Silver nanowire anti-freezing self-powered hydrogel flexible sensor and preparation method and application thereof
By introducing silver nanowires and dual network structures into the conductive hydrogel, combining hydrogen bonds of butene glycol to form anti-freeze properties, and attaching conductive copper sheets to the surface, the conductive hydrogel is solved by freezing at low temperatures and external power supply. The demand problem has achieved a flexible sensor that is self-powered at -40℃, improving the stability and environmental friendliness of the sensor.
Patent Information
- Application Number
- CN202411071383.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-06
AI Technical Summary
The freezing of existing conductive hydrogels at low temperatures leads to a reduced conductivity, and the sensor requires an external power supply, resulting in increased battery count and environmental pollution problems.
PVA/p (HEAA-co-BD) hydrogel with silver nanowires and dual network structures is used to form hydrogen bonds through the conductivity of silver nanowires and butene glycol to impart anti-freeze properties, and is pasted on the surface of the hydrogel. Conductive copper sheet forms a self-powered flexible sensor.
Good conductivity and sensing performance are maintained at -40°C, avoiding external power supply requirements and improving the stability and environmental friendliness of the sensor.
Smart Images

Figure CN118999631A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of flexible sensing and relates to a self-powered sensor, and in particular to a silver nanowire antifreeze self-powered hydrogel flexible sensor and a preparation method and application thereof. Background Art
[0002] Conductive hydrogel is a three-dimensional water-containing material with electrical conductivity. It has excellent stretchability, compressibility, flexibility and sensing properties, and has attracted extensive attention from researchers. However, most hydrogels are not conductive and require the addition of conductive substances to achieve their conductivity and sensing properties. In addition, because the water contained in the hydrogel freezes at low temperatures, the stretching and sensing properties of the conductive hydrogel at low temperatures are sharply reduced or lost.
[0003] Existing conductive fillers mainly include ionic conductive fillers and electronic conductive fillers. At low temperatures, the conductivity of ionic conductive fillers will drop sharply as the hydrogel freezes, while the conductivity of electronic conductive fillers is less affected than that of ionic conductive fillers at low temperatures. Silver nanowires (AgNWs), as a one-dimensional electronic conductive filler, have excellent electrical conductivity, thermal conductivity, resistance to oxidation and corrosion, and flexibility. At the same time, compared with other forms of silver nanomaterials, silver nanowires can greatly reduce the amount of silver used.
[0004] In addition, existing antifreeze conductive hydrogels are mainly made by introducing organic solvents such as ethylene glycol or glycerol, which form strong hydrogen bonds with water to destroy the formation of ice crystals at low temperatures, thereby giving conductive hydrogels antifreeze properties. However, the current types of organic antifreeze solvents are limited, which restricts the development of antifreeze hydrogels.
[0005] Flexible sensors based on conductive hydrogels detect skin physiological and motion signals in real time to improve health and prevention levels. Currently, conductive hydrogel flexible sensors need additional power to convert physiological and motion signals into electrical signals. As sensor networks become more multifunctional and complex, the number of batteries required increases dramatically, and power sources need to be replaced frequently, which poses new challenges to battery recycling and environmental protection.
[0006] Academician Wang Zhonglin's research group first invented a new self-driving technology, the friction nanogenerator (TENG), in 2012. It uses the triboelectric effect to convert mechanical energy into electrical energy, driving the conductive hydrogel flexible sensor without external power supply, thereby realizing the monitoring of human physiology and movement. In summary, how to provide an antifreeze, self-powered hydrogel flexible sensor without organic solvents is a technical problem that needs to be solved urgently by technicians in this field. Summary of the invention
[0007] In view of this, the present invention discloses a silver nanowire antifreeze self-powered hydrogel flexible sensor and a preparation method and application thereof.
