Superconducting wire critical current test sample preparation method and sample

Through deep hole drilling, oxygen-free copper pipes are made, the oxide layer is removed and the thermal pulling treatment is heat-dissipated, which solves the heat dissipation problem of copper-nickel-based multi-core niobium-titanium superconducting wires in critical current testing, and improves the test Accuracy and performance acquisition significantly improve the accuracy of test results.

CN119000216APending Publication Date: 2024-11-22XIAN SUPERCONDUCTING WIRE TECHNOLOGIES CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411179515.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Conventional sample preparation methods in the prior art result in abnormally overshooting of copper-nickel-based multi-core niobium-titanium superconducting wires during critical current testing due to heat dissipation problems, which reduces the accuracy of the test and cannot accurately obtain the performance of superconducting wires, affecting production and delivery. .

Method used

Anaerobic copper rod made of deep hole drilling is made of copper-nickel-based multi-core niobium-titanium superconducting wire, and the oxide layer is removed by pickling, and the oxygen-free copper pipe is heat-pulled to treat it to tightly fit the copper. Nickel-based multi-core niobium titanium superconducting wires form a heat dissipation structure to improve testing accuracy.

Benefits of technology

Through the thermal pulling process and the heat dissipation structure covered by oxygen-free copper tubes, the heat dissipation problem of copper-nickel-based multi-core niobium-titanium superconducting wire in critical current testing is solved, ensuring the accuracy and performance of the test, and significantly improving the The accuracy of the test results.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119000216A_ABST
    Figure CN119000216A_ABST
Patent Text Reader

Abstract

The invention discloses a superconducting wire critical current test sample preparation method and a sample. The method comprises the following steps: drilling a through hole in an oxygen-free copper bar through a deep hole drill to obtain an oxygen-free copper pipe; cleaning an oxide layer on the surface of the copper-nickel-based multi-core niobium-titanium superconducting wire and in the oxygen-free copper pipe through acid pickling; the copper-nickel-based multi-core niobium-titanium superconducting wire subjected to acid pickling is put into the through hole of the oxygen-free copper pipe subjected to acid pickling; and carrying out hot drawing treatment on the oxygen-free copper pipe on which the copper-nickel-based multi-core niobium-titanium superconducting wire is placed to obtain a critical current test sample. The heat dissipation problem during the critical current test of the copper-nickel-based multi-core niobium-titanium superconducting wire is solved through the hot drawing process and the oxygen-free copper pipe coated heat dissipation structure. And the accuracy of the critical current test of the copper-nickel-based multi-core niobium-titanium superconducting wire is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of superconducting wires, and in particular to a method for preparing a sample for testing critical current of a superconducting wire and a sample. Background Art

[0002] Since copper-nickel alloy has higher wire resistance than pure copper, superconducting wires using copper-nickel alloy as the matrix have shown great advantages over traditional copper-based superconducting wires in the field of superconducting switch wires and are widely used in continuous current switches (PCS). With the continuous development of nuclear magnetic resonance imaging equipment and superconducting energy storage equipment, the demand for copper-nickel-based superconducting switch wires is also increasing. However, the essential reason for its high resistance lies in the addition of nickel elements in copper metal. The increase in nickel content will cause the heat dissipation capacity of copper-nickel alloy to decrease rapidly. Therefore, when conducting critical current tests on copper-nickel-based multi-core niobium-titanium superconducting wires, if conventional sample preparation methods are used, the heat dissipation problem often causes the superconducting wire to abnormally lose superconductivity, greatly reducing the accuracy of the test. At the same time, the inability to accurately obtain the performance of superconducting wires will also hinder the subsequent optimization research of R&D personnel, seriously affecting the production and delivery of superconducting wires. Summary of the invention

[0003] The embodiment of the present invention provides a superconducting wire critical current test sample preparation method, which is used to solve the problem that the conventional sample preparation method in the prior art may cause abnormal quenching of the superconducting wire due to its heat dissipation problem, and the test accuracy is low, and the performance of the superconducting wire cannot be accurately obtained.

