[0058] The method steps of producing combustible gas by electrochemically oxidizing carbon fiber composite materials with molten salt and preparing high-performance hydrogen evolution electrodes are as follows:

[0059] S1. Preparation of electrolyte: 500 g of a mixed salt of three carbonates, Li2CO3, Na2CO3 and K2CO3, with a molar ratio of 43.5:31.5:25, the melting point of the three carbonate mixture is 393°C, and placed in an alumina crucible, the electrolyte working temperature range is about 500°C, to form a molten electrolyte;

[0060] S2, cutting the carbon fiber composite material into a sheet structure with a thickness of 2 mm, connecting it to the electrode collector through a conductive metal clip to serve as an anode;

[0061] S3, using a metal Ni sheet as a cathode material, connected to an electrode current collector via a conductive metal clip, as a cathode;

[0062] S4. Immerse the anode and cathode in a molten electrolyte at about 500°C, perform electrolysis at a constant cell voltage of 2.0V, and perform electrolysis for 2 hours. Use an online gas analyzer to analyze the concentration changes of the coupled conversion gas-phase products (H2, CO, and CH4). Figure 3 After the electrolysis is completed, the anode is recovered from the molten electrolyte, and the electrolyte remaining on the surface is removed by washing with water to obtain a carbon fiber-based electrode for electrochemical hydrogen evolution, which is referred to as a hydrogen evolution electrode.

[0063] Figure 1 This is a scanning electron microscope image of the hydrogen evolution electrode prepared in Example 1. Figure 1 It can be seen that there is no resin conversion product residue on the fiber surface, and many micropores are evenly distributed on the fiber surface.

[0064] Example 2

[0065] The method steps of producing combustible gas by electrochemically oxidizing carbon fiber composite materials with molten salt and preparing high-performance hydrogen evolution electrodes are as follows:

[0066] S1. Preparation of electrolyte: 500 g of a mixed salt of three chlorides of LiCl, NaCl and KCl with a molar ratio of 47.5:15:37.5, wherein the melting point of the three carbonate mixture is 399° C., is selected and placed in an alumina crucible, wherein the electrolyte working temperature range is about 600° C., to form a molten electrolyte;

[0067] S2, cutting the carbon fiber composite material into a sheet structure with a thickness of 2 mm, connecting it to the electrode collector through a conductive metal clip to serve as an anode;

[0068] S3, using a metal Ni sheet as a cathode material, connected to an electrode current collector via a conductive metal clip, as a cathode;

[0069] S4. Immerse the anode and cathode in a molten electrolyte at about 600°C, perform electrolysis at a constant current of 200 mA for 2 hours, and use an online gas analyzer to analyze the concentration changes of the coupled conversion gas-phase products (H2, CO and CH4) (e.g. Figure 6 After the electrolysis is completed, the anode is recovered from the molten electrolyte, and the electrolyte remaining on the surface is removed by washing with water to obtain a carbon fiber-based electrode for electrochemical hydrogen evolution, which is referred to as a hydrogen evolution electrode.

[0070] Example 3

[0071] The method steps of producing combustible gas by electrochemically oxidizing carbon fiber composite materials with molten salt and preparing high-performance hydrogen evolution electrodes are as follows:

[0072] S1. Preparation of electrolyte: 500 g of a mixed salt of two sulfates, Li2SO4 and K2SO4, with a molar ratio of 80.9:19.1, is selected. The melting point of the mixture is 546°C, and the mixture is placed in an alumina crucible. The electrolyte working temperature range is about 600°C to form a molten electrolyte;

[0073] S2, cutting the carbon fiber composite material into a sheet structure with a thickness of 2 mm, connecting it to the electrode collector through a conductive metal clip to serve as an anode;

[0074] S3, using a metal Ni sheet as a cathode material, connected to an electrode current collector via a conductive metal clip, as a cathode;

[0075] S4. Immerse the anode and cathode in a molten electrolyte at about 600°C, and perform electrolysis at a constant current of 200 mA for 2 hours. Use an online gas analyzer to analyze the concentration changes of the coupled conversion gas-phase products, combustible gases (H2, CO and CH4). After the electrolysis, recover the anode from the molten electrolyte, and remove the residual electrolyte on the surface by washing with water to obtain a carbon fiber-based electrode for electrochemical hydrogen evolution, which is referred to as a hydrogen evolution electrode.

[0076] Comparative Example 1

[0077] 500 g of a mixed salt of three carbonates, Li2CO3, Na2CO3 and K2CO3, with a molar ratio of 43.5:31.5:25, was selected. The melting point of the three carbonate mixture was 393°C, and the mixture was placed in an alumina crucible and heated to about 500°C to form a molten salt. The carbon fiber composite material same as that in Example 1 was placed in the molten salt medium and pyrolyzed for 2 h. The concentration changes of combustible gases (H2, CO and CH4) of the pyrolysis conversion gas phase products were analyzed by an online gas analyzer (such as Figure 3 After the pyrolysis is completed, the carbon fiber material is recovered from the liquid molten salt, and then the residual molten salt on the surface is removed by water washing to obtain a carbon fiber-based electrode for electrochemical hydrogen evolution.

