Sample manufacturing method for scanning electron microscope analysis of three-dimensional porous material

Through the infiltration technology of room temperature ionic liquid and solvent, the problems of poor conductivity and charge effect of three-dimensional porous materials in SEM test are solved, and all-round improvement of conductivity and image quality are achieved, ensuring the material's morphological observation quality.

CN119000754AActive Publication Date: 2024-11-22QUZHOU RES INST OF ZHEJIANG UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411076054.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

During the SEM test, the three-dimensional porous material has a severe charge effect due to poor conductivity and complex structure, which reduces the image quality. The existing gold spray sputtering conductive layer method cannot achieve all-round and blind spot improvements.

Method used

The three-dimensional porous material is infiltrated with a miscible solution of room temperature ionic liquid and solvent, and slowly immersed through a high-precision syringe pump and dried in the oven to ensure that each pore wall and surface of the material is uniformly wet with conductive particles and improve the conductivity of the sample.

Benefits of technology

The scanning electron microscope image quality of three-dimensional porous materials is significantly improved, reducing or eliminating the charge effect, ensuring the uniformity and integrity of the material's conductivity, and maintaining the stability of the original morphology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119000754A_ABST
    Figure CN119000754A_ABST
Patent Text Reader

Abstract

The invention discloses a manufacturing method of a three-dimensional porous material scanning electron microscope morphology analysis sample, which takes a three-dimensional porous material with a rich microporous structure as a morphology observation object, and utilizes good ionic conductivity of room-temperature ionic liquid and lossless infiltration of the sample to improve the conductivity of the sample in all directions. Therefore, a high-quality SEM image without a charge effect is obtained. The method can solve the problem that conductive particles cannot be sputtered on each hole wall, net and sheet layers of the three-dimensional porous material when the conductivity of a sample is increased by plating a conductive film at the present stage, so that the conductivity of the material can be increased in an omnibearing and dead-corner-free manner.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of increasing the conductivity of three-dimensional porous materials in an all-round and non-dead-angle manner using an ionic liquid mixture during SEM testing. More specifically, it relates to a method for increasing the conductivity of a three-dimensional porous sample by infiltrating the ionic liquid mixture, thereby reducing or even eliminating the charging effect generated during the SEM testing process and improving the quality of the observed SEM image. Background Art

[0002] Three-dimensional porous and structured porous materials have a wide range of applications in catalysis, adsorption, energy storage and biomedicine due to their high specific surface area, high porosity, low density and good diffusion properties. The geometric morphology characteristics of three-dimensional materials largely affect many basic properties and usage functions of the materials, especially for high porosity and high specific surface area materials, their microscopic morphology is one of the important factors affecting their application and performance. Therefore, the analysis and characterization of the microscopic morphology of three-dimensional materials is of great significance. However, for three-dimensional materials with complex microstructures, the elasticity and brittleness of their three-dimensional skeletons and their poor electrical conductivity result in obvious jitter, drift and obvious charge whitening during SEM morphology observation, which reduces the image quality. Therefore, the problems of difficult fixation and poor conductivity of three-dimensional materials need to be solved by changing the sample preparation method and improving the conductivity of the sample.

[0003] The most common method to reduce the charging effect during SEM testing is to use an ion sputtering instrument to sputter a conductive layer to change the conductivity of the sample surface, so that the charge accumulated on the sample surface can be exported through the sample stage, thereby effectively eliminating or reducing the impact of the charging effect on the test results, and also improving the image quality of the sample. However, the method of sputtering with a gold sprayer can only sputter the conductive film onto the sample surface. For solids with complex three-dimensional porous, mesh, and lamellar structures, the conductive film is mainly concentrated on the upper surface layer, and the sputtering efficiency of some sub-surface layers and sides of the sample is poor, which easily leads to uneven overall conductivity of the sample and poor observation effect. Therefore, the sample preparation method to improve the uniformity and integrity of the conductive film of three-dimensional porous, mesh, and lamellar structure samples has become a difficult point.

[0004] At present, due to the negligible vapor pressure and relatively high ionic conductivity of room temperature ionic liquids at room temperature, it can replace the conductive layer sputtered by the gold spraying instrument to conduct the sample. 1-ethyl-3-methylimidazolium tetrafluoroborate ionic liquid and ethanol and / or acetone diluent are used for the conductive pretreatment of insulating samples, which has the advantages of low cost and simple operation, but it does not pay attention to the structural stability and polarity of the sample. First, directly dripping the diluent of the ionic liquid on the surface of the sample can easily deform the sample, resulting in the accuracy of the analytical data being affected. Secondly, the polarity of a single ionic liquid is fixed, and it is difficult to have good wettability for samples with polarity that do not match it, and it is impossible to obtain a uniform infiltration of the ionic liquid on the surface of the three-dimensional material, thereby failing to improve the conductivity of the sample. Therefore, the polarity of the sample and the ionic liquid diluent is also a decisive factor affecting the uniformity and integrity of the ionic liquid conductive film. Summary of the invention

[0005] Based on the above problems, the purpose of the present invention is to provide a method for preparing samples for scanning electron microscope morphology analysis of three-dimensional porous materials. The sample preparation method in the present invention is simple, efficient, and low-cost, and the method can significantly improve the quality of scanning electron microscope images of three-dimensional porous materials, which is of great significance for the analysis and characterization of the microscopic morphology of three-dimensional materials.