[0008] It should be noted that the present invention introduces butenediol (BD) rich in hydroxyl groups, and the hydroxyl groups in butenediol BD form hydrogen bonds with water molecules in the hydrogel, giving the hydrogel anti-freezing properties, and the hydrogel sensor will not freeze at -40°C. At the same time, with polyvinyl alcohol (PVA) as the first network, N-hydroxyethyl acrylamide (HEAA) and butenediol (BD) copolymerized as the second network, the double network structure design gives the hydrogel good mechanical properties; and the addition of silver nanowires enables the hydrogel to maintain good conductivity and sensing properties at low temperatures.
[0009] Based on the hydrogel flexible sensor, the present invention designs and prepares a self-powered flexible sensor with a simple structure, which solves the limitation that the flexible sensor needs an external power supply.
[0010] In order to achieve the above object, the present invention adopts the following technical solution:
[0011] The first object of the present invention is to provide a silver nanowire antifreeze self-powered hydrogel flexible sensor, wherein the self-powered hydrogel flexible sensor is prepared by attaching a conductive copper sheet to one side of the hydrogel and then wrapping the hydrogel with silicone rubber; wherein,
[0012] The hydrogel is PVA / p(HEAA-co-BD) / AgNWs hydrogel.
[0013] The second object of the present invention is to provide a method for preparing the silver nanowire antifreeze self-powered hydrogel flexible sensor as described above, the method specifically comprising the following steps:
[0014] 1) Preparation of silver nanowires:
[0015] Slowly add the silver nitrate solution into the ethylene glycol solution containing polyvinyl pyrrolidone (PVP) and copper chloride, stir evenly, heat to react, centrifuge and wash to obtain silver nanowires (AgNWs);
[0016] 2) Preparation of PVA / p(HEAA-co-BD) / AgNWs hydrogel:
[0017] Dissolve N-hydroxyethyl acrylamide (HEAA), polyvinyl alcohol (PVA), butylene glycol (BD), N,N-methylene acrylamide, photoinitiator I2959, and the silver nanowires (AgNWs) prepared in step 1) in deionized water, and stir and mix to obtain a prepolymer solution;
[0018] The prepolymer solution was injected into a glass mold and irradiated with ultraviolet light to obtain a PVA / p(HEAA-co-BD) / AgNWs hydrogel;
[0019] 3) Preparation of PVA / p(HEAA-co-BD) / AgNWs hydrogel self-powered sensor:
[0020] The hydrogel obtained in step 2) is cut, a conductive copper sheet is attached to one side of the cut hydrogel, and the hydrogel is wrapped with silicone rubber to prepare a hydrogel self-powered sensor.
[0021] Optionally, in step 1), the mass ratio of silver nitrate (AgNO3), polyvinyl pyrrolidone (PVP) and cupric chloride dihydrate (CuCl2·2H2O) is 0.68:0.888:0.001364.
[0022] Furthermore, the reaction temperature in step 1) is 140° C. and the reaction time is 3 h.
[0023] Optionally, in step 2), the PVA / p(HEAA-co-BD) / AgNWs hydrogel is prepared from the following substances, calculated by mass percentage:
[0024] N-hydroxyethyl acrylamide (HEAA) 30%-50%, polyvinyl alcohol (PVA) 4%-8%, butene glycol (BD) 6%-10%, N,N-methylene acrylamide 0.1%-0.2%, photoinitiator (I2959) 1%-2%, silver nanowires (AgNWs) 0.2%-0.6%, deionized water 29.2%-58.7%.
[0025] Preferably, N-hydroxyethyl acrylamide (HEAA) 50%, polyvinyl alcohol (PVA) 8%, butene glycol (BD) 10%, N,N-methylene acrylamide 0.2%, photoinitiator (I2959) 1%, silver nanowires (AgNWs) 0.4%, and deionized water 30.4%.
[0026] It should be noted that under ultraviolet light irradiation, the photoinitiator triggers the monomer to undergo free radical polymerization to form a hydrogel. This preparation method adopts a one-pot operation and has the characteristics of simple operation.
