Film mirror surface and preparation method thereof

By adopting a combined design of the substrate, termination structure and protective layer in the film mirror, the mirror deformation and performance degradation caused by assembly stress is solved, and the film mirror with high reflectivity and high stability is achieved, which improves the imaging of the optical system. Mass and reflection efficiency.

CN119001940APending Publication Date: 2024-11-22INST OF SEMICONDUCTORS - CHINESE ACAD OF SCI
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202411118688.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Thin high reflectivity mirror surfaces are susceptible to stress during manufacturing and assembly, resulting in deformation and performance degradation, and mechanical stress during assembly significantly reduces reflectivity, affecting system performance.

Method used

The film mirror design consists of a substrate, a termination structure, a high reflectivity metal reflective layer covering the substrate and a protective reflective layer. The termination structure absorbs and relieves mechanical stress during the assembly process, and uses double-sided coating. Fix the stress influence between the film layers and improve the stability of the mirror surface.

Benefits of technology

Effectively prevent mirror deformation, improve imaging quality and reflection efficiency, enhance mirror durability and stability, and ensure excellent reflective performance and overall performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119001940A_ABST
    Figure CN119001940A_ABST
Patent Text Reader

Abstract

The invention provides a thin film mirror, which can be applied to the technical field of optical thin films, and comprises a substrate, a first reflecting layer, a second reflecting layer and a third reflecting layer, a second reflective layer on the second surface of the substrate; the protection layer is located on one side of the first reflection layer away from the substrate; and the terminating structure is located on the second surface of the substrate, the terminating structure and the substrate are of an integrated structure, and the first surface and the second surface are two opposite surfaces of the substrate. Through the arrangement of the end connection structure, mechanical stress generated in the assembling process is absorbed and relieved, and the mirror surface is prevented from deforming in the assembling process; the stress influence between the film layers is counteracted through double-sided film coating, so that the stability of the mirror surface is improved; and the reflecting layer is covered with the protective layer, so that the durability and the stability of the mirror surface are enhanced. The invention also provides a preparation method of the film mirror surface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of optical films, and in particular to a film mirror and a preparation method thereof. Background Art

[0002] Thin film mirrors with high reflectivity and high flatness are widely used in laser systems, optical communication equipment and precision instruments, and are essential core components for achieving high-quality reflection and precise optical control. With the advancement of technology and the increase in application requirements, the demand for thinner mirrors is becoming more and more urgent due to their low cost, light weight, high elasticity and fast response speed.

[0003] However, thinner high-reflectivity mirrors still face some technical difficulties during manufacturing and assembly. First, the film thickness needs to be precisely controlled to achieve optimal reflective performance, but thinner film layers are easily affected by stress, resulting in deformation and performance degradation. Second, thinner mirrors are easily affected by mechanical stress during assembly, which significantly reduces reflectivity and affects system performance. Therefore, selecting appropriate materials and manufacturing processes, and designing effective stress control structures, are the key to improving the performance of thin film mirrors. Summary of the invention

[0004] 1. Technical issues to be resolved

[0005] In order to solve at least one of the above technical problems of thin film mirrors in the prior art, the embodiments of the present invention provide a thin film mirror and a preparation method thereof, wherein the mirror is composed of a substrate, a terminal structure, a high reflectivity metal reflective layer covering the substrate, and a protective layer for protecting the reflective layer, and has the characteristics of high reflectivity and high flatness, and can effectively resist stress during assembly, so that the high-precision optical system has higher imaging quality and reflection efficiency. The problem of mirror deformation caused by assembly stress is solved, and the decrease in reflectivity caused by mirror deformation is avoided.

[0006] (II) Technical solution

[0007] In view of the above technical problems, an embodiment of the present invention provides a thin film mirror and a method for preparing the same.

[0008] According to a first aspect of the present invention, a thin film mirror is provided, comprising: a substrate, a first reflective layer, located on a first surface of the substrate; a second reflective layer, located on a second surface of the substrate; a protective layer, located on a side of the first reflective layer away from the substrate; and a termination structure, located on the second surface of the substrate, and the termination structure and the substrate form an integrated structure, wherein the first surface and the second surface are two opposite surfaces of the substrate.