[0006] The present invention provides a method for preparing a three-dimensional porous material scanning electron microscope morphology analysis sample, comprising the following steps:

[0007] Cutting porous materials into suitable sizes;

[0008] The porous material is glued into a conductive tank, wherein the conductive tank is a container made of conductive material and having an upper end open;

[0009] preparing a mixed solution of a room temperature ionic liquid and a solvent;

[0010] The room temperature ionic liquid refers to one or more molten salts that are liquid at room temperature or near room temperature (20-30°C) (melting point ≤ 30°C); usually composed of specific organic cations and inorganic anions or organic anions, and the organic cations include imidazoles (structural formula: ), piperidines (structural formula: ), pyrrolidines (structural formula ), pyridines (structural formula is ), etc., wherein R1, R2, and R3 are alkyl substituents with a carbon chain length of n, 0≤n≤8, and the carbon chain lengths n of R1, R2, and R3 are not all 0 at the same time; wherein R8, R9, R 10 are alkyl substituents with carbon chain length n, 0≤n≤8, and R8, R9, R 10The carbon chain length n is different and is taken as 0; wherein R4, R5, R6, R7 are alkyl substituents with carbon chain length n, 1≤n≤8;

[0011] The anion is one or more of halogen ion, tetrafluoroborate ion, hexafluorophosphate ion, bis(trifluoromethanesulfonyl imide) and the like;

[0012] The contact angle between the room temperature ionic liquid mixture and the sample to be tested exist Between (preferably More preferred );

[0013] Add the mixed solution into the conductive tank so that the solution slowly infiltrates the entire porous material, that is, each outer surface of the material is completely wetted;

[0014] The infiltrated porous material is dried to remove the solvent, so as to obtain a porous material sample placed in a conductive tank and used for scanning electron microscope morphology analysis.

[0015] The mixed solution is loaded into a syringe;

[0016] Install the above syringe on a high-precision syringe pump and set the flow rate to 0.05-0.5 mL / min to allow the solution to slowly infiltrate the porous body;

[0017] Put the conductive slot with porous material into an oven at a temperature of 30-90°C and a drying time of 8-24 hours.

[0018] Preferably, the preset length*width*height dimensions of the porous material are 0.5*0.5*0.1 cm 3 -1*1*1cm 3 ;

[0019] The conductive slot is made of one or both of conductive copper foil and aluminum foil, with a thickness of 0.01-0.2 cm. The internal cavity of the conductive slot is a rectangular parallelepiped. The length of the internal cavity of the conductive slot is 0.4-2.0 cm (preferably 0.5-1.5 cm, more preferably 0.8-1.2 cm) larger than the length of the porous material. The width of the internal cavity of the conductive slot is 0-1 cm (preferably 0-0.5 cm, more preferably 0.01-0.4 cm) larger than the width of the porous material. The height of the internal cavity of the conductive slot is 0-0.5 cm (preferably 0-0.05 cm, more preferably 0-0.02 cm) smaller than the height of the porous material.

[0020] Preferably, the thickness of the conductive slot material is 0.05-0.15 cm, the length of the preset size of the conductive slot is 0.5-1.0 cm larger than the size of the porous material, and the width and height of the preset size of the conductive slot are 0-0.5 cm larger than the size of the porous material; the length of the preset size of the conductive slot is 0.5-1.0 cm larger than the size of the porous material, the width of the preset size of the conductive slot is 0-0.4 cm larger than the width of the porous material, and the height of the preset size of the conductive slot is 0-0.2 cm smaller than the size of the porous material;

[0021] The room temperature ionic liquid is specifically: one or more of 1-ethyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide, 1-butyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium dinitrile amine salt, N-propyl-N-methylpiperidinium bis(trifluoromethanesulfonyl)imide salt, and N-butyl-N-methylpyrrolidine bis(trifluoromethanesulfonyl)imide salt.

[0022] The solvent is one or more of water, methanol, ethanol, ethyl acetate, and dichloromethane;

[0023] The volume ratio of the room temperature ionic liquid to the solvent in the prepared mixed solution of the room temperature ionic liquid and the solvent is 1:1 to 1:20 (preferably 1:2 to 1:16, more preferably 1:5 to 1:10).