[0004] On the one hand, an embodiment of the present invention provides a method for preparing a sample for testing critical current of a superconducting wire, comprising: The oxygen-free copper rod is drilled with a through hole by a deep hole drill to obtain an oxygen-free copper tube; Cleaning the oxide layer on the surface of the copper-nickel-based multi-core niobium-titanium superconducting wire and the inside of the oxygen-free copper tube by pickling; Putting the pickled copper-nickel-based multi-core niobium-titanium superconducting wire into the through hole of the pickled oxygen-free copper tube; The oxygen-free copper tube in which the copper-nickel-based multi-core niobium-titanium superconducting wire is placed is subjected to a hot drawing process to obtain a critical current test sample.

[0005] In one possible implementation, the outer diameter of the oxygen-free copper tube is between 7 and 10 times that of the copper-nickel-based multi-core niobium-titanium superconducting wire, and the through-hole diameter of the oxygen-free copper tube is between 1.1 and 1.2 times the outer diameter of the copper-nickel-based multi-core niobium-titanium superconducting wire.

[0006] In a possible implementation, the pickling solution for pickling the oxygen-free copper pipe is a sulfuric acid solution with a concentration of 4-7 mol / L, and the corrosion time is 1-5 min.

[0007] In a possible implementation, the pickling solution for pickling the copper-nickel-based multi-core niobium-titanium superconducting wire is a sulfuric acid solution with a concentration of 6 to 9 mol / L, and the corrosion time is 2 to 7 minutes.

[0008] In a possible implementation, the critical current test sample is obtained by hot drawing the oxygen-free copper tube in which the copper-nickel-based multi-core niobium-titanium superconducting wire is placed. The oxygen-free copper tube is heated during the drawing process at a temperature of 350-450°C. After heating, the hardness of the oxygen-free copper tube should be between 50-70Hv. The processing rate of the drawing process is 5%-10%. After the hot drawing, the inner wall of the oxygen-free copper tube is tightly attached to the surface of the copper-nickel-based multi-core niobium-titanium superconducting wire.

[0009] In a possible implementation, after the critical current test sample is obtained by hot drawing the oxygen-free copper tube in which the copper-nickel-based multi-core niobium-titanium superconducting wire is placed, the method further comprises: The oxygen-free copper tubes at both ends of the copper-nickel-based multi-core niobium-titanium superconducting wire are removed, so that the two end faces of the copper-nickel-based multi-core niobium-titanium superconducting wire are exposed at both ends of the oxygen-free copper tube.

[0010] On the other hand, an embodiment of the present invention provides a superconducting wire critical current test sample, comprising: An oxygen-free copper tube and a copper-nickel-based multi-core niobium-titanium superconducting wire, wherein the copper-nickel-based multi-core niobium-titanium superconducting wire is arranged inside the oxygen-free copper tube, the oxygen-free copper tube is tightly attached to the outer surface of the copper-nickel-based multi-core niobium-titanium superconducting wire, and the two ends of the copper-nickel-based multi-core niobium-titanium superconducting wire extend out of the two ends of the oxygen-free copper tube.

