Titanium dioxide nanotube loaded ruthenium oxide particle anode material as well as preparation method and application thereof

By growing titanium dioxide nanotube arrays on titanium foil and impregnating ruthenium oxide salts, the titanium dioxide nanotube-loaded ruthenium oxide particle anode material is prepared by horizontal rotation calcining method, which solves the problems of high cost and insufficient stability of precious metal anode materials, and achieves high efficiency Chlorine evolution reaction and stability are improved, suitable for industrial applications.

CN118996483APending Publication Date: 2024-11-22CHINA UNIV OF GEOSCIENCES (WUHAN)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411129410.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The precious metal or precious metal oxide anode materials used in the chlorine analysis reaction are costly and have insufficient stability, which leads to the active layer being easily eroded and chemically corroded by the electrolyte during long-term use, and severe wear, which limits its commercialization and Large-scale application.

Method used

After growing a titanium dioxide nanotube array on titanium foil and calcining it in a muffle furnace to form an anatase structure, the ruthenium oxide salt solution is impregnated, and the titanium dioxide nanotube supported ruthenium oxide particle anode material is prepared by horizontal rotation calcining method to improve the catalyst and The binding force of the substrate and the dispersion of the ruthenium oxide particles.

Benefits of technology

It significantly improves the stability and activity of the catalyst, extends the service life, reduces production costs, is suitable for large-scale industrial production, and improves the activity and selectivity of the chlorine evolution reaction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996483A_ABST
    Figure CN118996483A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of electrochemical materials, in particular to a titanium dioxide nanotube loaded ruthenium oxide particle anode material and a preparation method and application thereof. The preparation method comprises the following steps: S1, cleaning a titanium foil; s2, preparing a titanium dioxide nanotube array on the titanium foil by an anodic oxidation method; s3, calcining the titanium foil obtained in the step S2 in a muffle furnace for a period of time; and S4, dipping the titanium foil obtained in the step S3 in a ruthenium salt solution, taking out the titanium foil, airing the titanium foil, horizontally rotating the titanium foil, placing the titanium foil in a muffle furnace, and calcining the titanium foil to obtain the titanium dioxide nanotube loaded ruthenium oxide particle anode material. The titanium dioxide nanotube array disclosed by the invention is beneficial to dispersion of ruthenium oxide particles, and meanwhile, through horizontal rotary calcination, when nanotubes are vertically downward, steam can enable the ruthenium oxide nanoparticles on the surface to be uniformly dispersed and push more particles to enter the nanotubes, so that active sites are increased, the reaction active area is increased, and the catalytic activity is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electrochemical materials, and in particular to a titanium dioxide nanotube-loaded ruthenium oxide particle anode material and a preparation method and application thereof. Background Art

[0002] The chlorine evolution reaction occupies a core position in industrial electrochemical reactions. Its product, chlorine, produces more than 70 million tons of chlorine per year and is widely used in water treatment, organic synthesis, and polyvinyl chloride production. At present, industrial chlorine evolution reactions mostly rely on "dimensionally stable anodes", such as electrode materials such as ruthenium / titanium mixed oxides or ruthenium / iridium / titanium mixed oxides. However, current commercial anodes use a large amount of precious metals or precious metal oxides as active layers, which have high manufacturing costs and limit their commercialization and large-scale applications. In addition, the active layer of the dimensionally stable anode is attached to the titanium substrate through a coating and calcination process, and the bonding force is weak, resulting in the active layer being easily eroded and chemically corroded by the electrolyte during long-term use, thereby gradually wearing out and lacking stability. Therefore, it is particularly critical to develop chlorine evolution electrocatalysts that contain less precious metals and have excellent stability. Summary of the invention

[0003] The purpose of the present invention is to address the above-mentioned deficiencies in the prior art and to provide a titanium dioxide nanotube-loaded ruthenium oxide particle anode material and a preparation method and application thereof.