[0024] Preferably, the contact angle between the room temperature ionic liquid mixture and the sample to be tested is close to exist between;

[0025] Preferably, the preparation of a mixed solution of room temperature ionic liquid and organic solvent comprises the steps of:

[0026] Mixing a room temperature ionic liquid and an organic solvent according to a volume ratio, wherein the volume ratio is room temperature ionic liquid: organic solvent = 1:2 to 1:10;

[0027] Preferably, the propulsion speed of injecting the mixed solution with a high-precision injection pump is 0.01-1 mL / min;

[0028] Preferably, the removing of the volatile solvent in the porous material infiltrated by the miscible solution comprises the steps of:

[0029] Preferably, the oven drying temperature is 50-80° C., and the drying time is 12-24 hours.

[0030] The beneficial effects of the present invention are as follows:

[0031] The sample preparation method provided by the present invention is simple, efficient and low-cost. The method can not only maintain the original morphology of the three-dimensional material, but also make each pore wall, mesh and sheet layer of the three-dimensional porous material infiltrated with conductive particles, thereby achieving an all-round and dead-angle increase in the conductivity of the material, thereby significantly improving the quality of its scanning electron microscope image, which is of great significance for the analysis and characterization of the microscopic morphology of three-dimensional materials.

[0032] The present invention uses three-dimensional porous materials with rich microporous structures as the morphology observation object, and utilizes the good ionic conductivity of room temperature ionic liquids and the non-destructive infiltration of samples to comprehensively increase the conductivity of samples, thereby obtaining high-quality SEM images without charging effects, which is beneficial to SEM morphology observation.

[0033] It can solve the problem that when conductive film plating is used to increase the conductivity of samples at the current stage, it is impossible to sputter conductive particles on each pore wall, mesh and sheet layer of the three-dimensional porous material to achieve an all-round and dead-angle-free increase in the conductivity of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] The specific implementation modes of the present invention will be further described in detail below in conjunction with the accompanying drawings.

[0035] Figure 1 Optical images of SiO2 aerogel before (a) and after (b) infiltration of SiO2 aerogel with room temperature ionic liquid in Example 1 are shown.

[0036] Figure 2 The SEM images (ac) of the SiO2 aerogel after gold spraying and (de) of the SiO2 aerogel after being infiltrated with room temperature ionic liquid in Example 1 are shown, wherein the magnifications are 4K, 20K and 20K, respectively. DETAILED DESCRIPTION

[0037] In order to more clearly illustrate the present invention, the present invention is further described below in conjunction with preferred embodiments and accompanying drawings. Similar components in the accompanying drawings are represented by the same reference numerals. It should be understood by those skilled in the art that the content specifically described below is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.

[0038] Example 1

[0039] Here we take SiO2 nanofiber aerogel and 1-ethyl-3-methylimidazolidine dinitrile amine salt-ethyl acetate mixture as an example:

[0040] The preparation method of SiO2 nanofiber aerogel is prepared according to the method of ACS Appl. Mater. Interfaces 2019, 11, 29056-29064, and the specific steps include the following:

[0041] First, TEOS (tetraethyl orthosilicate), H2O, EtOH and C2H2O4 (oxalic acid) were mixed at room temperature for 8 hours in a molar ratio of 1:3.57:0.71:0.016 to prepare a SiO2 precursor sol solution. Then, 0.26g SiO2 was uniformly dispersed in the above-mentioned SiO2 precursor sol solution, and homogenized and dispersed for 10 minutes under high-speed stirring to prepare a SiO2 sol. At the same time, PVB powder (polyvinyl butyral) was dissolved in EtOH and stirred for 8 hours at room temperature to prepare a 23wt% PVB / EtOH solution. Subsequently, SiO2 sol and PVB / EtOH solution were mixed in a mass ratio of 3:1, and stirred for another 4 hours to obtain an electrospinning precursor solution. Subsequently, an electrostatic spinning process was performed using a DXES-1 spinning device (the inner diameter of the nozzle was 0.1-1.6mm, and the inner diameter used in this embodiment was 0.8mm), applying a high voltage of 15kV, a receiving distance of 15cm, and a constant feed rate of 1mL / h. The spun composite PVB / TEOS composite nanofibers were gradually heated to 800°C at a heating rate of 5°C / min in a muffle furnace for calcination to obtain pure SiO2 nanofiber aerogel.