[0011] The superconducting wire critical current test sample preparation method and sample in the present invention have the following advantages: The heat dissipation problem of the copper-nickel-based multi-core niobium-titanium superconducting wire during the critical current test is solved through the hot drawing process and the oxygen-free copper tube-coated heat dissipation structure, which ensures the accuracy of the critical current test of the copper-nickel-based multi-core niobium-titanium superconducting wire. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0013] Figure 1A schematic diagram of combining an oxygen-free copper tube with a copper-nickel-based multi-core niobium-titanium superconducting wire in a method for preparing a sample for a superconducting wire critical current test provided by an embodiment of the present invention; Figure 2 A schematic diagram of the thermal drawing effect of a superconducting wire critical current test sample preparation method provided by an embodiment of the present invention; Figure 3 A critical current test diagram of Example 1 of a superconducting wire critical current test sample preparation method provided by an embodiment of the present invention; Figure 4 A critical current test diagram of Example 2 of a superconducting wire critical current test sample preparation method provided by an embodiment of the present invention; Figure 5 A critical current test diagram of Example 3 of a superconducting wire critical current test sample preparation method provided by an embodiment of the present invention; Figure 6 Critical current test diagram of Example 4 of a superconducting wire critical current test sample preparation method provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0014] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0015] Figure 1 A schematic diagram of combining an oxygen-free copper tube and a copper-nickel-based multi-core niobium-titanium superconducting wire in a method for preparing a sample for a superconducting wire critical current test provided by an embodiment of the present invention; an embodiment of the present invention provides a method for preparing a sample for a superconducting wire critical current test, comprising: Drilling a through hole through the oxygen-free copper rod by deep hole drilling to obtain an oxygen-free copper tube 1; Cleaning the oxide layer on the surface of the copper-nickel-based multi-core niobium-titanium superconducting wire 2 and the inside of the oxygen-free copper tube 1 by pickling; Putting the pickled copper-nickel-based multi-core niobium-titanium superconducting wire 2 into the through hole of the pickled oxygen-free copper tube 1; The oxygen-free copper tube 1 in which the copper-nickel-based multi-core niobium-titanium superconducting wire 2 is placed is subjected to a hot drawing process to obtain a critical current test sample.

[0016] For example, first, a through hole is drilled out of an oxygen-free copper rod using a deep hole drilling technique to obtain an oxygen-free copper tube 1, and the prepared copper-nickel-based multi-core niobium-titanium superconducting wire 2 and the oxygen-free copper tube 1 are pickled to remove the surface and internal oxide layer and increase the roughness, so as to enhance the interface contact state between the copper-nickel-based multi-core niobium-titanium superconducting wire 2 and the oxygen-free copper tube 1, and then, as Figure 1 As shown, the copper-nickel-based multi-core niobium-titanium superconducting wire 2 is inserted into the interior of the oxygen-free copper tube 1, and as shown in Figure 2 As shown, the outer oxygen-free copper tube 1 is stretched by a hot drawing process to shrink the inner hole and fit tightly with the inner copper-nickel-based multi-core niobium-titanium superconducting wire 2, so that the copper-nickel-based multi-core niobium-titanium superconducting wire 2 sample for testing the critical current can be obtained, and then the conventional superconducting wire critical current test method can be used to test it. Relying on the oxygen-free copper tube 1 that fits tightly with the outer layer of the copper-nickel-based multi-core niobium-titanium superconducting wire 2, the heat dissipation capacity of the copper-nickel-based multi-core niobium-titanium superconducting wire 2 during the critical current test can be effectively improved, and the superconducting wire 2 can be prevented from quenching in advance during the test, thereby ensuring the accuracy of the test results, which is suitable for the critical current test of superconducting wires. The oxygen-free copper tube 1 is subjected to an empty drawing experiment before hot drawing and the change of its inner hole is tested after stretching. After adjusting the appropriate processing rate, the superconducting wire can be assembled and stretched. After stretching, it is ensured to fit just right and the copper-nickel-based multi-core niobium-titanium superconducting wire 2 is not deformed.

