Surface modification preparation method based on medical magnesium alloy

Through the comprehensive methods of sandblasting, anodizing, hydrothermal immersion and electrochemical deposition, the problem of insufficient corrosion resistance of magnesium alloy is solved, the wear resistance and biocompatibility of the surface of magnesium alloy is improved, and stable oxidation is formed The film and nanoscale bimetallic hydroxide layer achieve effective protection of the surface of magnesium alloy.

CN118996574APending Publication Date: 2024-11-22ZHENGZHOU RAILWAY VOCATIONAL & TECH COLLEGE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410657729.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-26
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Magnesium alloy has poor corrosion resistance under the physiological environment of the human body. The existing micro-arc oxidized ceramic layer lacks binding force and is unstable when it is subjected to load, making it difficult to effectively protect the surface of magnesium alloy.

Method used

The combination of sandblasting pretreatment, anodization, hydrothermal immersion and electrochemical deposition methods is used to form a solid oxide film and a nano-scale bimetallic hydroxide layer to improve the corrosion resistance and binding force of the magnesium alloy surface.

Benefits of technology

It significantly improves the wear resistance and biocompatibility of the surface of magnesium alloy, reduces the risk of coating shedding, enhances the binding force with the matrix, and has simple material composition and low preparation cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996574A_ABST
    Figure CN118996574A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of coating preparation, in particular to a surface modification preparation method based on a medical magnesium alloy, which comprises the following steps: S1, pretreatment based on the surface of the medical magnesium alloy, S2, anodic oxidation based on the medical magnesium alloy, S3, surface cleaning based on the medical magnesium alloy, S4, hydrothermal soaking based on the medical magnesium alloy, and S5, surface modification based on the medical magnesium alloy. S5, an electrochemical deposition method is conducted on the basis of the medical magnesium alloy, 0.1%-1.0% of calcium (Ca), 0.1%-5.0% of zinc (Zn) and the balance magnesium (Mg) and inevitable impurities are included, and the content of the impurities does not exceed 0.01%; the hydrogel can be automatically absorbed and metabolized by a human body after completing the action, has very high biocompatibility, and has the advantages of simple material components and low preparation cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coating preparation, and in particular to a surface modification preparation method based on medical magnesium alloy. Background Art

[0002] In the field of medical materials, magnesium alloys are considered as a potential human implant material due to their abundant resources, low price, good biocompatibility and biodegradability. However, the use of magnesium alloys in clinical applications is limited, mainly due to their poor corrosion resistance in the human physiological environment. In the atmosphere or solution, a porous, thin and fragile film layer often forms on the surface of magnesium alloys. The density coefficient of this film layer is very low and it has almost no protective effect on the matrix, making the magnesium alloy susceptible to corrosion damage. Therefore, it is of great significance to develop a method to improve the corrosion resistance of magnesium alloys.

[0003] In the existing general magnesium alloy micro-arc oxidation process, on the one hand, the pre-treatment is generally grinding or pickling for degreasing and rust removal. There are obvious differences in strength and hardness between the micro-arc oxidation ceramic layer and the magnesium alloy surface. There is a large stress difference between the medical magnesium alloy and the micro-arc oxidation ceramic coating when bearing loads, which will significantly reduce the bonding force between the ceramic layer and the magnesium alloy surface, resulting in the ceramic coating being easy to peel off as a whole during use; on the other hand, since the micro-arc oxidation ceramic layer is mostly composed of MgO and components in the electrolyte, MgO is unstable and easily decomposed in the human body environment. At the same time, a single micro-arc oxidation ceramic layer is a porous material with limited protective effect on the magnesium alloy surface, resulting in relatively insufficient corrosion resistance of the single micro-arc oxidation ceramic coating and bonding force with the matrix magnesium alloy. Summary of the invention

[0004] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a surface modification preparation method based on medical magnesium alloy.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A surface modification preparation method based on medical magnesium alloy comprises the following steps: S1: pre-treating the surface of the medical magnesium alloy, S2: anodizing the medical magnesium alloy, S3: cleaning the surface of the medical magnesium alloy, S4: hydrothermal immersion of the medical magnesium alloy, and S5: electrochemical deposition of the medical magnesium alloy.

[0007] As a further description of the above technical solution:

[0008] The pre-treatment in step S1 is sandblasting, cleaning, and drying performed in sequence, and also includes cleaning and drying the medical magnesium alloy after the treatment in step S3 to obtain a completed surface coating.

[0009] As a further description of the above technical solution:

[0010] The anodic oxidation in S2 is specifically a method of generating oxides using electrochemical principles. Under specific electrolyte and voltage process conditions, a firmly bonded oxide film is formed on the surface of magnesium and magnesium alloys to improve their corrosion resistance.

[0011] As a further description of the above technical solution:

[0012] The surface cleaning in S3 specifically includes sandblasting, cleaning and drying the medical magnesium alloy twice.

[0013] As a further description of the above technical solution:

[0014] The hydrothermal soaking in S4 is specifically to hydrothermally treat the product obtained in step S1 in an alkaline solution containing an aluminum source and a zinc source, thereby constructing a nanoscale Mg-Zn-Al layered double metal hydroxide layer on the surface of the micron-scale magnesium oxide layer, and the magnesium alloy soaking passivation time is 10 to 60 minutes.

[0015] As a further description of the above technical solution:

[0016] The electrochemical deposition method in S5 is specifically to use electrochemical deposition method in 2+2+L, the molar concentration ratio of Ca and Zn is 1:2, the concentration of supporting electrolyte is 0.05-0.1 mol / L, the pH value is 4.0-6.0, and the base material is used as cathode, graphite or stainless steel is used as anode, immersed in the deposition solution, and electro-deposition is carried out under the conditions of temperature of 50-70°C and current density of 0.5-5mA / cm2.