[0027] Optionally, in step 2), the stirring temperature of the prepolymer liquid is 80° C.-95° C., the stirring time is 30 min-60 min, and the stirring rate is 400-700 rpm.
[0028] Optionally, in step 2), the ultraviolet light irradiation wavelength is 365 nm and the irradiation time is 2-5 h.
[0029] Preferably, the thickness of the glass mold is in the range of 1 mm to 2 mm, and a layer of PET film is provided between the contact surface of the glass mold and the prepolymerized liquid.
[0030] Optionally, in step 3), the hydrogel is cut into a size of 20 mm×30 mm.
[0031] The third object of the present invention is to provide an application of a silver nanowire antifreeze self-powered hydrogel flexible sensor in the field of flexible wearable equipment.
[0032] Furthermore, the silver nanowire antifreeze self-powered hydrogel flexible sensor is used for physiological, sports and health monitoring.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] (1) The conductive hydrogel disclosed in the present invention adopts a double network structure design, with polyvinyl alcohol (PVA) as the first network and N-hydroxyethyl acrylamide (HEAA) and butene glycol (BD) copolymerized as the second network. The double network structure design gives the hydrogel good mechanical properties.
[0035] (2) The friction layer disclosed in the present invention completely covers the electrode layer to prevent the electrode layer from being exposed and worn, thereby ensuring the long-term working stability of the antifreeze self-powered hydrogel sensor.
[0036] (3) The electrode layer of the hydrogel sensor disclosed in the present invention is composed of PVA / p(HEAA-co-BD) / AgNWs hydrogel. The hydrogel is copolymerized with N-hydroxyethyl acrylamide by the introduction of butene glycol (BD). The hydroxyl groups in BD form hydrogen bonds with the water molecules in the hydrogel, giving the hydrogel freezing properties. The hydrogel sensor will not freeze at -40°C.
[0037] (4) The silver nanowires (AgNWs) synthesized by the present invention have a high aspect ratio, and the use of a small amount of high aspect ratio silver nanowires can still give the hydrogel good conductivity and sensing properties. And the silver nanowires, as conductive fillers, can still play a conductive role at low temperatures, thereby overcoming the technical defect that ion conductive hydrogels are easily frozen at low temperatures and lose their conductive ability.
[0038] (5) The electrode layer of the hydrogel sensor disclosed in the present invention transmits electrical energy into the circuit through the conductive copper sheet, thereby improving the charge collection capability of the antifreeze hydrogel flexible sensor. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0040] Figure 1It is a structural schematic diagram of the self-powered flexible sensor of the present invention.
[0041] Figure 2 This is a schematic diagram of the power generation principle of the self-powered flexible sensor of the present invention.
[0042] Figure 3 This is a physical picture of the self-powered flexible sensor of the present invention.
[0043] Figure 4 This is the SEM image of silver nanowires in Example 1 of the present invention.
[0044] Figure 5 This is a test diagram of the tensile properties of PVA / p(HEAA-co-BD) / AgNWs hydrogel at room temperature in Example 1 of the present invention.
[0045] Figure 6 This is a test graph of the tensile properties of PVA / p(HEAA-co-BD) / AgNWs hydrogel at -40°C in Example 1 of the present invention.
[0046] Figure 7 Schematic diagram of voltage output of the self-powered flexible sensor according to Example 1 of the present invention.
[0047] Figure 8 This is a schematic diagram of the current output of the self-powered flexible sensor according to Example 1 of the present invention.
[0048] Fig. 9 Schematic diagram of charge output of the self-powered flexible sensor according to Example 1 of the present invention.
[0049] Fig.10 This is a durability test of the self-powered flexible sensor of Example 1 of the present invention for 2000 cycles.
[0050] Fig.11 This is a schematic diagram of the voltage output of the self-powered flexible sensor for monitoring knee bending at room temperature according to Example 4 of the present invention.