[0017] In a possible embodiment, the outer diameter of the oxygen-free copper tube 1 is one of 7 times to 10 times that of the copper-nickel-based multi-core niobium-titanium superconducting wire 2, the through-hole diameter of the oxygen-free copper tube 1 is one of 1.1 times to 1.2 times the outer diameter of the copper-nickel-based multi-core niobium-titanium superconducting wire 2, the pickling solution for pickling the oxygen-free copper tube 1 is a sulfuric acid solution with a concentration of 4 to 7 mol / L, and the corrosion time is 1 to 5 minutes, and the pickling solution for pickling the copper-nickel-based multi-core niobium-titanium superconducting wire 2 is a sulfuric acid solution with a concentration of 6 to 9 mol / L, and the corrosion time is 2 to 7 minutes. The critical current test sample obtained by the hot drawing treatment of the oxygen-free copper tube 1 on which the copper-nickel-based multi-core niobium-titanium superconducting wire 2 is placed is that the oxygen-free copper tube 1 is heated during the drawing process, and the temperature is 350-450° C. After heating, the hardness of the oxygen-free copper tube 1 should be between 50-70 Hv, and the processing rate of the drawing process is 5%-10%. After the oxygen-free copper tube 1 is subjected to the hot drawing, the inner wall of the oxygen-free copper tube 1 is closely attached to the surface of the copper-nickel-based multi-core niobium-titanium superconducting wire 2. After the critical current test sample is obtained by the hot drawing treatment of the oxygen-free copper tube 1 on which the copper-nickel-based multi-core niobium-titanium superconducting wire 2 is placed, the following further includes: The oxygen-free copper tubes 1 at both ends of the copper-nickel-based multi-core niobium-titanium superconducting wire 2 are removed, so that the two end faces of the copper-nickel-based multi-core niobium-titanium superconducting wire 2 are exposed at both ends of the oxygen-free copper tube 1 .

[0018] Exemplarily, this application is verified by four groups of experiments as follows: In Example 1, a copper-nickel-based multi-core niobium-titanium superconducting wire 2 with an outer diameter of 0.5 mm is selected, the outer diameter of the oxygen-free copper tube 1 is 7 times that of the copper-nickel-based multi-core niobium-titanium superconducting wire 2, i.e., 3.5 mm, and the through-hole diameter is 1.1 times that of the copper-nickel-based multi-core niobium-titanium superconducting wire 2, i.e., 0.55 mm. The pickling solution of the oxygen-free copper tube 1 is a sulfuric acid solution with a concentration of 4 mol / L, and the corrosion time is 1 min. The pickling solution of the copper-nickel-based multi-core niobium-titanium superconducting wire 2 is a sulfuric acid solution with a concentration of 6 mol / L, and the corrosion time is 2 min. The niobium-titanium superconducting wire 2 did not scratch the inner wall of the copper tube when penetrating into the oxygen-free copper tube 1, and the copper-nickel-based multi-core niobium-titanium superconducting wire 2 did not show defects such as bending and folding. The oxygen-free copper tube 1 was heated at 350°C during the drawing process. After heating, the hardness of the oxygen-free copper tube 1 should be 70Hv. The processing rate of the drawing process was 5%. After drawing, it was determined by observation that the wire cross-section was closely fitted to the inner wall of the copper tube, and the wire cross-section did not change. The sample obtained after drawing was tested in a conventional critical current test experiment at 4.2K. The results are as follows: Figure 3 shown.

[0019] Example 2, a copper-nickel-based multi-core niobium-titanium superconducting wire 2 with an outer diameter of 0.5 mm is selected, the outer diameter of the oxygen-free copper tube 1 is 8 times that of the copper-nickel-based multi-core niobium-titanium superconducting wire 2, i.e., 4 mm, the through-hole diameter is 1015 times that of the copper-nickel-based multi-core niobium-titanium superconducting wire 2, i.e., 0.575 mm, the pickling solution of the oxygen-free copper tube 1 is a sulfuric acid solution with a concentration of 5 mol / L, and the corrosion time is 2 min, the pickling solution of the copper-nickel-based multi-core niobium-titanium superconducting wire 2 is a sulfuric acid solution with a concentration of 7 mol / L, and the corrosion time is 3 min, and the copper-nickel-based multi-core niobium-titanium superconducting wire 2 is a ... The niobium-titanium superconducting wire 2 did not scratch the inner wall of the copper tube when penetrating into the oxygen-free copper tube 1, and the copper-nickel-based multi-core niobium-titanium superconducting wire 2 did not show defects such as bending and folding. The oxygen-free copper tube 1 was heated at 400°C during the drawing process. After heating, the hardness of the oxygen-free copper tube 1 should be 60Hv. The processing rate of the drawing process was 7%. After drawing, it was determined by observation that the wire cross-section was closely fitted to the inner wall of the copper tube, and the wire cross-section did not change. The sample obtained after drawing was tested in a conventional critical current test experiment at 4.2K. The results are as follows Figure 4 shown.