[0004] The present invention provides a method for preparing a titanium dioxide nanotube-loaded ruthenium oxide particle anode material, comprising the following steps:

[0005] A method for preparing a titanium dioxide nanotube-loaded ruthenium oxide particle anode material comprises the following steps:

[0006] S1, cleaning titanium foil;

[0007] S2, growing titanium dioxide nanotube arrays on titanium foil by anodization;

[0008] S3, calcining the titanium foil obtained in step S2 in a muffle furnace for a period of time to form an anatase titanium dioxide crystal structure;

[0009] S4, immersing the titanium foil obtained in step S3 in a ruthenium salt solution, taking it out and drying it, and calcining the titanium foil while keeping it in a horizontal rotation to obtain the titanium dioxide nanotube-loaded ruthenium oxide particle anode material.

[0010] Furthermore, in step S2, the anodization voltage is 20 to 30 V and the time is 1 to 2 hours.

[0011] Furthermore, the anodizing electrolyte is an ethylene glycol solution containing ammonium fluoride and a small amount of deionized water, the ammonium fluoride content is 0.13-0.14 M / L, and the volume ratio of the deionized water to the ethylene glycol solution is 5-10 mL:50-100 mL.

[0012] Furthermore, in step S3, the calcination temperature is 400-500° C., and the calcination time is 1-2 hours.

[0013] Furthermore, in step S4, the ruthenium salt is anhydrous ruthenium trichloride or hydrous ruthenium trichloride, and the ruthenium salt solution is a mixed solution of ethanol and water, with the ratio of ethanol to water being 2-3:2-1.

[0014] Furthermore, the concentration of the ruthenium salt is 0.05-0.08 M / L.

[0015] Furthermore, the calcination temperature is 400-500° C., and the calcination time is 0.5-1 h.

[0016] A titanium dioxide nanotube-loaded ruthenium oxide particle anode material prepared by the above-mentioned preparation method.

[0017] An application of the titanium dioxide nanotube-loaded ruthenium oxide particle anode material as described above in electrolyzing salt water to prepare a sodium hypochlorite solution.

[0018] Furthermore, the sodium hypochlorite solution is prepared by electrolyzing salt water at room temperature and using a 6 mol / L sodium chloride solution as an electrolyte.

[0019] The titanium dioxide nanotube array grown in situ by anodic oxidation has a strong bonding force with the substrate, which greatly improves the stability of the catalyst and thus prolongs the service life of the catalyst.

[0020] In addition, the titanium dioxide nanotube array, due to its hollow tubular structure, is conducive to the dispersion of ruthenium oxide particles, reduces aggregation, and evenly distributes the catalyst, which can provide more active surfaces for catalytic reactions, thereby improving the stability and activity of the catalyst. At the same time, through horizontal rotation calcination, when the nanotubes are vertically downward, the steam can make the ruthenium oxide nanoparticles on the surface evenly dispersed and push more particles into the interior of the nanotubes, increasing the active sites, increasing the reaction active area, and improving the catalytic activity. The chlorine evolution activity and selectivity of the titanium dioxide nanotube-loaded ruthenium oxide particle anode material are greatly improved, and the ruthenium oxide nanoparticles on the surface are evenly dispersed, reducing the contact angle of the electrode surface, which is conducive to the infiltration of the electrolyte.

[0021] The synthesis process of the invention has simple steps, convenient operation, short reaction time, reliable repeatability and low production cost, and is very suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a scanning electron microscope image of the titanium dioxide nanotube-loaded ruthenium oxide particle anode material prepared in Example 1;

[0023] Figure 2 This is a scanning electron microscope image of the titanium dioxide nanotube-loaded ruthenium oxide particle anode material prepared in Comparative Example 1;

[0024] Figure 3 This is a graph showing the chlorine evolution selectivity of the titanium dioxide nanotube-loaded ruthenium oxide particle anode material prepared in Example 1;

[0025] Figure 4 This is a contact angle diagram of the titanium dioxide nanotube-loaded ruthenium oxide particle anode material prepared in Example 1;

[0026] Figure 5 This is a contact angle diagram of the titanium dioxide nanotube-loaded ruthenium oxide particle anode material prepared in Comparative Example 1;

[0027] Figure 6 This is an X-ray diffraction pattern of the titanium dioxide nanotube-loaded ruthenium oxide particle anode material prepared in Example 1 of the present application;

[0028] Figure 7 This is a stability test diagram of the titanium dioxide nanotube-loaded ruthenium oxide particle anode material prepared in Example 1 of the present application;

[0029] Figure 8 This is a comparison chart of the chlorine evolution reaction activity of the titanium dioxide nanotube-loaded ruthenium oxide particle anode material prepared in Comparative Examples 1-5 of the present application and the commercial anode and this Example 1;

[0030] Fig. 9 This is a comparison chart of the chlorine evolution reaction activity of the titanium dioxide nanotube-loaded ruthenium oxide particle anode materials prepared in Examples 1-5 of the present application. DETAILED DESCRIPTION

[0031] The following are specific embodiments of the present invention and the accompanying drawings to further describe the technical solution of the present invention, but the present invention is not limited to these embodiments.