[0042] Cut the above SiO2 nanofiber aerogel into pieces with length * width * height = 0.62 * 0.51 * 0.33 cm 3 Size;

[0043] The aerogel was adhered to a conductive slot (a container with an upper opening) made of copper foil using Nissin 732 aluminum-based double-sided carbon conductive tape. The thickness of the copper foil was 0.1 cm, and the size of the inner chamber of the conductive slot was length*width*height=1.14*0.53*0.30 cm 3 ;

[0044] Preparation of mixed solutions of room temperature ionic liquids and organic solvents:

[0045] Take the 1-ethyl-3-methylimidazolium dinitrile amine salt and ethyl acetate and mix them to prepare 200uL of a mixed solution with a volume ratio of 0.2. The contact angle of the room temperature ionic liquid mixed solution with the sample to be tested is

[0046] The mixed solution was loaded into a 200uL syringe;

[0047] The syringe was mounted on a high-precision syringe pump, and the advancement speed was set to 0.1 mL / min and the advancement time was set to 1.5 min, so that the solution slowly infiltrated the porous material, that is, all the outer surfaces of the material were completely wetted;

[0048] The infiltrated aerogel was placed in a clean oven at 50° C. and dried for 12 h to remove volatile solvents such as ethyl acetate.

[0049] like Figure 1Shown are optical images of the SiO2 nanofiber aerogel in Example 1 before and after infiltration. It can be seen that all outer surfaces of the aerogel are wetted, indicating that it has been completely infiltrated by the room temperature ionic liquid mixture, and the length, width and height changes before and after infiltration are less than ±0.02 cm. It is preliminarily believed that the three-dimensional configuration is well maintained (volume deformation is less than 5%).

[0050] The sample in Example 1 was subjected to SEM detection, and the SEM model was SU8230 produced by Hitachi;

[0051] The test conditions for SEM detection are: vacuum degree of 0.0001 Pa, acceleration voltage of 10 kV, electron beam current of 10 pA, and working distance of 10 mm. The present invention uses a secondary electron detector to receive signals and conduct morphological analysis on SiO2 nanofiber aerogel.

[0052] The morphology of SiO2 nanofiber aerogel is as follows Figure 2 As shown in df, the fiber interlaced structure of SiO2 nanofiber aerogel is well maintained without collapse; no obvious charge accumulation and drift phenomenon occurs at a magnification of less than 50K during the test, thus obtaining a high-quality SiO2 nanofiber aerogel morphology. From the SEM image, it can be seen that the diameter of SiO2 nanofibers is 100-200nm. This shows that treating SiO2 aerogel with a mixture of 1-ethyl-3-methylimidazole dinitrile amine salt and ethyl acetate is not only simple to operate and low in cost, but also can increase its conductivity in all directions, reduce or eliminate the charging effect, and improve the imaging quality.

[0053] Example 2

[0054] Here we take SiO2 nanofiber aerogel and 1-ethyl-3-methylimidazolidine dinitrile amine salt-ethanol mixed solution as an example:

[0055] The SiO2 nanofiber aerogel prepared in Example 1 was cut into 0.7*0.6*0.3cm 3 Size;

[0056] The aerogel was adhered to a conductive slot (a container with an upper opening) made of copper foil using Nissin 732 aluminum-based double-sided carbon conductive tape. The thickness of the copper foil was 0.1 cm, and the size of the inner chamber of the conductive slot was length*width*height=1.2*0.7*0.3 cm. 3 ;

[0057] Preparation of mixed solutions of room temperature ionic liquids and organic solvents:

[0058] Take the 1-ethyl-3-methylimidazolium dinitrile salt and ethanol and mix them to prepare 300uL of a mixed solution with a volume ratio of 0.2. The contact angle of the room temperature ionic liquid mixed solution with the sample to be tested is

[0059] The mixed solution was loaded into a 500uL syringe;

[0060] The above syringes were installed on a high-precision syringe pump, and the pushing speed was set to 0.2 mL / min and the pushing time was set to 1.0 min, so that the solution slowly infiltrated the porous material, that is, each outer surface of the material was completely wetted;

[0061] The infiltrated aerogel was placed in a clean oven at 50° C. and dried for 12 h to remove volatile solvents such as ethanol.

[0062] In Example 2, the height of the SiO2 nanofiber aerogel changed slightly before and after being infiltrated, and the configuration was well maintained.

[0063] The samples in Example 2 were subjected to SEM examination, and the SEM model was SU8230 produced by Hitachi;

[0064] The test conditions for SEM detection are: vacuum degree of 0.0001 Pa, acceleration voltage of 10 kV, electron beam current of 10 pA, and working distance of 10 mm. The present invention uses a secondary electron detector to receive signals and conduct morphological analysis on SiO2 nanofiber aerogel.

[0065] The structure of SiO2 nanofiber aerogel is well maintained and has not collapsed. During the test, when the magnification is 35K, the fiber surface is abnormally bright due to charge accumulation, causing one part of the image to be abnormally bright and the other part to be dark. However, no charging effect is observed at a magnification of less than 30K. The image brightness is uniform, and the interweaving of the fibers can be clearly seen. It can be seen from the figure that the diameter of SiO2 nanofibers is 100-200nm. This shows that treating SiO2 nanofiber aerogel with a mixture of 1-ethyl-3-methylimidazole dinitrile amine salt and ethanol can increase its conductivity, reduce the charging effect, and improve the imaging quality.