[0017] The present invention has the following beneficial effects:

[0018] Before micro-arc oxidation of magnesium alloy, the surface of magnesium alloy is pretreated by sandblasting to coarsen the surface and improve the surface roughness. On the one hand, sandblasting will cause a large number of dislocations and slip bands on the surface, which is specifically manifested as a more complex surface structure after coarsening, which can be closely combined with the outer coating and significantly improve the coating bonding strength; on the other hand, sandblasting can introduce residual stress to the surface of magnesium alloy, which can offset part of the stress when the sample is under load, reduce the stress difference with the outer coating, improve the surface hardness and wear resistance, and prevent the outer coating from falling off as a whole. In addition, 0.1-1.0% calcium (Ca), 0.1-5.0% zinc (Zn), and the remainder magnesium (Mg) and unavoidable impurities, the impurity content of which does not exceed 0.01%; can be absorbed and metabolized by the human body after completing the effect, has high biocompatibility, and has the advantages of simple material composition and low preparation cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1This is a schematic diagram of the overall structure of a surface modification preparation method based on medical magnesium alloy proposed by the present invention; DETAILED DESCRIPTION

[0020] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings, which are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific position, be constructed and operated in a specific position, and therefore cannot be understood as limiting the present invention; the terms "first", "second", and "third" are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance. In addition, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be an indirect connection through an intermediate medium, or it can be a communication between the two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0022] Reference Figure 1 , an embodiment provided by the present invention:

[0023] A surface modification preparation method based on medical magnesium alloy comprises the following steps: S1: pre-treating the surface of the medical magnesium alloy, S2: anodizing the medical magnesium alloy, S3: cleaning the surface of the medical magnesium alloy, S4: hydrothermal immersion of the medical magnesium alloy, and S5: electrochemical deposition of the medical magnesium alloy.

[0024] Specifically, the pre-treatment in step S1 is sandblasting, cleaning, and drying performed in sequence, and also includes cleaning and drying the medical magnesium alloy after the treatment in step S3 to obtain a completed surface coating.

[0025] Specifically, the anodizing in S2 is a method of generating oxides using electrochemical principles, and under specific electrolyte and voltage process conditions, a firmly bonded oxide film is formed on the surface of magnesium and magnesium alloys to improve their corrosion resistance.

[0026] Specifically, the surface cleaning in S3 is to sandblast, clean and dry the medical magnesium alloy twice.

[0027] Specifically, the hydrothermal soaking in S4 is to hydrothermally treat the product obtained in step S1 in an alkaline solution containing an aluminum source and a zinc source, thereby constructing a nanoscale Mg-Zn-Al layered double metal hydroxide layer on the surface of the micron-scale magnesium oxide layer, and the magnesium alloy soaking passivation time is 10 to 60 minutes.

[0028] Specifically, the electrochemical deposition method in S5 is to use an electrochemical deposition method in 2+2+L, the molar concentration ratio of Ca and Zn is 1:2, the concentration of the supporting electrolyte is 0.05-0.1 mol / L, the pH value is 4.0-6.0, and the base material is used as the cathode, graphite or stainless steel is used as the anode, immersed in the deposition solution, and electro-deposition is carried out under the conditions of a temperature of 50-70°C and a current density of 0.5-5mA / cm2.

[0029] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A surface modification preparation method based on medical magnesium alloy, characterized in that: The following steps are involved: S1: Pretreatment of the surface of medical magnesium alloy, S2: Anodizing of medical magnesium alloy, S3: Surface cleaning of medical magnesium alloy, S4: Hydrothermal immersion of medical magnesium alloy, S5: Electrochemical deposition of medical magnesium alloy.

2. The surface modification preparation method based on medical magnesium alloy according to claim 1, characterized in that: The pre-treatment in step S1 is sandblasting, cleaning, and drying performed in sequence, and also includes cleaning and drying the medical magnesium alloy after the treatment in step S3 to obtain a completed surface coating.

3. The surface modification preparation method based on medical magnesium alloy according to claim 1, characterized in that: The anodic oxidation in S2 is specifically a method of generating oxides using electrochemical principles. Under specific electrolyte and voltage process conditions, a firmly bonded oxide film is formed on the surface of magnesium and magnesium alloys to improve their corrosion resistance.

4. The surface modification preparation method based on medical magnesium alloy according to claim 1, characterized in that: The surface cleaning in S3 specifically includes sandblasting, cleaning and drying the medical magnesium alloy twice.

5. The surface modification preparation method based on medical magnesium alloy according to claim 1, characterized in that: The hydrothermal soaking in S4 is specifically to hydrothermally treat the product obtained in step S1 in an alkaline solution containing an aluminum source and a zinc source, thereby constructing a nanoscale Mg-Zn-Al layered double metal hydroxide layer on the surface of the micron-scale magnesium oxide layer, and the magnesium alloy soaking passivation time is 10 to 60 minutes.

6. The surface modification preparation method based on medical magnesium alloy according to claim 1, characterized in that: The electrochemical deposition method in S5 is specifically to use electrochemical deposition method in 2+2+L, the molar concentration ratio of Ca and Zn is 1:2, the concentration of supporting electrolyte is 0.05-0.1 mol / L, the pH value is 4.0-6.0, and the base material is used as cathode, graphite or stainless steel is used as anode, immersed in the deposition solution, and electro-deposition is carried out under the conditions of temperature of 50-70°C and current density of 0.5-5mA / cm2.