[0032] Example 1

[0033] (1) Pretreatment of titanium foil substrate: The titanium foil (30 mm × 20 mm × 0.3 mm) was placed in a mixed solution of acetone, ethanol and water (1:1:1) and ultrasonically cleaned for 30 min. After the ultrasonic cleaning, it was rinsed with deionized water several times.

[0034] (2) Anodic oxidation growth of titanium dioxide nanotube arrays: At room temperature, using a two-electrode electrochemical power source, the treated titanium foil was placed in an ethylene glycol solution (60 mL) containing ammonium fluoride (0.135 M / L) and a small amount of deionized water (6 mL), and anodized at 20 V for 2 h to prepare titanium dioxide nanotube arrays;

[0035] (3) calcining the obtained titanium dioxide nanotube array in a muffle furnace for 2 hours at a calcination temperature of 450° C. to obtain anatase titanium dioxide crystal structure;

[0036] (4) Loading ruthenium oxide nanoparticles: The titanium foil obtained in step (3) was immersed in a mixed solution of RuCl3·xH2O ethanol and water (0.06M / L, ethanol: water = 3:1) for 2 h, taken out and air-dried, and then placed in a muffle furnace and horizontally rotated for calcination at a calcination temperature of 450°C and a calcination time of 0.5 h to obtain a chlorine evolution catalytic electrode of titanium dioxide loaded with ruthenium oxide particles.

[0037] Example 2

[0038] (1) Pretreatment of titanium foil substrate: The titanium foil (30 mm × 20 mm × 0.3 mm) was placed in a mixed solution of acetone, ethanol and water (1:1:1) and ultrasonically cleaned for 30 min. After the ultrasonic cleaning, it was rinsed with deionized water several times.

[0039] (2) Anodic oxidation growth of titanium dioxide nanotube arrays: At room temperature, using a two-electrode electrochemical power source, the treated titanium foil was placed in an ethylene glycol solution (60 mL) containing ammonium fluoride (0.135 M / L) and a small amount of deionized water (6 mL), and anodized at 20 V for 2 h to prepare titanium dioxide nanotube arrays;

[0040] (3) calcining the obtained titanium dioxide nanotube array in a muffle furnace for 2 hours at a calcination temperature of 450° C. to obtain anatase titanium dioxide crystal structure;

[0041] (4) Loading ruthenium oxide nanoparticles: The titanium foil obtained in step (3) is immersed in a mixed solution of RuCl3·xH2O ethanol and water (0.06M / L, ethanol: water = 1:1) for 2 h, taken out and air-dried, and then placed in a muffle furnace and horizontally rotated for calcination at a calcination temperature of 450°C and a calcination time of 1 h to obtain a chlorine evolution catalytic electrode of titanium dioxide loaded with ruthenium oxide particles.

[0042] Example 3

[0043] (1) Pretreatment of titanium foil substrate: The titanium foil (30 mm × 20 mm × 0.3 mm) was placed in a mixed solution of acetone, ethanol and water (1:1:1) and ultrasonically cleaned for 30 min. After the ultrasonic cleaning, it was rinsed with deionized water several times.

[0044] (2) Anodic oxidation growth of titanium dioxide nanotube arrays: At room temperature, using a two-electrode electrochemical power source, the treated titanium foil was placed in an ethylene glycol solution (60 mL) containing ammonium fluoride (0.135 M / L) and a small amount of deionized water (6 mL), and anodized at 20 V for 2 h to prepare titanium dioxide nanotube arrays;

[0045] (3) calcining the obtained titanium dioxide nanotube array in a muffle furnace for 2 hours at a calcination temperature of 450° C. to obtain anatase titanium dioxide crystal structure;

[0046] (4) Loading ruthenium oxide nanoparticles: The titanium foil obtained in step (3) is immersed in a mixed solution of RuCl3·xH2O ethanol and water (0.06M / L, ethanol: water = 1:3) for 2 h, taken out and air-dried, and then placed in a muffle furnace and horizontally rotated for calcination at a calcination temperature of 450°C and a calcination time of 1 h to obtain a chlorine evolution catalytic electrode of titanium dioxide loaded with ruthenium oxide particles.