[0066] Example 3

[0067] Here we take boron nitride microporous material and N-butyl-N-methylpyrrolidine bis(trifluoromethanesulfonyl)imide salt-methanol mixed solution as an example:

[0068] Boron nitride microporous material was purchased from Qingzhou Haoyu Special Ceramics New Materials Co., Ltd., and its theoretical density is 2.29 g / cm 3 , molecular weight is 24.81, Mohs hardness is 1-2;

[0069] Cut the above-mentioned boron nitride microporous material into 0.6*0.5*0.4cm 3 Size;

[0070] The above sample was glued into a conductive slot (a container with an upper opening) made of copper foil using Nissin 732 aluminum-based double-sided carbon conductive tape. The thickness of the copper foil was 0.1 cm, and the size of the internal chamber of the conductive slot was length * width * height = 1.3 * 0.6 * 0.3 cm 3 ;

[0071] Preparation of mixed solutions of room temperature ionic liquids and organic solvents:

[0072] Take the N-butyl-N-methylpyrrolidine bis(trifluoromethanesulfonyl)imide salt and methanol and mix them to prepare 200uL of a mixed solution with a volume ratio of 0.1. The contact angle of the room temperature ionic liquid mixed solution with the sample to be tested is

[0073] The mixed solution was loaded into a 200uL syringe;

[0074] Install the above syringes on a high-precision syringe pump, and set the pushing speed to 0.05 mL / min and the pushing time to 4.0 min, so that the solution slowly infiltrates the sample, that is, all outer surfaces of the material are completely wetted;

[0075] The infiltrated samples were placed in a clean oven at 50° C. and dried for 12 h to remove volatile solvents such as methanol.

[0076] In Example 3, the structure of the boron nitride microporous material remains unchanged before and after being infiltrated.

[0077] The samples in Example 3 were subjected to SEM examination, and the SEM model was SU8230 produced by Hitachi;

[0078] The test conditions for SEM detection are: vacuum degree of 0.0001 Pa, acceleration voltage of 10 kV, electron beam current of 10 pA, and working distance of 10 mm. The present invention uses a secondary electron detector to receive signals and perform morphological analysis on the boron nitride microporous material.

[0079] The structure of the boron nitride microporous material is well maintained, and there is no structural collapse or micropore blockage. During the test, when the magnification is greater than 20K, irregular bright spots and bright lines appear in the image, but by speeding up the scanning speed, a high-quality SEM image can still be obtained at 20K. From the SEM image, it can be seen that the pore size of the boron nitride microporous material is 80-200um. This shows that the treatment of the boron nitride microporous material with a mixture of N-butyl-N-methylpyrrolidine bis (trifluoromethanesulfonyl) imide salt-methanol is effective in increasing its conductivity and can meet normal test requirements.

[0080] Example 4

[0081] Here we take polyurethane foam and 1-butyl-3-methylimidazolium tetrafluoroborate-ethanol mixed solution as an example:

[0082] Polyurethane foam was purchased from Wenzhou Nanbao Sponge Co., Ltd. with a density of 0.022-0.08 g / cm 3 ;

[0083] Cut the above polyurethane foam into 0.65*0.53*0.37cm 3 Size;

[0084] The polyurethane foam was adhered to a conductive slot (a container with an upper opening) made of copper foil using Nissin 732 aluminum-based double-sided carbon conductive tape. The thickness of the aluminum foil was 0.5 cm, and the size of the inner chamber of the conductive slot was length*width*height=1.2*0.55*0.30 cm 3 ;

[0085] Preparation of mixed solutions of room temperature ionic liquids and organic solvents:

[0086] Take the 1-ethyl-3-methylimidazolium dinitrile amine salt and ethyl acetate and mix them to prepare 200uL of a mixed solution with a volume ratio of 0.15. The contact angle of the room temperature ionic liquid mixed solution with the sample to be tested is is 38°;

[0087] The mixed solution was loaded into a 200uL syringe;

[0088] The syringe was installed on a high-precision syringe pump, and the advancement speed was set to 0.1 mL / min and the advancement time was set to 1.5 min, so that the solution slowly infiltrated the polyurethane foam, that is, all outer surfaces of the material were completely wetted;

[0089] After the polyurethane foam was infiltrated, there was no structural collapse or deformation;

[0090] The impregnated polyurethane foam was placed in a clean oven at 50° C. and dried for 12 hours to remove volatile solvents such as ethanol.

[0091] The sample in Example 4 was subjected to SEM detection, and the SEM model was SU8230 produced by Hitachi; the test conditions during SEM detection were: vacuum degree of 0.0001Pa, acceleration voltage of 10kV, electron beam current of 10pA, and working distance of 10mm. The present invention uses a secondary electron detector to receive signals and perform morphological analysis on polyurethane foam.