[0009] In some exemplary embodiments, the substrate material includes one of glass, single crystal silicon, ceramic, silicon carbide, or quartz; and the first surface and the second surface have nanometer-scale flatness.

[0010] In some exemplary embodiments, the thicknesses of the first reflective layer and the second reflective layer are equal; and the thicknesses of the first reflective layer and the second reflective layer are one quarter or an integer multiple of a preset wavelength.

[0011] In some exemplary embodiments, the material of the first reflective layer and the second reflective layer includes one of a metal material and a dielectric material.

[0012] In some exemplary embodiments, the metal material includes one of aluminum, silver, or gold; and / or the dielectric material includes one of silicon oxide, titanium oxide, or aluminum oxide.

[0013] In some exemplary embodiments, the surface roughness of the first reflective layer and the second reflective layer is less than 5 nm; and / or the root mean square of the surface shape of the first reflective layer and the second reflective layer is less than one tenth of a preset wavelength.

[0014] In some exemplary embodiments, the material of the protective layer includes one of aluminum nitride, silicon oxide, or aluminum oxide; and / or the thickness of the protective layer is one quarter or an integer multiple of a preset wavelength.

[0015] According to a second aspect of the present invention, a method for preparing a thin film mirror is provided, comprising: preparing a substrate material; forming a termination structure on the second surface of the substrate by photolithography and etching processes; depositing a first reflective layer on the first surface of the substrate; depositing a second reflective layer on the second surface of the substrate; and depositing a protective layer on a side of the first reflective layer away from the substrate; wherein the first surface and the second surface are two opposite surfaces of the substrate.

[0016] In some exemplary embodiments, the method further includes: trimming surface defects of the substrate, the first reflective layer, the second reflective layer, and the protective layer so that their surface flatness meets preset requirements.

[0017] In some exemplary embodiments, a method of depositing a first reflective layer on a first surface of a substrate comprises at least one of physical vapor deposition, electrochemical deposition, and chemical vapor deposition; and / or a method of depositing a second reflective layer on a second surface of a substrate comprises at least one of physical vapor deposition, electrochemical deposition, and chemical vapor deposition; and / or a method of depositing a protective layer on a side of the first reflective layer away from the substrate comprises at least one of physical vapor deposition, electrochemical deposition, and chemical vapor deposition.

[0018] (III) Beneficial effects

[0019] It can be seen from the above technical solutions that a thin film mirror and a method for preparing the same provided by the embodiments of the present invention have at least the following beneficial effects:

[0020] (1) By setting up the termination structure, the mechanical stress generated during the assembly process is absorbed and relieved, preventing the mirror from deforming during the assembly process.

[0021] (2) Double-sided coating is used to offset the stress between film layers, thereby improving the stability of the mirror.

[0022] (3) Achieve excellent reflective performance by using high reflectivity thin film materials.

[0023] (4) By covering the reflective layer with a protective layer, the durability and stability of the mirror are enhanced.

[0024] (5) Through advanced deposition technology and post-processing technology, the thickness and uniformity of the film layer are ensured, further improving the overall performance of the mirror. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The above contents and other objects, features and advantages of the present invention will become more apparent through the following description of the embodiments of the present invention with reference to the accompanying drawings, in which:

[0026] Figure 1 A schematic diagram of the structure of a thin film mirror according to an embodiment of the present invention is shown;

[0027] Figure 2 A schematic diagram of a process for preparing a thin film mirror according to an embodiment of the present invention is shown;

[0028] Figure 3 A schematic diagram of the structure of a thin film mirror preparation process according to an embodiment of the present invention is shown;

[0029] Figure 4 A schematic diagram of a process of preparing another thin film mirror according to an embodiment of the present invention is shown;

[0030] Figure 5 A schematic diagram showing a surface shape measurement result of a thin film mirror according to an embodiment of the present invention is shown;

[0031] Figure 6 A schematic diagram schematically shows a surface roughness measurement result of a thin film mirror according to an embodiment of the present invention; and

[0032] Figure 7 The following is a schematic diagram showing the reflectivity measurement result of a thin film mirror according to an embodiment of the present invention.

