Ag / CoFe2O4 alkaline electrolyzed water catalyst and preparation method thereof

Through the preparation of Ag/CoFe2O4 catalyst, the problems of high cost and low catalytic activity of electrolytic water catalysts are solved, and efficient OER/HER dual-function catalytic activity and stability are achieved, production costs are reduced, and electrocatalytic performance is significantly improved.

CN118996475APending Publication Date: 2024-11-22JINGDEZHEN CERAMIC UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410975999.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing electrolytic water catalysts are expensive and have low catalytic activity, which limits the industrialization of electrolytic hydrogen production.

Method used

Using Ag/CoFe2O4 alkaline electrolytic catalyst, by mixing silver salt with CoFe2O4 catalyst and processing under specific temperature and atmosphere, a catalyst with high active sites and conductivity is formed, and the porosity and ratio of the catalyst are increased by urea. Surface area.

Benefits of technology

It realizes efficient OER/HER dual-function catalytic activity and stability in 1M KOH, reduces the production cost of the catalyst, improves the electrocatalytic performance, and significantly improves the overpotential.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996475A_ABST
    Figure CN118996475A_ABST
Patent Text Reader

Abstract

The invention discloses an Ag / CoFe2O4 alkaline electrolyzed water catalyst and a preparation method thereof, and belongs to the technical field of catalysts. The preparation method comprises the following steps: dissolving cobalt salt, ferric salt and citric acid in a solvent, stirring for reaction, and then drying and calcining; the CoFe2O4 is obtained; the preparation method comprises the following steps: dissolving silver salt and urea in a solvent, stirring and reacting to obtain an impregnation liquid, mixing the impregnation liquid with CoFe2O4, stirring and reacting, and then drying and calcining to obtain the CoFe2O4 / silver composite material. The catalyst material can be used as a catalyst for OER and HER reactions at the same time, and the problem that an existing non-noble metal catalyst is low in catalytic activity is effectively solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysts, and in particular relates to an Ag / CoFe2O4 alkaline water electrolysis catalyst and a preparation method thereof. Background Art

[0002] With the rapid development of social science and economy, fossil fuels can no longer meet the needs of modern people. Although fossil fuels are widely used, their reserves are limited, and excessive use will cause great damage to the environment. Therefore, people are developing more sustainable, pollution-free and efficient new energy materials. Hydrogen energy has attracted much attention as a green, environmentally friendly and renewable energy source. At present, water electrolysis to produce hydrogen is an efficient, clean and pollution-free method for hydrogen production, which includes two parts: hydrogen evolution reaction and oxygen evolution reaction. Among them, the oxygen evolution reaction is often less efficient due to its high activation energy and slow reaction rate. Due to the lack of highly active oxygen evolution reaction catalysts, the reaction energy barrier is high and the energy consumption is increased, which limits the development of industrial water electrolysis to produce hydrogen. Although precious metal catalysts perform well in OER and HER, they are expensive and scarce, which increases the cost of hydrogen production. Therefore, there is an urgent need to develop stable, cheap and efficient OER and HER bifunctional electrocatalysts. Summary of the invention

[0003] In view of the above-mentioned prior art, the present invention provides an Ag / CoFe2O4 alkaline water electrolysis catalyst and a preparation method thereof, so as to solve the technical problems of the existing water electrolysis catalyst being expensive and having low catalytic activity.

[0004] In order to achieve the above object, the technical solution adopted by the present invention is: to provide a method for preparing an Ag / CoFe2O4 alkaline water electrolysis catalyst, comprising the following steps:

[0005] S1: Dissolve cobalt salt, iron salt and citric acid in a solvent, heat and dry at 180-250°C for 10-15h to obtain a CoFe2O4 precursor;

[0006] S2: calcining the CoFe2O4 precursor to obtain a CoFe2O4 catalyst;

[0007] S3: dissolving silver salt and urea in a mixed solvent of anhydrous ethanol and deionized water to obtain an impregnation solution, mixing the CoFe2O4 catalyst with the impregnation solution, stirring the mixture for reaction, and then heating and drying at 90 to 120° C. for 10 to 15 hours to obtain an Ag / CoFe2O4 precursor;

[0008] S4: Heat the Ag / CoFe2O4 precursor to 380-420°C at a heating rate of 2°C / min, and keep it warm for 0.5-2h; then heat it to 480-520°C at a heating rate of 1°C / min, and keep it warm for 0.5-2h; then heat it to 780-820°C at a heating rate of 3°C / min, and keep it warm for 4h; then naturally cool it to room temperature.