[0020] Example 3, a copper-nickel-based multi-core niobium-titanium superconducting wire 2 with an outer diameter of 0.6 mm is selected, the outer diameter of the oxygen-free copper tube 1 is 10 times that of the copper-nickel-based multi-core niobium-titanium superconducting wire 2, that is, 5.4 mm, and the through-hole diameter is 1.2 times that of the copper-nickel-based multi-core niobium-titanium superconducting wire 2, that is, 0.72 mm. The pickling solution of the oxygen-free copper tube 1 is a sulfuric acid solution with a concentration of 7 mol / L, and the corrosion time is 5 min. The pickling solution of the copper-nickel-based multi-core niobium-titanium superconducting wire 2 is a sulfuric acid solution with a concentration of 9 mol / L, and the corrosion time is 7 min. The copper-nickel-based multi-core niobium-titanium superconducting wire 2 does not scratch the inner wall of the copper tube when it penetrates into the interior of the oxygen-free copper tube 1, and the copper-nickel-based multi-core niobium-titanium superconducting wire Wire 2 has no defects such as bending and folding. The oxygen-free copper tube 1 is heated at 450°C during the drawing process. The hardness of the oxygen-free copper tube 1 after heating should be 50Hv. The processing rate of the drawing process is 10%. After drawing, it is determined by observation that the cross-section of the wire is not tightly fitted to the inner wall of the copper tube. Therefore, the drawing process is repeated at 450°C. The hardness of the oxygen-free copper tube 1 after heating should be 50Hv. The processing rate of the drawing process is 10%. After drawing, it is determined by observation that the cross-section of the wire is tightly fitted to the inner wall of the copper tube, and the cross-section of the wire has not changed. The sample obtained after drawing is tested in the 4.2K conventional critical current test experiment. The results are as follows: Figure 5 shown.

[0021] Example 4: The copper-nickel-based multi-core niobium-titanium superconducting wire 2 was directly tested in a 4.2K conventional critical current test experiment without being treated by the method of the present application. The results are as follows: Figure 6 shown.

[0022] According to the description of Examples 1-4, through the method of the present application (Examples 1-3), the test voltage of all copper-nickel-based multi-core niobium-titanium superconducting wires 2 can obtain a complete superconducting current transition curve during the continuous increase of the test current, and can slowly reach the critical current test criterion (i.e., 10μV / cm) during the wire test, that is, they can directly reflect the critical current value of the wire. In Example 4, the critical current test sample of the copper-nickel-based superconducting wire 2 prepared by the conventional technical method was not processed but directly installed and tested at 4.2K for critical current. It can be clearly found that with the increase of the applied current, the voltage at both ends of the wire jumped abnormally in advance, and failed to slowly reach the critical current test criterion (i.e., 10μV / cm), that is, it is impossible to obtain a complete superconducting current transition curve. Example 4 effectively proves that the sample preparation method proposed in the present application significantly improves the accuracy and success rate of the results of the critical current test of the copper-nickel-based multi-core niobium-titanium superconducting wire.

[0023] The embodiment of the present invention further provides a superconducting wire critical current test sample, comprising: An oxygen-free copper tube 1 and a copper-nickel-based multi-core niobium-titanium superconducting wire 2, wherein the copper-nickel-based multi-core niobium-titanium superconducting wire 2 is arranged inside the oxygen-free copper tube 1, the oxygen-free copper tube 1 is tightly attached to the outer surface of the copper-nickel-based multi-core niobium-titanium superconducting wire 2, and the two ends of the copper-nickel-based multi-core niobium-titanium superconducting wire 2 extend out of the two ends of the oxygen-free copper tube 1.