[0047] Example 4

[0048] (1) Pretreatment of titanium foil substrate: The titanium foil (30 mm × 20 mm × 0.3 mm) was placed in a mixed solution of acetone, ethanol and water (1:1:1) and ultrasonically cleaned for 30 min. After the ultrasonic cleaning, it was rinsed with deionized water several times.

[0049] (2) Anodic oxidation growth of titanium dioxide nanotube arrays: At room temperature, using a two-electrode electrochemical power source, the treated titanium foil was placed in an ethylene glycol solution (60 mL) containing ammonium fluoride (0.135 M / L) and a small amount of deionized water (6 mL), and anodized at 30 V for 1 h to prepare titanium dioxide nanotube arrays;

[0050] (3) calcining the obtained titanium dioxide nanotube array in a muffle furnace for 2 hours at a calcination temperature of 450° C. to obtain anatase titanium dioxide crystal structure;

[0051] (4) Loading ruthenium oxide nanoparticles: The titanium foil obtained in step (3) was immersed in a mixed solution of RuCl3·xH2O ethanol and water (0.06M / L, ethanol: water = 3:1) for 2 h, taken out and air-dried, and then placed in a muffle furnace and horizontally rotated for calcination at a calcination temperature of 450°C and a calcination time of 0.5 h to obtain a chlorine evolution catalytic electrode of titanium dioxide loaded with ruthenium oxide particles.

[0052] Example 5

[0053] (1) Pretreatment of titanium foil substrate: The titanium foil (30 mm × 20 mm × 0.3 mm) was placed in a mixed solution of acetone, ethanol and water (1:1:1) and ultrasonically cleaned for 30 min. After the ultrasonic cleaning, it was rinsed with deionized water several times.

[0054] (2) Anodic oxidation growth of titanium dioxide nanotube arrays: At room temperature, using a two-electrode electrochemical power source, the treated titanium foil was placed in an ethylene glycol solution (80 mL) containing ammonium fluoride (0.14 M / L) and a small amount of deionized water (8 mL), and anodized at 30 V for 1 h to prepare titanium dioxide nanotube arrays;

[0055] (3) calcining the obtained titanium dioxide nanotube array in a muffle furnace for 2 hours at a calcination temperature of 450° C. to obtain anatase titanium dioxide crystal structure;

[0056] (4) Loading ruthenium oxide nanoparticles: The titanium foil obtained in step (3) was immersed in a mixed solution of RuCl3·xH2O ethanol and water (0.06M / L, ethanol: water = 3:1) for 2 h, taken out and air-dried, and then placed in a muffle furnace and horizontally rotated for calcination at a calcination temperature of 450°C and a calcination time of 0.5 h to obtain a chlorine evolution catalytic electrode of titanium dioxide loaded with ruthenium oxide particles.

[0057] Comparative Example 1

[0058] (1) Pretreatment of titanium foil substrate: The titanium foil (30 mm × 20 mm × 0.3 mm) was placed in a mixed solution of acetone, ethanol and water (1:1:1) and ultrasonically cleaned for 30 min. After the ultrasonic cleaning, it was rinsed with deionized water several times.

[0059] (2) Anodic oxidation growth of titanium dioxide nanotube arrays: At room temperature, using a two-electrode electrochemical power source, the treated titanium foil was placed in an ethylene glycol solution (60 mL) containing ammonium fluoride (0.135 M / L) and a small amount of deionized water (6 mL), and anodized at 20 V for 2 h to prepare titanium dioxide nanotube arrays;

[0060] (3) calcining the obtained titanium dioxide nanotube array in a muffle furnace for 2 hours at a calcination temperature of 450° C. to obtain anatase titanium dioxide crystal structure;

[0061] (4) Loading ruthenium oxide nanoparticles: The titanium foil obtained in step (3) was immersed in a mixed solution of RuCl3·xH2O ethanol and water (0.06M / L, ethanol: water = 3:1) for 2 hours, taken out and air-dried, and then placed horizontally in a muffle furnace for calcination (the horizontal upward surface is the prepared chlorine evolution catalyst), the calcination temperature is 450°C, the calcination time is 0.5 hours, and a chlorine evolution catalytic electrode of titanium dioxide loaded with ruthenium oxide particles is prepared.