[0009] Based on the above technical solution, the present invention can also be improved as follows.

[0010] Furthermore, the molar ratio of the cobalt salt, the iron salt and the citric acid is 1:2:4.5.

[0011] Furthermore, the cobalt salt is Co(NO3)2·6H2O, the iron salt is Fe(NO3)3·9H2O; and the solvent is deionized water.

[0012] Furthermore, the heating and drying temperature in S1 is 200° C., and the heating and drying time is 12 h.

[0013] Furthermore, the calcination process in S2 is as follows: in an air atmosphere, the CoFe2O4 precursor is heated to 380-420°C at a heating rate of 5-7°C / min, kept warm for 3.5-5h, and then air-cooled to room temperature; then heated to 380-420°C at a heating rate of 2°C / min, and kept warm for 0.5-2h; then heated to 480-520°C at a heating rate of 1°C / min, and kept warm for 0.5-2h; then heated to 780-820°C at a heating rate of 3°C / min, and kept warm for 4h; then naturally cooled to room temperature.

[0014] Furthermore, the mixed solvent is prepared by mixing anhydrous ethanol and deionized water in a volume ratio of 7:3.

[0015] Furthermore, the concentration of silver salt and urea in the impregnation solution is 0.1 mol / L; the CoFe2O4 catalyst and the impregnation solution are mixed at a mass ratio of Ag:CoFe2O4=5:95.

[0016] Furthermore, the silver salt is AgNO3.

[0017] Furthermore, the stirring reaction time in S3 is 1 hour; the heating and drying temperature is 100° C., and the heating and drying time is 12 hours.

[0018] The invention also discloses an Ag / CoFe2O4 alkaline water electrolysis catalyst prepared by the preparation method.

[0019] The beneficial effects of the present invention are:

[0020] 1. The catalyst of the present invention uses CoFe2O4 as a precursor, and adjusts its electronic structure by introducing metal Ag to increase the metal active sites, thereby improving the conductivity of the catalyst and further improving the electrochemical activity.

[0021] 2. In the present invention, urea is added as a precipitant. Under dry conditions, as the temperature rises, urea is hydrolyzed into ammonia and CO2, which can induce the formation of porosity to increase the surface area of ​​the catalyst, thereby increasing the exposure of active sites and improving the catalytic effect. In addition, urea can regulate the size of catalyst particles, increase the specific surface area of ​​the catalyst, and thus improve the catalytic activity.

[0022] 3. The catalyst of the present invention is made of non-precious metal materials, and the raw material source is abundant and low in cost, which can reduce the production cost of the catalyst; in addition, the preparation method of the catalyst is simple to operate and easy to mass produce. The catalyst prepared by the present invention has good OER / HER bifunctional catalytic activity and stability in alkaline electrolyte. The oxygen evolution reaction is measured in 1M KOH at a current density of 50mA cm -2 When the overpotential is 440 mV, the current density in the hydrogen evolution reaction is 250 mA cm -2 The corresponding overpotential is 434 mV, which has efficient electrocatalytic performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 are XRD patterns of CoFe2O4 (Comparative Example 1), Ag / CoFe2O4-D2 (Comparative Example 2), and Ag / CoFe2O4-S1 (Example 1);

[0024] Figure 2 is a SEM image of Ag / CoFe2O4-S1 (Example 1) of the present invention;

[0025] Figure 3 It is a linear sweep voltammetry (LSV) graph of oxygen evolution reaction of CoFe2O4 (Comparative Example 1), Ag / CoFe2O4-D2 (Comparative Example 2) and Ag / CoFe2O4-S1 (Example 1) in 1M KOH electrolyte;