[0033] Reference numerals:

[0034] 1-first reflective layer; 2-substrate; 3-second reflective layer; 4-termination structure; 5-protective layer. DETAILED DESCRIPTION

[0035] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in combination with specific embodiments and with reference to the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] Figure 1 The schematic diagram of the structure of a thin film mirror according to an embodiment of the present invention is shown schematically.

[0037] like Figure 1 As shown, a thin film mirror according to an embodiment of the present invention includes: a substrate 2, a first reflective layer 1 located on the first surface of the substrate 2; a second reflective layer 3 located on the second surface of the substrate 2; a protective layer 5 located on the side of the first reflective layer 1 away from the substrate 2; and a terminal structure 4 located on the second surface of the substrate 2, and the terminal structure 4 and the substrate 2 form an integrated structure, wherein the first surface and the second surface are two opposite surfaces of the substrate 2.

[0038] In some exemplary embodiments, the substrate material is a material with high thermal stability and mechanical strength, and optionally, the substrate material includes one of glass, single crystal silicon, ceramic, silicon carbide or quartz. The surface of the substrate 2 is processed by an ultra-precision machining process, including at least one of mechanical polishing, chemical mechanical polishing or ion beam polishing, to achieve nanometer-level flatness.

[0039] For example, a single crystal silicon material is selected as the substrate 2, and the total thickness variation (TTV) is first controlled within 1 μm by grinding with a grinder, and then magnetorheological finishing is performed to ensure that the surface roughness Ra is no greater than 5 nm and the surface root mean square value (RMS) is no greater than 0.05λ, where λ is a preset wavelength.

[0040] In some exemplary embodiments, the termination structure 4 and the substrate 2 are an integrated structure, which can be formed on the substrate 2 by photolithography and etching processes. For example, the termination structure 4 is first patterned on the substrate 2 by photolithography, and then dry-etched by plasma etching equipment to form the desired termination structure 4. The thin film mirror surface of the termination structure 4 is used to absorb and relieve the mechanical stress generated during the assembly process to prevent the mirror surface from deforming during the assembly process.

[0041] In some exemplary embodiments, the thicknesses of the first reflective layer 1 and the second reflective layer 3 are equal; and the thicknesses of the first reflective layer 1 and the second reflective layer 3 are one quarter or an integer multiple of a preset wavelength.

[0042] In some exemplary embodiments, the material of the first reflective layer 1 and the second reflective layer 3 includes one of a metal material or a dielectric material. Optionally, the metal material includes one of aluminum, silver or gold; and / or the dielectric material includes one of silicon oxide, titanium oxide or aluminum oxide. Optionally, the surface roughness of the first reflective layer 1 and the second reflective layer 3 is less than 5nm; and / or the root mean square of the surface shape of the first reflective layer 1 and the second reflective layer 3 is less than one tenth of the preset wavelength.

[0043] For example, metal aluminum is selected as the material of the first reflective layer 1 and the second reflective layer 3, and the thickness of the first reflective layer 1 and the second reflective layer 3 is equal, both 135nm. The surface roughness Ra of the first reflective layer 1 and the second reflective layer 3 is not greater than 5nm, and the surface root mean square value (RMS) of the first reflective layer 1 and the second reflective layer 3 is not greater than 0.1λ. Double-sided coating is used to offset the stress effect between the film layers, thereby improving the stability of the mirror surface. In addition, a high-reflectivity thin film material is used to achieve excellent reflection performance.

[0044] In some exemplary embodiments, the material of the protective layer 5 is selected from materials with high transparency, wear resistance, chemical corrosion resistance, and high thermal stability. Optionally, the material of the protective layer 5 includes one of aluminum nitride, silicon oxide, or aluminum oxide; and / or the thickness of the protective layer 5 is one quarter or an integer multiple of the preset wavelength. The protective layer 5 is provided to enhance the durability and environmental resistance of the mirror.

[0045] For example, silicon oxide is selected as the protective layer 5, and the thickness of the silicon oxide is designed to be 53 nm.

[0046] Figure 2 The flowchart of a method for preparing a thin film mirror according to an embodiment of the present invention is schematically shown.

[0047] like Figure 2 As shown, a method for preparing a thin film mirror according to an embodiment of the present invention includes steps S110-S150.

[0048] In step S110 , a base material is prepared.