[0092] During the test, within the magnification of 30K, the image was slightly distorted, but the morphology of the polyurethane foam could still be obtained after increasing the scanning speed, and it can be seen that the pore size of the polyurethane foam is 50-200um. When the magnification is greater than 30K, the image distortion becomes serious and the true morphology cannot be obtained. This shows that treating the polyurethane foam with a mixture of 1-butyl-3-methylimidazolium tetrafluoroborate 1-ethyl-3-methylimidazolium dinitrile amine salt-ethyl acetate ethanol can increase its conductivity and reduce the accumulation of charges on the sample surface, thereby obtaining the desired morphology.

[0093] Example 5

[0094] Here we take porous alumina ceramics and 1-ethyl-3-methylimidazolidine dinitrile amine salt-ethyl acetate mixture as an example:

[0095] Porous alumina ceramics were purchased from Jiangxi Yitian Filler Industry Co., Ltd. and have a density of 0.42 g / cm 3 , porosity is 80-90%;

[0096] Cut the porous alumina ceramic into pieces of 0.7*0.6*0.5cm 3 Size;

[0097] The porous alumina ceramic was glued to a conductive slot (a container with an upper opening) made of copper foil using Nissin 732 aluminum-based double-sided carbon conductive tape. The thickness of the aluminum foil was 0.5 cm, and the size of the inner chamber of the conductive slot was length*width*height=1.3*0.9*0.30 cm. 3 ;

[0098] Preparation of mixed solutions of room temperature ionic liquids and organic solvents:

[0099] The 1-ethyl-3-methylimidazolium dinitrile amine salt was mixed with ethyl acetate to prepare 400uL of a mixed solution with a volume ratio of 0.15. The contact angle of the room temperature ionic liquid mixed solution with the sample to be tested was is 34°;

[0100] The mixed solution was loaded into a 500uL syringe;

[0101] The syringe was installed on a high-precision syringe pump, and the advancement speed was set to 0.1 mL / min and the advancement time was set to 3.5 min, so that the solution slowly infiltrated the polyurethane foam, that is, all outer surfaces of the material were completely wetted;

[0102] After the porous alumina ceramics were infiltrated, there was no structural collapse or deformation;

[0103] The infiltrated porous alumina ceramics were placed in a clean oven at 50° C. and dried for 12 h to remove volatile solvents such as ethanol.

[0104] The sample in Example 5 was subjected to SEM detection, and the SEM model was SU8230 produced by Hitachi; the test conditions during SEM detection were: vacuum degree of 0.0001Pa, acceleration voltage of 10kV, electron beam current of 10pA, and working distance of 10mm. The present invention uses a secondary electron detector to receive signals and perform morphological analysis on porous alumina ceramics.

[0105] A clear alumina ceramic morphology can be obtained at a magnification of 30K, from which it can be seen that the pore size of the porous alumina ceramic is 50-200um. This shows that treating porous alumina ceramics with a mixture of 1-butyl-3-methylimidazolium tetrafluoroborate 1-ethyl-3-methylimidazolium dinitrile amine salt-ethyl acetate ethanol can improve the conductivity of the material, reduce the charging effect, and improve the imaging quality.

[0106] Example 6

[0107] Here we take glass fiber, 1-ethyl-3-methylimidazoline bis(trifluoromethylsulfonyl)imide-methanol mixed solution as an example:

[0108] The glass fiber was purchased from Shaoguan Haoli Recycling Resources Utilization Co., Ltd. with a density of 1.63g / cm 3 ;

[0109] Cut the above glass fiber into 0.8*0.8*0.5cm 3 Size;

[0110] The glass fiber was glued to a conductive slot (a container with an upper opening) made of copper foil using Nissin 732 aluminum-based double-sided carbon conductive tape. The thickness of the aluminum foil was 0.5 cm, and the size of the inner chamber of the conductive slot was length*width*height=1.3*1.2*0.30 cm. 3 ;

[0111] Preparation of mixed solutions of room temperature ionic liquids and organic solvents:

[0112] Take the 1-ethyl-3-methylimidazoline bis(trifluoromethylsulfonyl)imide and methanol and mix them to prepare 200uL of a mixed solution with a volume ratio of 0.1. The contact angle of the room temperature ionic liquid mixed solution with the sample to be tested is is 38°;

[0113] The mixed solution was loaded into a 200uL syringe;

[0114] The syringe was installed on a high-precision syringe pump, and the advancement speed was set to 0.1 mL / min and the advancement time was set to 4 min, so that the solution slowly infiltrated the glass fiber, that is, all outer surfaces of the material were completely wetted;

[0115] After the glass fiber was impregnated, there was no structural collapse or deformation;

[0116] The impregnated glass fiber is placed in a clean oven at 50° C. and dried for 12 hours to remove volatile solvents such as methanol.