[0026] Figure 4 are electrochemical impedance spectroscopy (EIS) graphs of CoFe2O4 (Comparative Example 1), Ag / CoFe2O4-D2 (Comparative Example 2) and Ag / CoFe2O4-S1 (Example 1) in 1M KOH electrolyte;

[0027] Figure 5It is a linear sweep voltammetry (LSV) diagram of the hydrogen evolution reaction of CoFe2O4 (Comparative Example 1), Ag / CoFe2O4-D2 (Comparative Example 2) and Ag / CoFe2O4-S1 (Example 1) in 1M KOH electrolyte;

[0028] Figure 6 are electrochemical impedance spectroscopy (EIS) graphs of CoFe2O4 (Comparative Example 1), Ag / CoFe2O4-D2 (Comparative Example 2) and Ag / CoFe2O4-S1 (Example 1) in 1M KOH electrolyte;

[0029] Figure 7 It is a linear sweep voltammetry (LSV) diagram of the complete hydrolysis of CoFe2O4 (Comparative Example 1), Ag / CoFe2O4-D2 (Comparative Example 2) and Ag / CoFe2O4-S1 (Example 1) in 1M KOH electrolyte;

[0030] Figure 8 It is a test graph of the total hydrolysis stability (IT) of CoFe2O4 (Comparative Example 1), Ag / CoFe2O4-D2 (Comparative Example 2) and Ag / CoFe2O4-S1 (Example 1) in 1M KOH. DETAILED DESCRIPTION

[0031] The specific implementation modes of the present invention are described in detail below with reference to the embodiments.

[0032] Example 1

[0033] An Ag / CoFe2O4 alkaline water electrolysis catalyst is prepared by the following steps:

[0034] (1) Dissolve 0.05 mol of Co(NO3)2·6H2O, 0.1 mol of Fe(NO3)3·9H2O and 0.225 mol of C6H8O7·H2O in 200 ml of deionized water and stir to form a uniform solution; heat and dry the solution at 200°C for 12 h to obtain a CoFe2O4 precursor;

[0035] (2) The CoFe2O4 precursor was heated at 6℃min in air atmosphere. -1 The temperature was raised to 400°C at a rate of 100°C, kept at that temperature for 4 hours, and then cooled to room temperature; then the temperature was raised to 400°C at a rate of 2°C min -1 The temperature was raised to 400℃ and kept at this temperature for 1h; then the temperature was raised to 400℃ and kept at this temperature for 1h. -1 The temperature was raised to 500℃ and kept at this temperature for 1h; then the temperature was raised at 3℃min -1 The temperature was raised to 800°C at a heating rate of 100°C, kept at that temperature for 4 hours, and then naturally cooled to room temperature to obtain a CoFe2O4 catalyst;

[0036] (3) 70 ml of anhydrous ethanol and 30 ml of deionized water were mixed to obtain a mixed solvent; 1.70 g of AgNO3 and 0.60 g of urea were weighed and dissolved in the mixed solvent and stirred to form an impregnation solution; 23.18 ml of the impregnation solution was mixed with 4.75 g of CoFe2O4 catalyst, stirred at room temperature for 1 h, and then heated and dried at 100°C for 12 h to obtain an Ag / CoFe2O4 precursor;

[0037] (4) The Ag / CoFe2O4 precursor was heated at 2°C min in air atmosphere. -1 The temperature was raised to 400℃ and kept at this temperature for 1h; then the temperature was raised to 400℃ and kept at this temperature for 1h. -1 The temperature was raised to 500℃ and kept at this temperature for 1h; then the .... -1 The temperature was raised to 800°C at a rate of 100 °C and kept for 4 h; then the temperature was naturally cooled to room temperature to obtain Ag / CoFe2O4 alkaline water electrolysis catalyst, which was named Ag / CoFe2O4-S1.