[0049] In some exemplary embodiments, preparing the base material includes selecting a base material with high thermal stability and mechanical strength, and performing surface cleaning and ultra-precision machining.

[0050] For example, single crystal silicon with high thermal stability and mechanical strength is selected as the substrate material, and deionized water, anhydrous ethanol and acetone and other solvents are used for ultrasonic cleaning to remove surface contaminants. The total thickness deviation (TTV) is limited to within 1 μm by grinding with a grinder, and the surface roughness Ra (Ra is the arithmetic mean of the absolute value of the profile deviation within the sampling length L) is limited to within 5 nm by magnetorheological finishing, and the surface shape RMS is limited to within 0.05λ. For the initial morphology of the substrate material, see Figure 3 (a) shows the structure of the base material after grinding and magnetorheological finishing. Figure 3 (b) in the figure.

[0051] In step S120 , a termination structure 4 is formed on the second surface of the substrate 2 by photolithography and etching processes.

[0052] For example, the termination structure 4 is patterned on the substrate 2 using photolithography technology, and then dry etching is performed using plasma etching equipment to form the desired termination structure 4.

[0053] In step S130 , a first reflective layer 1 is deposited on a first surface of the substrate 2 .

[0054] In some exemplary embodiments, in a vacuum environment, a first reflective layer 1 is deposited on the first surface of the substrate 2 by at least one of physical vapor deposition (PVD), electrochemical deposition or chemical vapor deposition (CVD), and the first reflective layer 1 has a high reflectivity.

[0055] For example, in a vacuum environment, the first reflective layer 1 is deposited on the first surface of the substrate 2 by evaporation, the material of the first reflective layer 1 is metal aluminum, and the thickness of the first reflective layer 1 is 135 nm.

[0056] In step S140, a second reflective layer 3 is deposited on the second surface of the substrate 2; wherein the second surface and the first surface in step S130 are two opposite surfaces of the substrate 2. The structure obtained in this step is shown in FIG. Figure 3 (c) in it includes: a substrate 2, a first reflective layer 1 located on the first surface of the substrate 2; a second reflective layer 3 located on the second surface of the substrate 2; and a termination structure 4 located on the second surface of the substrate 2, and the termination structure 4 and the substrate 2 are an integrated structure, wherein the first surface and the second surface are two opposite surfaces of the substrate 2.

[0057] In some exemplary embodiments, in a vacuum environment, the second reflective layer 3 is deposited on the second surface of the substrate 2 by at least one of physical vapor deposition (PVD), electrochemical deposition or chemical vapor deposition (CVD), and the second reflective layer 3 has a high reflectivity.

[0058] For example, in a vacuum environment, the second reflective layer 3 is deposited on the second surface of the substrate 2 by evaporation, and the material of the second reflective layer 3 is metal aluminum and has a thickness of 135 nm.

[0059] In step S150, a protective layer 5 is deposited on the side of the first reflective layer 1 away from the substrate 2. The structure obtained in this step is shown in FIG. Figure 3 (d) in it includes: a substrate 2, a first reflective layer 1 located on the first surface of the substrate 2; a second reflective layer 3 located on the second surface of the substrate 2; a protective layer 5 located on the side of the first reflective layer 1 away from the substrate 2; and a termination structure 4 located on the second surface of the substrate 2, and the termination structure 4 and the substrate 2 are an integrated structure, wherein the first surface and the second surface are two opposite surfaces of the substrate 2.

[0060] For example, in a vacuum environment, a protective layer 5 is deposited on the side of the first reflective layer 1 away from the substrate 2 by evaporation to enhance the durability and environmental resistance of the mirror. Optionally, the material of the protective layer 5 is silicon oxide, and the thickness of the protective layer 5 is one quarter or an integer multiple of a preset wavelength. For silicon oxide material, the thickness can be set to 53nm.

[0061] Figure 4 The flowchart of another method for preparing a thin film mirror according to an embodiment of the present invention is schematically shown.

[0062] like Figure 4 As shown, according to another method for preparing a thin film mirror according to an embodiment of the present invention, in Figure 2 The preparation method shown further includes step S160.

[0063] In step S160, surface defects of the substrate 2, the first reflective layer 1, the first reflective layer 1 and the protective layer 5 are repaired so that the surface flatness thereof meets the preset requirement.