[0117] The sample in Example 6 was subjected to SEM detection, the SEM model was SU8230 produced by Hitachi; the test conditions during SEM detection were: vacuum degree of 0.0001Pa, acceleration voltage of 10kV, electron beam current of 10pA, and working distance of 10mm. The present invention uses a secondary electron detector to receive signals and perform morphological analysis on the glass fiber.

[0118] At a magnification of 15K, the uniformly distributed glass fibers can be clearly seen, and the diameter of the fibers is 10-20um. This indicates that treating the glass fibers with a mixture of 1-ethyl-3-methylimidazoline bis(trifluoromethylsulfonyl)imide-methanol can increase their conductivity, reduce the charging effect, and improve the imaging quality.

[0119] Comparative Example 1

[0120] The SiO2 aerogel prepared in Example 1 was cut into 0.6*0.5*0.3cm 3 Size;

[0121] The porous material is fixed on a sample stage with Nissin 732 aluminum-based double-sided carbon conductive tape;

[0122] Place the sample stage into the chamber of a Hitachi MC1000 ion sputtering instrument, set the sputtering current to 10 mA, the time to 90 s, and click to start sputtering a platinum metal coating on the sample surface. The thickness of the sputtered metal layer is 5 nm.

[0123] The sample in comparative example 1 was subjected to SEM detection, and the SEM model was SU8230 produced by Hitachi;

[0124] The test conditions for SEM detection are: vacuum degree of 0.0001 Pa, acceleration voltage of 10 kV, electron beam current of 10 pA, and working distance of 10 mm. The present invention uses a secondary electron detector to receive signals and perform morphological analysis on SiO2 aerogel.

[0125] The morphology of SiO2 aerogel is as follows Figure 2As shown in Figures ac, the SiO2 aerogel structure is well maintained without collapse; during the test, there is obvious charge accumulation and drift, and even at a magnification of 4K, the image drift is serious when using a fast scan method. There are multiple charged black stripes in the image and the image is distorted, so it is impossible to obtain a high-quality SiO2 aerogel morphology image. This shows that the method of sputtering metal coating with a gold spraying instrument is not effective in improving the overall conductivity of SiO2 aerogel.

[0126] Comparative Example 2

[0127] Example 1 was repeated (the process and conditions were the same as those of Example 1), except that the SiO2 aerogel prepared in Example 1 was replaced with a hydrophobic SiO2 nanofiber aerogel, and other conditions remained unchanged. The preparation method of the hydrophobic SiO2 nanofiber aerogel is as follows: the SiO2 nanofiber aerogel of Example 1 was immersed in a 5.0g SiF3 ethanol solution (15wt.%) and aged for 3 days, the solvent was exchanged with ethanol, and finally the hydrophobic SiO2 nanofiber aerogel was obtained by drying with supercritical carbon dioxide. The contact angle of the hydrophobic SiO2 nanofiber aerogel with the 1-ethyl-3-methylimidazole dinitrile amine salt-ethyl acetate mixture was The mixed liquid cannot infiltrate the sample. During the SEM test, due to the poor conductivity of the sample itself and the lack of effective infiltration by the ionic liquid mixed liquid, an obvious charging effect occurs. During the scanning process, the image jitters and drifts. The resulting morphology shows fiber distortion, phase difference, and abnormal brightening of the fiber edge, making it impossible to display sample details.

[0128] Comparative Example 3

[0129] Example 1 was repeated (process and conditions were the same as in Example 1), except that the 1-ethyl-3-methylimidazolidine dinitrile amine salt-ethyl acetate mixture was replaced with an equal volume ratio of N-hexylpyridinium bromide salt-ethanol mixture, and other conditions remained unchanged. Since the melting point of N-hexylpyridinium bromide salt is 46° C., during the SEM detection process, when the incident electron beam interacts with the sample surface, the temperature of the sample surface will rise, causing the N-hexylpyridinium bromide salt solidified at 46° C. to melt, affecting the stability of the sample, and the SEM image obtained by the shooting will show artifacts of deformation and morphological distortion.

[0130] Comparative Example 4

[0131] Example 1 was repeated (process and conditions were the same as Example 1), except that the advancement speed of the syringe on the high-precision syringe pump was 0.1 mL / min, and the advancement time was 1.5 min. The infiltration operation was changed to an advancement speed of 1.8 mL / min for 5 s, and other conditions remained unchanged. Due to the excessive advancement speed, the SiO2 nanofiber aerogel structure collapsed, and the volume deformation was greater than 30%, and it could not be tested.

[0132] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.