[0038] Example 2

[0039] An Ag / CoFe2O4 alkaline water electrolysis catalyst is prepared by the following steps:

[0040] (1) Dissolve 0.05 mol of Co(NO3)2·6H2O, 0.1 mol of Fe(NO3)3·9H2O and 0.225 mol of C6H8O7·H2O in 200 ml of deionized water and stir to form a uniform solution; heat and dry the solution at 180°C for 15 h to obtain a CoFe2O4 precursor;

[0041] (2) The CoFe2O4 precursor was heated at 5°C min in air atmosphere. -1 The temperature was raised to 380°C at a rate of 100 °C, kept at this temperature for 5 h, and then cooled to room temperature; then -1 The temperature was raised to 420℃ and kept at this temperature for 0.5h; then the .... -1 The temperature was raised to 480℃ and kept at this temperature for 2h; then the .... -1 The temperature was raised to 820°C at a rate of 10000 ℃, kept at that temperature for 4 hours, and then naturally cooled to room temperature to obtain a CoFe2O4 catalyst;

[0042] (3) 70 ml of anhydrous ethanol and 30 ml of deionized water were mixed to obtain a mixed solvent; 1.70 g of AgNO3 and 0.60 g of urea were weighed and dissolved in the mixed solvent and stirred to form an impregnation solution; 23.2 ml of the impregnation solution was mixed with 4.75 g of CoFe2O4 catalyst, stirred at room temperature for 1 h, and then heated and dried at 90°C for 15 h to obtain an Ag / CoFe2O4 precursor;

[0043] (4) The Ag / CoFe2O4 precursor was heated at 2°C min in air atmosphere. -1 The temperature was raised to 380℃ and kept at this temperature for 2h; then the .... -1 The temperature was raised to 520℃ and kept at this temperature for 0.5h; then the temperature was raised to 3℃min -1 The temperature was raised to 820°C and kept for 4 hours; then the temperature was naturally cooled to room temperature to obtain Ag / CoFe2O4-U alkaline water electrolysis catalyst, which was named Ag / CoFe2O4-S2.

[0044] Example 3

[0045] An Ag / CoFe2O4 alkaline water electrolysis catalyst is prepared by the following steps:

[0046] (1) Dissolve 0.05 mol of Co(NO3)2·6H2O, 0.1 mol of Fe(NO3)3·9H2O and 0.225 mol of C6H8O7·H2O in 200 ml of deionized water and stir to form a uniform solution; heat and dry the solution at 250°C for 10 h to obtain a CoFe2O4 precursor;

[0047] (2) The CoFe2O4 precursor was heated at 7°C min in air atmosphere. -1 The temperature was raised to 420℃ at a rate of 100℃, kept at this temperature for 3.5h and then cooled to room temperature; then -1 The temperature was raised to 380℃ and kept at this temperature for 2h; then the .... -1 The temperature was raised to 520℃ and kept at this temperature for 0.5h; then the temperature was raised at 3℃min -1 The temperature was raised to 780°C at a heating rate of 10000 ℃, kept at that temperature for 4 hours, and then naturally cooled to room temperature to obtain a CoFe2O4 catalyst;

[0048] (3) 70 ml of anhydrous ethanol and 30 ml of deionized water were mixed to obtain a mixed solvent; 1.70 g of AgNO3 and 0.60 g of urea were weighed and dissolved in the mixed solvent and stirred to form an impregnation solution; 23.2 ml of the impregnation solution was mixed with 4.75 g of CoFe2O4 catalyst, stirred at room temperature for 1 h, and then heated and dried at 120° C. for 10 h to obtain an Ag / CoFe2O4 precursor;

[0049] (4) The Ag / CoFe2O4 precursor was heated at 2°C min in air atmosphere. -1 The temperature was raised to 420℃ and kept at this temperature for 0.5h; then the .... -1 The temperature was raised to 480℃ and kept at this temperature for 2h; then the .... -1The temperature was raised to 780°C and kept for 4 hours; then the temperature was naturally cooled to room temperature to obtain Ag / CoFe2O4-U alkaline water electrolysis catalyst, which was named Ag / CoFe2O4-S3.