[0051] Fig.12 This is a schematic diagram of the voltage output of the self-powered flexible sensor for monitoring finger bending at -40°C in Example 5 of the present invention.
[0052] Fig.13 45 small light bulbs are lit for the self-powered flexible sensor of Example 1 of the present invention.
[0053] In the figure, 1 is the friction layer (silicone rubber (-Ecoflex)), 2 is the electrode layer (PVA / p(HEAA-co-BD) / AgNWs hydrogel), 3 is the base layer (polyurethane (PU)), 4 is the copper sheet, 5 is the negative charge, and 6 is the positive charge. DETAILED DESCRIPTION
[0054] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0055] The word "embodiment" used here as an "exemplary" does not necessarily mean that any embodiment described is superior to or better than other embodiments. Unless otherwise specified, the performance index tests in the embodiments of this application are performed using conventional test methods in the art. It should be understood that the terms described in this application are only used to describe specific implementation methods and are not used to limit the content disclosed in this application.
[0056] Unless otherwise specified, the technical and scientific terms used in this document have the same meanings as commonly understood by ordinary technicians in the technical field to which this application belongs; other experimental methods and technical means not specifically specified in this application refer to experimental methods and technical means commonly used by ordinary technicians in this field.
[0057] In the description of the present invention, it is necessary to understand that the terms "middle", "upper", "lower", "ascending", "descending", "vertical", "face", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0058] In order to better illustrate the content of the present application, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that the present application can also be implemented without certain specific details. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail in order to highlight the main purpose of the present application.
[0059] Under the premise of no conflict, the technical features disclosed in the embodiments of the present application can be combined arbitrarily, and the resulting technical solutions belong to the contents disclosed in the embodiments of the present application.
[0060] The invention discloses a silver nanowire antifreeze self-powered hydrogel flexible sensor and a preparation method thereof.
[0061] Figure 1 1 is the friction layer, 2 is the electrode layer. The electrode layer 2 is composed of PVA / p(HEAA-co-BD) / AgNWs hydrogel, wherein PVA is polyvinyl alcohol, HEAA is N-hydroxyethyl acrylamide, BD is butene glycol, and AgNWs is silver nanowires.
[0062] Figure 2 Schematic diagram of power generation for the self-powered flexible sensor.
[0063] Step ①: When the friction layer 1 contacts the base layer 3, due to the different electron acquisition abilities of the two materials in the friction electrification phenomenon, equal amounts of opposite charges are generated at the interface.
[0064] Step ②: Under the action of external force, the friction layer 1 and the base layer 3 are gradually separated, and free electrons migrate from the ground to the hydrogel electrode 2, forming a potential difference between the electrode and the ground.
[0065] Step ③: When the distance between the friction layer 1 and the base layer 3 is large, the open circuit voltage reaches saturation.
[0066] Step ④: Under the action of external force, the friction layer 1 and the base layer 3 materials gradually come into contact from a separated state, and free electrons migrate from the hydrogel electrode 2 to the ground, forming an electric potential difference between the electrode and the ground, and this cycle is repeated to form an AC voltage.
[0067] The electrode layer 2 is composed of PVA / p(HEAA-co-BD) / AgNWs hydrogel. The hydrogel is copolymerized with N-hydroxyethyl acrylamide by the introduction of butene glycol (BD). The hydroxyl groups in BD form hydrogen bonds with the water molecules in the hydrogel, giving the hydrogel freezing properties. The hydrogel sensor will not freeze at -40°C. The silver nanowires (AgNWs) in the hydrogel are used as conductive fillers and can still play a conductive role at low temperatures. However, ion-conductive hydrogels are easy to freeze at low temperatures and lose their conductivity.
[0068] In order to better understand the present invention, the present invention is further specifically described below through the following examples, but it should not be understood as a limitation of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above invention content are also considered to fall within the protection scope of the present invention.