[0062] Comparative Example 2

[0063] (1) Pretreatment of titanium foil substrate: The titanium foil (30 mm × 20 mm × 0.3 mm) was placed in a mixed solution of acetone, ethanol and water (1:1:1) and ultrasonically cleaned for 30 min. After the ultrasonic cleaning, it was rinsed with deionized water several times.

[0064] (2) Loading ruthenium oxide nanoparticles: The titanium foil obtained in step (1) is immersed in a mixed solution of RuCl3·xH2O ethanol and water (0.06M / L, ethanol: water = 1:1) for 2 h, taken out and air-dried, and then placed in a muffle furnace and horizontally rotated for calcination at a calcination temperature of 450°C and a calcination time of 1 h to obtain a chlorine evolution catalytic electrode of titanium foil loaded with ruthenium oxide particles.

[0065] Comparative Example 3

[0066] (1) Pretreatment of titanium foil substrate: The titanium foil (30 mm × 20 mm × 0.3 mm) was placed in a mixed solution of acetone, ethanol and water (1:1:1) and ultrasonically cleaned for 30 min. After the ultrasonic cleaning, it was rinsed with deionized water several times.

[0067] (2) Loading ruthenium oxide nanoparticles: The titanium foil obtained in step (1) is immersed in a mixed solution of RuCl3·xH2O ethanol and water (0.06M / L, ethanol: water = 1:1) for 2 hours, taken out and air-dried, then placed horizontally in a muffle furnace for calcination (the horizontal upward surface is the prepared chlorine evolution catalyst), the calcination temperature is 450°C, the calcination time is 1 hour, and a chlorine evolution catalytic electrode of titanium foil loaded with ruthenium oxide particles is prepared.

[0068] Comparative Example 4

[0069] (1) Pretreatment of titanium foil substrate: The titanium foil (30 mm × 20 mm × 0.3 mm) was placed in a mixed solution of acetone, ethanol and water (1:1:1) and ultrasonically cleaned for 30 min. After the ultrasonic cleaning, it was rinsed with deionized water several times.

[0070] (2) Anodic oxidation growth of titanium dioxide nanotube arrays: At room temperature, using a two-electrode electrochemical power source, the treated titanium foil was placed in an ethylene glycol solution (60 mL) containing ammonium fluoride (0.135 M / L) and a small amount of deionized water (6 mL), and anodized at 20 V for 2 h to prepare titanium dioxide nanotube arrays;

[0071] (3) calcining the obtained titanium dioxide nanotube array in a muffle furnace for 2 hours at a calcination temperature of 450° C. to obtain anatase titanium dioxide crystal structure;

[0072] (4) Loading ruthenium oxide nanoparticles: The titanium foil obtained in step (3) is immersed in a mixed solution of RuCl3·xH2O ethanol and water (0.06M / L, ethanol: water = 3:1) for 2 hours, taken out and air-dried, and then placed horizontally in a muffle furnace for calcination (the horizontal downward surface is the prepared chlorine evolution catalyst), the calcination temperature is 450°C, the calcination time is 0.5 hours, and a chlorine evolution catalytic electrode of titanium dioxide loaded with ruthenium oxide particles is prepared.

[0073] Comparative Example 5

[0074] (1) Pretreatment of titanium foil substrate: The titanium foil (30 mm × 20 mm × 0.3 mm) was placed in a mixed solution of acetone, ethanol and water (1:1:1) and ultrasonically cleaned for 30 min. After the ultrasonic cleaning, it was rinsed with deionized water several times.

[0075] (2) Loading ruthenium oxide nanoparticles: The titanium foil obtained in step (1) is immersed in a mixed solution of RuCl3·xH2O ethanol and water (0.06M / L, ethanol: water = 1:1) for 2 hours, taken out and air-dried, and then suspended horizontally in a muffle furnace for calcination (the horizontal downward surface is the prepared chlorine evolution catalyst), the calcination temperature is 450°C, the calcination time is 1 hour, and a chlorine evolution catalytic electrode of titanium foil loaded with ruthenium oxide particles is prepared.