[0064] For example, an atomic force microscope (AFM) is used to measure surface roughness, a surface interferometer is used to measure surface shape, and surface defects found during the inspection process are corrected, such as using ion beam polishing (IBP) technology to further improve surface flatness.

[0065] The thin film mirror obtained according to the embodiment of the present invention has a surface shape highest point and a surface shape lowest point test value difference (PV) of 0.964λ; and a surface shape mean square error (RMS) of 0.066λ. Figure 5 ; Surface roughness Ra is 1.65nm, see Figure 6 ; and reflectance measurement results in the wavelength range of 400nm-1800nm, see Figure 7 ,Depend on Figure 7 It can be seen that the reflectivity is more than 85%. Figure 5, Figure 6 and Figure 7 The test results show that through advanced deposition technology and post-processing technology, the thickness and uniformity of the film layer are ensured, further improving the overall performance of the mirror.

[0066] The above specific embodiments further illustrate the purpose, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above are only specific embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A thin film mirror, characterized in that: include: Base, A first reflective layer, located on the first surface of the substrate; A second reflective layer, located on the second surface of the substrate; A protective layer, located on a side of the first reflective layer away from the substrate; as well as A termination structure is located on the second surface of the substrate, and the termination structure and the substrate form an integrated structure, The first surface and the second surface are two opposite surfaces of the substrate.

2. The thin film mirror according to claim 1, characterized in that: The substrate material comprises one of glass, single crystal silicon, ceramic, silicon carbide or quartz; and The first surface and the second surface have nanometer-level flatness.

3. The thin film mirror according to claim 1, characterized in that: The first reflective layer and the second reflective layer have equal thickness; and The thickness of the first reflective layer and the second reflective layer is one quarter or an integer multiple of a preset wavelength.

4. The thin film mirror according to claim 1, characterized in that: The material of the first reflective layer and the second reflective layer includes one of a metal material and a dielectric material.

5. The thin film mirror according to claim 4, characterized in that: The metal material comprises one of aluminum, silver or gold; and / or The dielectric material includes one of silicon oxide, titanium oxide or aluminum oxide.

6. The thin film mirror according to claim 1, characterized in that: The surface roughness of the first reflective layer and the second reflective layer is less than 5 nm; and / or The root mean square of the surface shapes of the first reflecting layer and the second reflecting layer is smaller than one tenth of a preset wavelength.

7. The thin film mirror according to claim 1, characterized in that: The material of the protective layer includes one of aluminum nitride, silicon oxide or aluminum oxide; and / or The thickness of the protective layer is one quarter or an integer multiple of a preset wavelength.

8. A method for preparing a thin film mirror, characterized in that: include: Prepare base material; forming a termination structure on the second surface of the substrate by photolithography and etching processes; depositing a first reflective layer on a first surface of the substrate; depositing a second reflective layer on the second surface of the substrate; Depositing a protective layer on a side of the first reflective layer away from the substrate; The first surface and the second surface are two opposite surfaces of the substrate.

9. The preparation method according to claim 8, characterized in that: Also includes: Surface defects of the substrate, the first reflective layer, the second reflective layer and the protective layer are repaired so that their surface flatness meets preset requirements.

10. The preparation method according to claim 8 or 9, characterized in that: The method of depositing the first reflective layer on the first surface of the substrate comprises at least one of physical vapor deposition, electrochemical deposition and chemical vapor deposition; and / or The method of depositing the second reflective layer on the second surface of the substrate comprises at least one of physical vapor deposition, electrochemical deposition and chemical vapor deposition; and / or The method of depositing the protection layer on the side of the first reflective layer away from the substrate comprises at least one of physical vapor deposition, electrochemical deposition and chemical vapor deposition.

Citation Information

Patent Citations

  • Device for detecting wave front of large-aperture optical system

    CN102507155A

  • Ultra-wideband laser reflecting mirror with thin films

    CN106324732A

  • Interdigitating vertical dampers for MEMS-based actuators

    CN108803004A

  • Flow field measuring instrument based on rectangular pyramid sensor and flow field measuring method

    CN113252295A

  • Method for regulating and controlling stress deformation of film layer of large-caliber high-precision optical element

    CN113655592A