[0078] Comparative Example 2

[0079] The method steps of producing combustible gas by electrochemically oxidizing carbon fiber composite materials with molten salt and preparing high-performance hydrogen evolution electrodes are as follows:

[0080] S1. Preparation of electrolyte: 500 g of a mixed salt of three carbonates, Li2CO3, Na2CO3 and K2CO3, with a molar ratio of 43.5:31.5:25, the melting point of the three carbonate mixture is 393°C, and placed in an alumina crucible, the electrolyte working temperature range is about 500°C, to form a molten electrolyte;

[0081] S2, cutting the carbon fiber composite material into a sheet structure with a thickness of 2 mm, connecting it to the electrode collector through a conductive metal clip to serve as an anode;

[0082] S3, using a metal Ni sheet as a cathode material, connected to an electrode current collector via a conductive metal clip, as a cathode;

[0083] S4. Immerse the anode and cathode in a molten electrolyte at about 500°C, and perform electrolysis at a constant cell voltage of 4.0V for 2 hours. Use an online gas analyzer to analyze the concentration changes of the coupled conversion gas-phase products, combustible gases (H2, CO and CH4). After the electrolysis, recover the anode from the molten electrolyte, and remove the residual electrolyte on the surface by washing with water to obtain a carbon fiber-based electrode for electrochemical hydrogen evolution, which is referred to as a hydrogen evolution electrode.

[0084] Figure 5 The XRD diagrams of the carbon fiber-based electrodes in Example 1 and Comparative Example 2 are shown in FIG. As can be seen from the figure, about 25° corresponds to the diffraction peak of carbon. Compared with Example 1, the electrolytic cell pressure of Comparative Example 2 is greater, and the degree of oxidation of the carbon fiber surface is greater, which is manifested in that the peak intensity of the XRD diffraction peak of the carbon fiber in Comparative Example 2 is reduced and the half-peak width is increased.

[0085] Figure 2 The scanning electron microscope image of the carbon fiber-based electrode for electrochemical hydrogen evolution prepared in Comparative Example 1 is shown in FIG. Figure 2 It can be seen that there are many solid products produced by resin pyrolysis attached to the fiber surface.

[0086] Figure 3 is the concentration change of the combustible gas in Example 1 and Comparative Example 1, Figure 3 It can be seen that when electrochemistry participates in the reaction, the output of combustible gas is higher than that of pure thermochemical reaction.

[0087] Figure 4 The linear voltammetric scan diagram of the hydrogen evolution electrode prepared in Example 1 and the carbon fiber-based electrode for electrochemical hydrogen evolution prepared in Comparative Example 1 used as electrochemical hydrogen evolution electrodes in 1M KOH solution is shown in FIG. Figure 4 It can be seen that the carbon fiber obtained in Example 1 has a larger hydrogen production polarization current density and exhibits stronger electrochemical hydrogen evolution performance.

[0088] Figure 6 2 is the concentration change of the combustible gas in Example 2. It can be seen that when constant current electrolysis is adopted, the combustible gas generation rate is relatively stable.

[0089] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for producing combustible gas and preparing a high-performance hydrogen evolution electrode by electrochemically oxidizing carbon fiber composite materials with molten salt, characterized in that the steps include: A two-electrode system consisting of a cathode and an anode is constructed using molten salt as an electrolyte, and the anode is converted by electrolysis to prepare a combustible gas and a hydrogen evolution electrode; The working temperature of the molten salt is 400-600°C; The anode is made of carbon fiber composite material.

2. The method according to claim 1, characterized in that: The molten salt is at least one of carbonate, chloride, sulfate, fluoride and hydroxide.

3. The method according to claim 2, characterized in that The carbonate is at least one of Li2CO3, Na2CO3, K2CO3 and CaCO3; the chloride salt is at least one of LiCl, NaCl, KCl and CaCl2; the sulfate is at least one of Li2SO4, Na2SO4, K2SO4 and CaSO4; the fluoride is at least one of LiF, NaF, KF and CaF2; the hydroxide is at least one of LiOH, NaOH, KOH and Ca(OH)2.

4. The method according to claim 1, characterized in that: The cathode is one of Au, Ag, Pt, Ni, Cu, Mo, NiFe alloy, NiFeCu alloy and graphite.

5. The method according to claim 1, characterized in that The electrolysis step is: heating the molten salt electrolyte to 400-600° C., then immersing the anode and cathode in the molten salt electrolyte, and performing electrolysis in a constant current or constant voltage manner for 0.5-3 hours.

6. The method according to claim 5, characterized in that The constant voltage is 1.5 to 5V; the constant current is 50mA to 2A.

7. The method according to claim 1, characterized in that The combustible gas includes at least one of H2, CO and CH4.

8. The method according to claim 1, characterized in that The method further comprises the step of washing the anode with water after electrolysis.

9. A hydrogen evolution electrode prepared by the method according to any one of claims 1 to 8.

10. A method for recycling carbon fiber composite materials, characterized in that the steps include: A two-electrode system consisting of a cathode and an anode is constructed using a carbon fiber composite material as an anode and a molten salt as an electrolyte. The carbon fiber composite material is converted into a combustible gas and a hydrogen evolution electrode through electrolysis; The working temperature of the molten salt is 400-600°C.

Citation Information

Patent Citations

  • Recovery method of carbon fibers

    CN104499039A

  • Method for preparing synthesis gas based on electrolysis CO2 and H2O of molten carbonate electrolytic tank

    CN104630812A

  • Preparation method of coal tar pitch resin-based amorphous carbon-coated few-layer molybdenum disulfide nanometer box for negative electrode of sodium-ion battery and application of nanometer box

    CN106876702A

  • Molten salt electrochemical process for preparing hydrogen and carbon monoxide by oxidizing methane at medium and low temperatures

    CN110257848A

  • Ruthenium quantum dot loaded carbon fiber hydrogen evolution catalyst, preparation method and application thereof

    CN113278990A

Cited By

  • Fused salt pyrolysis recovery system and method for phenolic resin composite material

    CN119839013A

  • A molten salt pyrolysis recovery system and method for phenolic resin composite materials

    CN119839013B