[0050] Comparative Example 1

[0051] A CoFe2O4 alkaline water electrolysis catalyst, the preparation method of which comprises the following steps:

[0052] (1) Dissolve 0.05 mol of Co(NO3)2·6H2O, 0.1 mol of Fe(NO3)3·9H2O and 0.225 mol of C6H8O7·H2O in 200 ml of deionized water and stir to form a uniform solution; heat and dry the solution at 200°C for 12 h to obtain a CoFe2O4 precursor;

[0053] (2) The CoFe2O4 precursor was heated at 6℃min in air atmosphere. -1 The temperature was raised to 400°C at a rate of 100°C, kept at that temperature for 4 hours, and then cooled to room temperature; then the temperature was raised to 400°C at a rate of 2°C min -1 The temperature was raised to 400℃ and kept at this temperature for 1h; then the temperature was raised to 400℃ and kept at this temperature for 1h. -1 The temperature was raised to 500℃ and kept at this temperature for 1h; then the temperature was raised at 3℃min -1 The temperature was raised to 800°C at a heating rate of , and then naturally cooled to room temperature after being kept for 4 hours to obtain a CoFe2O4 catalyst, which was named CoFe2O4.

[0054] Comparative Example 2

[0055] An Ag / CoFe2O4 alkaline water electrolysis catalyst is prepared by the following steps:

[0056] (1) Dissolve 0.05 mol of Co(NO3)2·6H2O, 0.1 mol of Fe(NO3)3·9H2O and 0.225 mol of C6H8O7·H2O in 200 ml of deionized water and stir to form a uniform solution; heat and dry the solution at 200°C for 12 h to obtain a CoFe2O4 precursor;

[0057] (2) The CoFe2O4 precursor was heated at 6℃min in air atmosphere. -1 The temperature was raised to 400°C at a rate of 100°C, kept at that temperature for 4 hours, and then cooled to room temperature; then the temperature was raised to 400°C at a rate of 2°C min -1 The temperature was raised to 400℃ and kept at this temperature for 1h; then the temperature was raised to 400℃ and kept at this temperature for 1h. -1 The temperature was raised to 500℃ and kept at this temperature for 1h; then the temperature was raised at 3℃min -1 The temperature was raised to 800°C at a heating rate of 100°C, kept at that temperature for 4 hours, and then naturally cooled to room temperature to obtain a CoFe2O4 catalyst;

[0058] (3) 70 ml of anhydrous ethanol and 30 ml of deionized water were mixed to obtain a mixed solvent; 1.70 g of AgNO3 was weighed and dissolved in the mixed solvent and stirred to form an impregnation solution; 23.18 ml of the impregnation solution was mixed with 4.75 g of CoFe2O4 catalyst, stirred at room temperature for 1 h, and then heated and dried at 100°C for 12 h to obtain an Ag / CoFe2O4 precursor;

[0059] (4) The Ag / CoFe2O4 precursor was heated at 2°C min in air atmosphere. -1 The temperature was raised to 400℃ and kept at this temperature for 1h; then the temperature was raised to 400℃ and kept at this temperature for 1h. -1 The temperature was raised to 500℃ and kept at this temperature for 1h; then the .... -1 The temperature was raised to 800°C at a rate of 100 °C and kept for 4 h; then the temperature was naturally cooled to room temperature to obtain Ag / CoFe2O4 alkaline water electrolysis catalyst, which was named Ag / CoFe2O4-D2.

[0060] Experimental example

[0061] The Ag / CoFe2O4 alkaline water electrolysis catalysts prepared in Examples 1 to 3 have similar performances. Taking the Ag / CoFe2O4-S1 alkaline water electrolysis catalyst in Example 1 as an example, its performance is described.

[0062] XRD analysis was performed on the alkaline water electrolysis catalysts in Example 1, Comparative Example 1 and Comparative Example 2. The results are as follows: Figure 1 The characteristic peaks of the sample CoFe2O4 correspond to the (003), (104), (113), (024) and (125) crystal planes, and Ag corresponds to the (111), (200) and (220) crystal planes.