Claims

1. A method for preparing samples for scanning electron microscope morphology analysis of three-dimensional porous materials, characterized in that: The steps include: Cutting three-dimensional porous materials into required sizes; Adhere the porous material in a conductive tank using conductive glue, wherein the conductive tank is a container made of conductive material and having an upper end open; preparing a mixed solution of a room temperature ionic liquid and a solvent; The room temperature ionic liquid refers to one or more molten salts that are liquid at room temperature or near room temperature (20-30°C) (melting point ≤ 30°C); usually composed of specific organic cations and inorganic anions or organic anions, and the organic cations include imidazoles (structural formula: Piperidines (structural formula: Pyrrolidines (structural formula: Pyridines (structural formula: wherein R1, R2, and R3 are alkyl substituents with a carbon chain length of n, 0≤n≤8, and the carbon chain lengths n of R1, R2, and R3 are not all 0 at the same time; wherein R8, R9, and R 10 are alkyl substituents with carbon chain length n, 0≤n≤8, and R8, R9, R 10 The carbon chain length n is different and is taken as 0; wherein R4, R5, R6, R7 are alkyl substituents with carbon chain length n, 1≤n≤8; The anion is one or more of halogen ion, tetrafluoroborate ion, hexafluorophosphate ion, bis(trifluoromethanesulfonyl imide) and the like; The contact angle between the room temperature ionic liquid mixture and the sample to be tested exist Between (preferably More preferred Add the mixed solution into the conductive tank so that the solution slowly infiltrates the entire porous material, that is, each outer surface of the material is completely wetted; The infiltrated porous material is dried to remove the solvent, so as to obtain a porous material sample placed in a conductive tank and used for scanning electron microscope morphology analysis.

2. The method according to claim 1, characterized in that: The porous material is a cuboid, and its length*width*height dimensions are 0.1-2cm*0.1-2cm*0.1-2cm respectively.

3. The method according to claim 1, characterized in that: The conductive slot is made of one or both of conductive copper foil and aluminum foil, with a thickness of 0.01-0.2 cm. The internal cavity of the conductive slot is a rectangular parallelepiped. The length of the internal cavity of the conductive slot is 0.4-2.0 cm (preferably 0.5-1.5 cm, more preferably 0.8-1.2 cm) larger than the length of the porous material. The width of the internal cavity of the conductive slot is 0-1 cm (preferably 0-0.5 cm, more preferably 0.01-0.4 cm) larger than the width of the porous material. The height of the internal cavity of the conductive slot is 0-0.5 cm (preferably 0-0.05 cm, more preferably 0-0.02 cm) smaller than the height of the porous material.

4. The method according to claim 1, characterized in that: The room temperature ionic liquid is specifically: one or more of 1-ethyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide, 1-butyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium dinitrile amine salt, N-propyl-N-methylpiperidinium bis(trifluoromethanesulfonyl)imide salt, and N-butyl-N-methylpyrrolidine bis(trifluoromethanesulfonyl)imide salt.

5. The method according to claim 1 or 4, characterized in that: The solvent is one or more of water, methanol, ethanol, ethyl acetate, and dichloromethane; The volume ratio of the room temperature ionic liquid to the solvent in the prepared mixed solution of the room temperature ionic liquid and the solvent is 1:1 to 1:20 (preferably 1:2 to 1:16, more preferably 1:5 to 1:10).

6. The method according to claim 1, characterized in that: The process of adding the above mixed solution into the conductive tank so that the solution infiltrates the entire porous material is as follows: The mixed solution is loaded into a syringe; The syringe is mounted on a high-precision syringe pump, and the flow rate is set so that the solution slowly infiltrates the porous material, that is, each outer surface of the material is completely wetted; The wetted porous substrate is placed in a clean oven to remove the volatile solvent.

7. The method according to claim 6, characterized in that: The flow rate of the mixed solution injected by the high-precision injection pump is 0.01-1 mL / min, until each outer surface of the material is completely wetted or the entire conductive groove is filled.

8. The method according to claim 1, characterized in that: The method of removing the solvent from the porous material infiltrated by the miscible solution comprises the steps of: Put the conductive slot with porous material into an oven at a temperature of 30-90°C and a drying time of 8-24 hours.

9. The method according to claim 1, characterized in that: The three-dimensional porous material includes one or more of foam material, hydrogel, porous ceramic, porous polymer material, porous carbon material, porous glass material and other three-dimensional porous materials.

10. The method according to claim 1, characterized in that: The conductive adhesive is one or more of double-sided aluminum-based carbon conductive tape or double-sided non-woven carbon conductive tape; Conductive adhesive is used to adhere the side surface and the lower surface of the porous material to the inner side surface and the bottom surface of the conductive groove.

Citation Information

Patent Citations

  • Cellulose / sodium alginate composite gel electrolyte membrane, preparation and aqueous zinc ion battery

    CN118281372A

  • Ion conductor

    JP2007311311A

  • Biochip with a three dimensional mesoporous layer and method for forming the same

    US20100254855A1

  • Energy storage device and an electrode for an energy storage device

    US20200411862A1

  • KR20220040896A