[0069] Example 1
[0070] 1) The method for preparing silver nanowires comprises the following steps:
[0071] 0.888 g of polyvinyl pyrrolidone (PVP) was weighed and dissolved in 40 mL of ethylene glycol solution, and stirred at 90°C to prepare S1 solution; 0.0341 g of CuCl2·2H2O was weighed and dissolved in ethylene glycol solution to prepare 50 mL of S2 solution; 2 mL of S2 solution was weighed and dissolved in S1 solution to prepare S3 solution; 0.68 g of silver nitrate was weighed and dissolved in 40 mL of ethylene glycol solution, and stirred at room temperature to prepare S4 solution; S4 solution was slowly added to S3 solution, and stirred evenly at room temperature to obtain S5 solution; S5 solution was transferred to a 100 mL reactor, placed in an oven at 140°C for reaction for 3 hours, then taken out and centrifuged, and washed with ethanol and centrifuged 3 times, and washed with deionized water and centrifuged 2 times to obtain silver nanowires (AgNWs).
[0072] 2) Preparation of PVA / p(HEAA-co-BD) / AgNWs hydrogel:
[0073] N-Hydroxyethylacrylamide (2.5 g, 50 wt%), polyvinyl alcohol (0.4 g, 8 wt%), butene glycol (0.5 g, 10 wt%), N,N-methyleneacrylamide (0.01 g, 0.2%), photoinitiator I2959 (0.05 g, 1 wt%), and silver nanowires (0.02 g, 0.4 wt%) were dissolved in deionized water (1.52 g, 30.4 wt%), and stirred at 95 °C and 700 rpm for 30 min to obtain S6 solution; the S6 solution was transferred to a 1 mm thick glass template and irradiated with 365 nm ultraviolet light for 3 h to obtain PVA / p(HEAA-co-BD) / AgNWs hydrogel S7.
[0074] 3) Preparation of PVA / p(HEAA-co-BD) / AgNWs hydrogel self-powered sensor:
[0075] The hydrogel S7 was cut into a size of 20 mm × 30 mm, a conductive copper sheet was attached to one side of the hydrogel S7, and the hydrogel S7 was wrapped with silicone rubber to prepare a hydrogel self-powered sensor S8;
[0076] The prepared hydrogel self-powered sensor S8 is friction-powered with polyurethane (PU), the wire of the hydrogel self-powered sensor S8 is connected to an external circuit, the other end of the external circuit is grounded, and the output performance of the prepared hydrogel self-powered sensor is further tested.
[0077] Example 2
[0078] 1) Preparation method of silver nanowires: refer to Example 1.
[0079] 2) Preparation of PVA / p(HEAA-co-BD) / AgNWs hydrogel:
[0080] N-Hydroxyethylacrylamide (1.5 g, 30 wt %), polyvinyl alcohol (0.2 g, 4 wt %), butene glycol (0.3 g, 6 wt %), N,N-methyleneacrylamide (0.005 g, 0.1 wt %), photoinitiator I2959 (0.05 g, 1 wt %), and silver nanowires (0.01 g, 0.2 wt %) were dissolved in deionized water (2.935 g, 58.7 wt %), and stirred at 80 ° C and 400 rpm for 30 min to obtain S6 solution; the S6 solution was transferred to a 2 mm thick glass template and irradiated with 365 nm ultraviolet light for 2 h to obtain PVA / p(HEAA-co-BD) / AgNWs hydrogel S7.
[0081] 3) Preparation method of PVA / p(HEAA-co-BD) / AgNWs hydrogel self-powered sensor: refer to Example 1.
[0082] Example 3
[0083] 1) Preparation method of silver nanoparticles: refer to Example 1.