[0063] The Ag / CoFe2O4-S1 alkaline water electrolysis catalyst in Example 1 was subjected to SEM analysis, and the results were as follows: Figure 2 As shown in the figure, it can be seen that Ag nanoparticles are uniformly attached to the surface of CoFe2O4, where the diameter of Ag nanoparticles is about 8-10nm, and the particle size of CoFe2O4 is about 400-500nm. The loading of Ag nanoparticles increases the specific surface area of ​​the catalyst and improves the exposure of active sites, which is conducive to the adsorption of reactants and the occurrence of reactions. At the same time, the conductivity of Ag nanoparticles may promote electron transfer and catalytic reactions, improving its catalytic performance.

[0064] 10 mg of each alkaline water electrolysis catalyst in Example 1, Comparative Example 1 and Comparative Example 2 were taken, mixed with 10 mg of SuperP Li respectively, and then dispersed into a mixture solution of 1 ml of anhydrous ethanol and 0.1 ml of Nafion respectively, and ultrasonicated for 30 min to form a uniform slurry. 0.23 ml of the catalyst slurry was uniformly dropped on a 1×1×0.1 cm nickel foam electrode as a working electrode.

[0065] Electrochemical test: The electrochemical test was performed using a DH7000 electrochemical workstation (Jiangsu Donghua Analytical Instrument Co., Ltd.) using a traditional three-electrode system: the electrode prepared using the alkaline water electrolysis catalyst in Example 1, Comparative Example 1 and Comparative Example 2 was used as the working electrode, the graphite rod was used as the counter electrode, and the mercury / mercury oxide (Hg / HgO) electrode was used as the reference electrode (all electrodes were calibrated to the reversible hydrogen electrode RHE, the same below). The electrochemical tests were all performed in 1M KOH solution, and the oxygen evolution reaction (OER) curve (the potential was set to 0-1V vs. RHE) and the hydrogen evolution reaction (HER) curve (the potential was set to 0-2V vs. RHE) were tested by linear sweep voltammetry (LSV), with a scan rate of 0.01V s -1 , OER and HER curves were IR corrected; in addition, electrochemical impedance spectroscopy (EIS) tests were performed with a frequency range of 0.1-100 kHz and an amplitude of 10 mV; a two-electrode battery was constructed for full water splitting performance testing, and linear sweep voltammetry (LSV) was used to test the full water splitting polarization curve (the potential was set at 0-2.5 V); at the same time, the electrolyte was charged at 20 mA cm in 1 M KOH. -2 The stability test was carried out for 100 hours. The specific test results are shown in Figures 3 to 8 .

[0066] Figure 3 The polarization curves of oxygen evolution reaction of CoFe2O4, Ag / CoFe2O4-D2 and Ag / CoFe2O4-S1 in 1M KOH are shown in the figure. It can be seen that at a current density of 50mA cm -2 When , the corresponding overpotentials of CoFe2O4, Ag / CoFe2O4-D2 and Ag / CoFe2O4-S1 are 520mV, 500mV and 440mV respectively.

[0067] Figure 4 The electrochemical impedance spectra of CoFe2O4, Ag / CoFe2O4-D2 and Ag / CoFe2O4-S1 in 1M KOH are as follows: at @1.52V vs.RHE, the ohmic resistances of CoFe2O4, Ag / CoFe2O4-D2 and Ag / CoFe2O4-S1 are 27.25Ω, 24.35Ω and 18.25Ω, respectively.

[0068] Figure 5 The polarization curves of the hydrogen evolution reaction of CoFe2O4, Ag / CoFe2O4-D2 and Ag / CoFe2O4-S1 in 1M KOH are shown in the figure. -2 When , the corresponding overpotentials of CoFe2O4, Ag / CoFe2O4-D2 and Ag / CoFe2O4-S1 are 466mV, 446mV and 434mV respectively.

[0069] Figure 6 The electrochemical impedance spectra of CoFe2O4, Ag / CoFe2O4-D2 and Ag / CoFe2O4-S1 in 1M KOH are as follows: at @-0.37vs.RHE, the ohmic resistances of CoFe2O4, Ag / CoFe2O4-D2 and Ag / CoFe2O4-S1 are 0.99Ω, 0.79Ω and 0.62Ω respectively.