[0076] Performance Testing:

[0077] The test process of the chlorine evolution selectivity of the anode material is as follows: the standard iodine titration method is used for determination. In the three-electrode system, the counter electrode is a titanium sheet and the reference electrode is a saturated calomel electrode. 60mL of saturated NaCl solution is fully electrolyzed for 30 minutes, and then 20mL of the electrolytic solution is transferred to a 500mL volumetric flask for dilution to obtain a test solution. Finally, 10mL of the test solution is titrated, and then 10mL of KI (100g / L) and 10mL of H2SO4 (0.5mol / L) solution are added in sequence. Subsequently, 2mL of starch indicator solution (10g / L) is added to the iodine volumetric flask, and the color of the solution changes to blue. Finally, titrate with sodium thiosulfate standard solution (0.001M / L) until the blue color disappears.

[0078] The stability test process of the anode material is as follows: the stability test is carried out in a three-electrode system, the test solution is saturated NaCl, the test temperature is room temperature, and the test current density is 100mA / cm 2 , the testing time is 15 days.

[0079] The chlorine evolution reaction activity process of the anode material is as follows: the chlorine evolution activity test is carried out in a three-electrode system, the prepared titanium dioxide nanotube-loaded ruthenium oxide particle anode material is the working electrode, the titanium sheet is the counter electrode, the saturated calomel electrode is the reference electrode, and the test voltage range is 0.8~1.8V vs.SCE.

[0080] Figure 1 This is a scanning electron microscope image of the titanium dioxide nanotube-loaded ruthenium oxide particle anode material prepared in Example 1. It can be seen from the image that the particles grow evenly and are relatively dispersed.

[0081] Figure 2 This is a scanning electron microscope image of the titanium dioxide nanotube-loaded ruthenium oxide particle anode material prepared in Comparative Example 1. It can be seen from the image that the ruthenium oxide nanoparticles are obviously aggregated.

[0082] Figure 3 This is a selectivity diagram of the titanium dioxide nanotube-loaded ruthenium oxide particle anode material prepared in Example 1. It can be seen that the chlorine evolution selectivity of Example 1 prepared is as high as over 90%.

[0083] Figure 4 This is a contact angle diagram of the titanium dioxide nanotube-loaded ruthenium oxide particle anode material prepared in Example 1. Since the prepared electrode nanoparticles are evenly dispersed and the contact angle is small, it means that the electrolyte has good wettability, which is conducive to the catalytic reaction.

[0084] Figure 5 This is a contact angle diagram of the titanium dioxide nanotube-loaded ruthenium oxide particle anode material prepared in Comparative Example 1. Since the prepared electrode nanoparticles are obviously aggregated, the contact angle is large, indicating that the electrolyte wettability is poor, which is not conducive to the catalytic reaction.

[0085] Figure 6 This is the X-ray diffraction diagram of Example 1. It can be seen from the figure that the diffraction peaks of Example 1 are consistent with the PDF cards of RuO2 and TiO2, confirming the successful synthesis of titanium dioxide nanotubes and the successful loading of ruthenium oxide particles.

[0086] Figure 7 This is a stability test chart of the titanium dioxide nanotube-loaded ruthenium oxide particle anode material prepared in Example 1. It can be seen that the voltage of the prepared titanium dioxide nanotube-loaded ruthenium oxide particle anode material remains basically unchanged after 15 days of testing at a large current density, and has excellent stability. This is because the titanium dioxide nanotubes are firmly bonded to the titanium substrate and the tubular structure has a protective effect on the ruthenium oxide nanoparticles.

[0087] Figure 8This is a comparison chart of the chlorine evolution reaction activity of the composite electrocatalyst obtained by testing Example 1, Comparative Examples 1-5 and a commercial anode (DSA, China National Energy Group Co., Ltd.) under a standard three-electrode system. It can be found that the chlorine evolution performance of the prepared titanium dioxide nanotube-loaded ruthenium oxide particle anode material is: Example 1 is better than Comparative Example 1, Comparative Example 2 is better than Comparative Example 3, Comparative Example 1 is better than Comparative Example 4, and Comparative Example 2 is better than Comparative Example 5, which fully demonstrates the superiority of the rotary calcination used in the present invention: the ruthenium oxide nanoparticles are evenly dispersed and more particles are pushed into the nanotubes, which increases the catalyst active sites and improves the catalytic activity.