[0024] Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0025] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing samples for superconducting wire critical current testing, characterized in that: include: Drilling a through hole in the oxygen-free copper rod by deep hole drilling to obtain an oxygen-free copper tube (1); Cleaning the oxide layer on the surface of the copper-nickel-based multi-core niobium-titanium superconducting wire (2) and the inside of the oxygen-free copper tube (1) by pickling; Putting the pickled copper-nickel-based multi-core niobium-titanium superconducting wire (2) into the through hole of the pickled oxygen-free copper tube (1); The oxygen-free copper tube (1) on which the copper-nickel-based multi-core niobium-titanium superconducting wire (2) is placed is subjected to a hot drawing process to obtain a critical current test sample.

2. A superconducting wire critical current test sample preparation method according to claim 1, characterized in that: The outer diameter of the oxygen-free copper tube (1) is one of 7 to 10 times that of the copper-nickel-based multi-core niobium-titanium superconducting wire (2), and the through-hole diameter of the oxygen-free copper tube (1) is one of 1.1 to 1.2 times the outer diameter of the copper-nickel-based multi-core niobium-titanium superconducting wire (2).

3. A method for preparing samples for superconducting wire critical current testing according to claim 1, characterized in that: The pickling solution for pickling the oxygen-free copper tube (1) is a sulfuric acid solution with a concentration of 4 to 7 mol / L, and the corrosion time is 1 to 5 minutes.

4. A superconducting wire critical current test sample preparation method according to claim 1, characterized in that: The pickling solution for pickling the copper-nickel-based multi-core niobium-titanium superconducting wire (2) is a sulfuric acid solution with a concentration of 6 to 9 mol / L, and the corrosion time is 2 to 7 minutes.

5. A superconducting wire critical current test sample preparation method according to claim 1, characterized in that: The critical current test sample obtained by hot drawing the oxygen-free copper tube (1) on which the copper-nickel-based multi-core niobium-titanium superconducting wire (2) is placed is obtained by heating the oxygen-free copper tube (1) during the drawing process at a temperature of 350-450° C. After heating, the hardness of the oxygen-free copper tube (1) should be between 50 and 70 Hv, and the processing rate of the drawing process is 5%-10%. After the hot drawing, the inner wall of the oxygen-free copper tube (1) is tightly attached to the surface of the copper-nickel-based multi-core niobium-titanium superconducting wire (2).

6. A superconducting wire critical current test sample preparation method according to claim 1, characterized in that: After obtaining a critical current test sample by hot drawing the oxygen-free copper tube (1) on which the copper-nickel-based multi-core niobium-titanium superconducting wire (2) is placed, the method further comprises: The oxygen-free copper tube (1) at both ends of the copper-nickel-based multi-core niobium-titanium superconducting wire (2) is removed, so that the two end faces of the copper-nickel-based multi-core niobium-titanium superconducting wire (2) are exposed at both ends of the oxygen-free copper tube (1).

7. A superconducting wire critical current test sample, characterized in that: include: An oxygen-free copper tube (1) and a copper-nickel-based multi-core niobium-titanium superconducting wire (2), wherein the copper-nickel-based multi-core niobium-titanium superconducting wire (2) is arranged inside the oxygen-free copper tube (1), the oxygen-free copper tube (1) is closely attached to the outer surface of the copper-nickel-based multi-core niobium-titanium superconducting wire (2), and two ends of the copper-nickel-based multi-core niobium-titanium superconducting wire (2) extend out of two ends of the oxygen-free copper tube (1).

Citation Information

Cited By

  • High-performance superconducting switch line and preparation method thereof

    CN119864210A

  • Method for detecting core breakage position and core breakage rate of superconducting wire

    CN119985095A