[0070] Figure 7 The polarization curves of CoFe2O4, Ag / CoFe2O4-D2 and Ag / CoFe2O4-S1 in 1M KOH for complete hydrolysis are shown in the figure. -2 When , the corresponding overpotentials of CoFe2O4, Ag / CoFe2O4-D2 and Ag / CoFe2O4-S1 are 2.36V, 2.29V and 2.24V respectively.

[0071] Figure 8 The stability test of CoFe2O4, Ag / CoFe2O4-D2 and Ag / CoFe2O4-S1 in 1M KOH is shown in the figure. -2 The stability test was carried out for 100 hours and there was no obvious voltage attenuation.

[0072] Although the specific implementation of the present invention is described in detail in conjunction with the embodiments, it should not be understood as limiting the scope of protection of this patent. Within the scope described in the claims, various modifications and variations that can be made by those skilled in the art without creative work still fall within the scope of protection of this patent.

Claims

1. A method for preparing an Ag / CoFe2O4 alkaline water electrolysis catalyst, characterized in that: The following steps are involved: S1: Dissolve cobalt salt, iron salt and citric acid in a solvent, heat and dry at 180-250°C for 10-15h to obtain a CoFe2O4 precursor; S2: calcining the CoFe2O4 precursor to obtain a CoFe2O4 catalyst; S3: dissolving silver salt and urea in a mixed solvent of anhydrous ethanol and deionized water to obtain an impregnation solution, mixing the CoFe2O4 catalyst with the impregnation solution, stirring the mixture for reaction, and then heating and drying at 90 to 120° C. for 10 to 15 hours to obtain an Ag / CoFe2O4 precursor; S4: Heat the Ag / CoFe2O4 precursor to 380-420°C at a heating rate of 2°C / min, and keep it warm for 0.5-2h; then heat it to 480-520°C at a heating rate of 1°C / min, and keep it warm for 0.5-2h; then heat it to 780-820°C at a heating rate of 3°C / min, and keep it warm for 4h; then naturally cool it to room temperature.

2. The preparation method according to claim 1, characterized in that: The molar ratio of the cobalt salt, the iron salt and the citric acid is 1:2:4.

5.

3. The preparation method according to claim 1 or 2, characterized in that: The cobalt salt is Co(NO3)2·6H2O, the iron salt is Fe(NO3)3·9H2O; and the solvent is deionized water.

4. The preparation method according to claim 1, characterized in that: The heating and drying temperature in S1 is 200° C., and the heating and drying time is 12 h.

5. The preparation method according to claim 1, characterized in that: The calcination process in S2 is as follows: in an air atmosphere, the CoFe2O4 precursor is heated to 380-420°C at a heating rate of 5-7°C / min, kept warm for 3.5-5h, and then air-cooled to room temperature; then heated to 380-420°C at a heating rate of 2°C / min, and kept warm for 0.5-2h; then heated to 480-520°C at a heating rate of 1°C / min, and kept warm for 0.5-2h; then heated to 780-820°C at a heating rate of 3°C / min, and kept warm for 4h; then naturally cooled to room temperature.

6. The preparation method according to claim 1, characterized in that: The mixed solvent is prepared by mixing anhydrous ethanol and deionized water in a volume ratio of 7:

3.

7. The preparation method according to claim 1, characterized in that: The concentration of silver salt and urea in the impregnation solution is 0.1 mol / L; the CoFe2O4 catalyst and the impregnation solution are mixed in a mass ratio of Ag:CoFe2O4=5:

95.

8. The preparation method according to claim 1 or 7, characterized in that: The silver salt is AgNO3.

9. The preparation method according to claim 1, characterized in that: The stirring reaction time in S3 is 1 hour; the heating and drying temperature is 100° C., and the heating and drying time is 12 hours.

10. The Ag / CoFe2O4 alkaline water electrolysis catalyst prepared by the preparation method according to any one of claims 1 to 8.