[0088] Fig. 9 The comparison chart of the chlorine evolution reaction activity of the titanium dioxide nanotube-loaded ruthenium oxide particle anode materials prepared in Examples 1-5 of the present application shows that Examples 1-5 prepared by horizontal rotary calcination all have good chlorine evolution activity, and Example 1 has the best chlorine evolution activity.

[0089] In step (4) of Example 2 and Example 1, the calcination temperatures are different, resulting in different oxidation degrees of ruthenium oxide, which leads to differences in catalytic performance compared with Example 1.

[0090] In step (4) of Example 3 and Example 1, the ratio of ethanol to water is different, resulting in differences in the dispersibility and loading of ruthenium oxide, and thus in its catalytic performance being different from that of Example 1.

[0091] The difference between Example 4 and Example 1 is that the voltage and oxidation time of step (2) are different, so that the grown titanium dioxide nanotube array is different from that of Example 1, resulting in different catalytic performance from that of Example 1.

[0092] The difference in Example 5 is that the specific parameters of step (2) are different, so that the grown titanium dioxide nanotube array is different from that in Example 1, resulting in different catalytic performance from that in Example 1.

[0093] For matters not mentioned above, the prior art applies.

[0094] Although some specific embodiments of the present invention have been described in detail through examples, those skilled in the art should understand that the above examples are for illustration only and are not intended to limit the scope of the present invention. Those skilled in the art to which the present invention belongs may make various modifications or supplements to the specific embodiments described or replace them in a similar manner, but they will not deviate from the direction of the present invention or exceed the scope defined by the attached claims. Those skilled in the art should understand that any modifications, equivalent substitutions, improvements, etc. made to the above embodiments based on the technical essence of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a titanium dioxide nanotube-loaded ruthenium oxide particle anode material, characterized in that: The steps include: S1, cleaning titanium foil; S2, growing titanium dioxide nanotube arrays on titanium foil by anodization; S3, calcining the titanium foil obtained in step S2 in a muffle furnace for a period of time to form an anatase titanium dioxide crystal structure; S4, immersing the titanium foil obtained in step S3 in a ruthenium salt solution, taking it out and drying it, and calcining the titanium foil while keeping it in a horizontal rotation to obtain the titanium dioxide nanotube-loaded ruthenium oxide particle anode material.

2. The preparation method according to claim 1, characterized in that In step S2, the anodization voltage is 20 to 30 V and the time is 1 to 2 hours.

3. The preparation method according to claim 1, characterized in that: The anodizing electrolyte is an ethylene glycol solution containing ammonium fluoride and a small amount of deionized water, the ammonium fluoride content is 0.13-0.14 M / L, and the volume ratio of the deionized water to the ethylene glycol solution is 5-10 mL:50-100 mL.

4. The preparation method according to claim 1, characterized in that: In step S3, the calcination temperature is 400-500° C., and the calcination time is 1-2 hours.

5. The preparation method according to claim 1, characterized in that: In step S4, the ruthenium salt is anhydrous ruthenium trichloride or aqueous ruthenium trichloride, and the ruthenium salt solution is a mixed solution of ethanol and water, with the ratio of ethanol to water being 2-3:2-1.

6. The preparation method according to claim 1, characterized in that: The concentration of the ruthenium salt is 0.05-0.08M / L.

7. The preparation method according to claim 1, characterized in that: The calcination temperature is 400-500° C., and the calcination time is 0.5-1 h.

8. A titanium dioxide nanotube-loaded ruthenium oxide particle anode material prepared by the preparation method according to any one of claims 1 to 7.

9. Use of the titanium dioxide nanotube-loaded ruthenium oxide particle anode material as claimed in claim 8 in electrolyzing salt water to prepare a sodium hypochlorite solution.

10. A use according to claim 9, characterized in that: The sodium hypochlorite solution was prepared by electrolyzing salt water at room temperature with a 6 mol / L sodium chloride solution as the electrolyte.