[0084] 2) Preparation of PVA / p(HEAA-co-BD) / AgNWs hydrogel:
[0085] N-Hydroxyethylacrylamide (2.5 g, 50 wt%), polyvinyl alcohol (0.4 g, 8 wt%), butene glycol (0.5 g, 10 wt%), N,N-methyleneacrylamide (0.01 g, 0.2%), photoinitiator I2959 (0.05 g, 1 wt%), and silver nanowires (0.03 g, 0.6 wt%) were dissolved in deionized water (1.51 g, 30.2 wt%), and stirred at 95 °C and 700 rpm for 60 min to obtain S6 solution; the S6 solution was transferred to a 1 mm thick glass template and irradiated with 365 nm ultraviolet light for 5 h to obtain PVA / p(HEAA-co-BD) / AgNWs hydrogel S7.
[0086] 3) Preparation method of PVA / p(HEAA-co-BD) / AgNWs hydrogel self-powered sensor: refer to Example 1.
[0087] Example 4
[0088] The difference from Example 1 is that the hydrogel self-powered sensor S8 is friction-powered by fitting it against the skin, and is self-powered to monitor human body movements.
[0089] Example 5
[0090] The difference from Example 1 is that the hydrogel self-powered sensor S8 is friction-powered by fitting it against the skin, and can monitor human body movements at -40°C with self-power.
[0091] The present invention adopts a polyol method to synthesize high aspect ratio silver nanowires, then dissolves N-hydroxyethyl acrylamide, polyvinyl alcohol, butylene glycol, N,N-methylene acrylamide, a photoinitiator, and silver nanowires in deionized water, mixes them according to a certain proportion, and prepares an antifreeze hydrogel through photopolymerization. Based on the antifreeze hydrogel, an antifreeze self-powered hydrogel flexible sensor is prepared.
[0092] The results of the examples show that the silver nanowires prepared by the present invention based on the optimized components of the polyol method have a high aspect ratio. Figure 4 The silver nanowires have a diameter of 50 nm, a length of 17 μm, and an aspect ratio of 340. The antifreeze hydrogel synthesized by the present invention has excellent tensile properties and good flexibility, and still has good tensile properties and flexibility at -40°C. Figure 5 The results show that the prepared hydrogel has a tensile stress of 1.42MPa and a tensile strain of 783% at room temperature. Figure 6 The prepared hydrogel showed that the tensile stress was 2.67 MPa and the tensile strain was 559% at -40°C. Figure 7 The open circuit voltage (Voc) of the silver nanowire antifreeze self-powered hydrogel flexible sensor prepared based on the hydrogel can reach 170V, and after 2000 cycles ( Fig.10 ) still maintains the initial open-circuit voltage, indicating good stability. Fig.11 The silver nanowire antifreeze self-powered hydrogel flexible sensor at room temperature does not require an external power supply and can monitor human motion, and at -40°C ( Fig.12 ) is still able to self-power and monitor human motion. Fig.13 The silver nanowire antifreeze self-powered hydrogel flexible sensor was shown to light up 45 small bulbs through self-powered energy.
[0093] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A silver nanowire antifreeze self-powered hydrogel flexible sensor, characterized in that: The self-powered hydrogel flexible sensor is prepared by attaching a conductive copper sheet to one side of the hydrogel and then wrapping the hydrogel with silicone rubber; wherein, The hydrogel is PVA / p(HEAA-co-BD) / AgNWs hydrogel.
2. A method for preparing the silver nanowire antifreeze self-powered hydrogel flexible sensor as claimed in claim 1, characterized in that: The method specifically comprises the following steps: 1) Preparation of silver nanowires: Slowly add the silver nitrate solution into the ethylene glycol solution containing polyvinyl pyrrolidone (PVP) and copper chloride, stir evenly, heat to react, centrifuge and wash to obtain silver nanowires (AgNWs); 2) Preparation of PVA / p(HEAA-co-BD) / AgNWs hydrogel: Dissolve N-hydroxyethyl acrylamide (HEAA), polyvinyl alcohol (PVA), butylene glycol (BD), N,N-methylene acrylamide, photoinitiator I2959, and the silver nanowires (AgNWs) prepared in step 1) in deionized water, and stir and mix to obtain a prepolymer solution; The prepolymer solution was injected into a glass mold and irradiated with ultraviolet light to obtain a PVA / p(HEAA-co-BD) / AgNWs hydrogel; 3) Preparation of PVA / p(HEAA-co-BD) / AgNWs hydrogel self-powered sensor: The hydrogel obtained in step 2) is cut, a conductive copper sheet is attached to one side of the cut hydrogel, and the hydrogel is wrapped with silicone rubber to prepare a hydrogel self-powered sensor.
3. The method for preparing the silver nanowire antifreeze self-powered hydrogel flexible sensor according to claim 2, characterized in that: In the step 1), the mass ratio of silver nitrate (AgNO3), polyvinyl pyrrolidone (PVP) and cupric chloride dihydrate (CuCl2·2H2O) is 0.68:0.888:0.001364.
4. The method for preparing the silver nanowire antifreeze self-powered hydrogel flexible sensor according to claim 2 or 3, characterized in that: The reaction temperature in step 1) is 140° C. and the reaction time is 3 h.
5. The method for preparing the silver nanowire antifreeze self-powered hydrogel flexible sensor according to claim 2, characterized in that: In the step 2), the PVA / p(HEAA-co-BD) / AgNWs hydrogel is prepared from the following substances, calculated by mass percentage: N-hydroxyethyl acrylamide (HEAA) 30%-50%, polyvinyl alcohol (PVA) 4%-8%, butene glycol (BD) 6%-10%, N,N-methylene acrylamide 0.1%-0.2%, photoinitiator (I2959) 1%-2%, silver nanowires (AgNWs) 0.2%-0.6%, deionized water 29.2%-58.7%.
6. The method for preparing the silver nanowire antifreeze self-powered hydrogel flexible sensor according to claim 2 or 5, characterized in that: In the step 2), the stirring temperature of the prepolymer liquid is 80° C.-95° C., the stirring time is 30 min-60 min, and the stirring speed is 400-700 rpm.
7. The method for preparing the silver nanowire antifreeze self-powered hydrogel flexible sensor according to claim 2, characterized in that: In the step 2), the wavelength of ultraviolet light irradiation is 365 nm, and the irradiation time is 2-5 h.
8. The method for preparing the silver nanowire antifreeze self-powered hydrogel flexible sensor according to claim 2, characterized in that: In the step 3), the hydrogel is cut into a size of 20 mm×30 mm.
9. An application of the silver nanowire antifreeze self-powered hydrogel flexible sensor as claimed in claim 1 or the silver nanowire antifreeze self-powered hydrogel flexible sensor prepared by the method as claimed in claim 2 in the field of flexible wearable equipment.
Citation Information
Patent Citations
Controllable preparation method of silver nanowires of different length-diameter ratios and preparation method of flexible transparent electrode
CN107146821A
Preparation method and application of dual-network flexible conductive adhesive anti-freezing hydrogel
CN112795029A
Anti-freezing conductive hydrogel as well as preparation method, and application of anti-freezing conductive hydrogel in force response sensing
CN113527714A
Hydrogel flexible sensor and preparation method thereof
CN115251900A
Sodium alginate hydrogel electrode and preparation method and application thereof
CN118252505A
Cited By
Hydrogel-based super-tensile flexible multifunctional input device and preparation and application thereof
CN119798515A
A hydrogel-based ultrastretchable flexible multifunctional input device and preparation and application thereof
CN119798515B
Method for forming gel flow channel on bipolar plate in situ, bipolar plate with gel flow channel, gel solution and flow battery
CN121565884A
Method of forming gel flow channels in situ on bipolar plates, bipolar plates having gel flow channels, gel solutions, flow batteries
CN121565884B