Polyimide high-strength corona-resistant frequency conversion enameled copper flat wire and preparation method thereof

By doping modified silica nanoparticles in polyimide resin and using hyperbranched polyethyleneimine to form a dendritic skeleton, the shortcomings of enameled wire in corona resistance and mechanical strength are solved, and high-performance paint is achieved Preparation of copper-clad flat wire.

CN119008125AInactive Publication Date: 2024-11-22ZHEJIANG SANHANG ELECTRIC TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410986339.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing enameled wire has shortcomings in corona resistance and mechanical strength, and it is difficult to meet the ever-increasing social needs.

Method used

Doping modified silica nanoparticles in polyimide resin and organically modifying their surfaces through silane coupling agent to prevent agglomeration and forming a dendritic skeleton with a branched structure of hyperbranched polyethyleneimine , improve the dispersion and mechanical strength of nano-silica in enameled wire.

Benefits of technology

The corona resistance and mechanical strength of the enameled copper flat wire is significantly improved, ensuring high-performance applications of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004957509240000101
    Figure BDA0004957509240000101
Patent Text Reader

Abstract

The invention relates to the technical field of enameled wires, in particular to a polyimide high-strength corona-resistant variable-frequency enameled copper flat wire and a preparation method thereof, and the preparation method comprises the following steps: preparing modified silicon dioxide nanoparticles; and blending the modified silicon dioxide nanoparticles with a polyimide insulating resin solution to obtain the wire enamel. And coating the surface of the copper flat wire with the wire enamel, and baking and curing to obtain the copper flat wire. The polyimide resin is doped with the silicon dioxide nanoparticles, and the silicon dioxide nanoparticles are inorganic insulating nanoparticles, so that the corona resistance of the enameled copper flat wire can be effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of enameled wires, and in particular to a polyimide high-strength corona-resistant variable-frequency enameled copper flat wire and a preparation method thereof. Background Art

[0002] Enameled wire is the main raw material for motors, electrical appliances, household appliances and other products. In particular, the power industry has continued to grow rapidly in recent years. The rapid development of household appliances has brought a wider application field for enameled wire, and with it, higher requirements for enameled wire. Enameled wire is a main type of winding wire. It consists of two parts: conductor and insulation layer. The bare wire is annealed and softened, and then painted and baked many times. However, it is not easy to produce products that meet both standard requirements and customer requirements. It is affected by factors such as raw material quality, process parameters, production equipment, and environment. Therefore, the quality characteristics of various enameled wires are different, but they all have four major properties: mechanical properties, chemical properties, electrical properties, and thermal properties.

[0003] There are many types of enameled wires. One of the earliest varieties developed in the world is acetal enameled wire. Although the temperature resistance level of this enameled wire is low, it is widely used in oil-immersed transformers due to its excellent high-temperature hydrolysis resistance. Secondly, polyester enameled wire and polyurethane enameled wire were successfully developed by Germany. Polyurethane enameled wire was developed by Bayer in Germany in 1937. Due to its direct welding, high-frequency resistance and dyeability, it is widely used in electronics, electrical appliances and other fields. Subsequently, the requirements for the properties of enameled wires became higher and higher. Polyesterimide enameled wires improved heat resistance by modifying polyester with imide, further expanding the application range of enameled wires; subsequently, enameled wires prepared from various materials such as polyimide enameled wires, polyamide enameled wires, and composite coated enameled wires were improved in different ways, improving the performance of enameled wires in all aspects.

[0004] Chinese patent publication number CN117327446 discloses a polyimide wire enamel and a preparation method thereof. The preparation method of the polyimide wire enamel comprises: mixing a volatile acid with a diamine, a dianhydride and a solvent and reacting to obtain the polyimide wire enamel. The preparation method adds an acid to the reaction system to inhibit the reaction of the acid anhydride with water, so that the acid anhydride can react with the amine first, thereby reducing the requirement of the reaction system for water content, greatly reducing the production cost, and the addition of the acid does not affect the reaction process of the diamine and the dianhydride, ensuring that the product has good film-forming properties.

[0005] Chinese patent publication number CN111234693 discloses a self-lubricating polyimide wire enamel and a preparation method thereof, comprising component A and component B, wherein component A is a polyamic acid solution, accounting for 90wt%-98wt% of the total mass of the lacquer liquid; component B is a blend of stearic acid, glycidyl ether propyl trimethoxy silane and tung oil anhydride in a mass ratio of 1:1-3:0.1-0.8, accounting for 2wt%-10wt% of the total mass of the lacquer liquid. At room temperature, component A and component B are uniformly mixed to obtain the self-lubricating polyimide wire enamel.

[0006] With the needs of social development, the requirements for the performance of enameled wires are becoming higher and higher. The corona resistance and mechanical strength of the enameled wires in the above-mentioned patented technical solution need to be improved. Summary of the invention

[0007] In order to overcome the above problems of the prior art, the present invention provides a polyimide high-strength corona-resistant frequency conversion enameled copper flat wire and a preparation method thereof. The enameled copper flat wire prepared by the present invention has both excellent corona resistance and mechanical strength.

[0008] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:

[0009] A method for preparing a polyimide high-strength corona-resistant frequency-conversion enameled copper flat wire comprises the following steps:

[0010] S1, preparation of modified silica nanoparticles;

[0011] S2, blending the modified silica nanoparticles with a polyimide insulating resin solution to obtain a wire enamel;

[0012] S3, coating the wire enamel on the surface of the copper flat wire, and baking and curing the wire.

[0013] Preferably, the method for preparing the modified silica nanoparticles comprises the following steps:

[0014] S11, adding silicon dioxide to a mixed solution of ethanol and water, stirring and mixing evenly, then adding an epoxy silane coupling agent, heating to react, and obtaining coupling agent-modified silicon dioxide through separation;

[0015] S12, adding the coupling agent modified silica into the hyperbranched polyethyleneimine solution, heating to 80° C., stirring and reacting for 3 hours, and separating to obtain modified silica nanoparticles.

[0016] In the technical solution of the present invention, in order to improve the corona resistance of the enameled copper flat wire, the present invention dopes silicon dioxide nanoparticles in the polyimide resin, and the silicon dioxide nanoparticles are inorganic insulating nanoparticles, which can effectively improve the corona resistance of the enameled copper flat wire. However, there is a problem that the silicon dioxide nanoparticles are easy to agglomerate in the polyimide resin material, which affects the improvement effect of nano silicon dioxide on the corona resistance of the enameled copper flat wire. Therefore, the present invention further modifies the silicon dioxide nanoparticles, uses a silane coupling agent to perform organic modification on the surface of the nano silicon dioxide, prevents the silicon dioxide nanoparticles from agglomerating, and the silicon dioxide nanoparticles can be effectively dispersed in the polyimide resin material, thereby improving the improvement effect of nano silicon dioxide on the corona resistance of the enameled copper flat wire.

[0017] In order to improve the mechanical strength of the enameled copper flat wire, the present invention further modifies the coupling agent-modified silica, utilizes the epoxy groups on the epoxy silane coupling agent molecules to react with the amino groups on the hyperbranched polyethyleneimine to generate a ring-opening reaction, thereby grafting the hyperbranched polyethyleneimine onto the surface of the silica, utilizes the numerous branched structures of the hyperbranched polyethyleneimine to be interlaced and interspersed in the polyimide resin, thereby forming a dendrite-like skeleton reinforcement structure, thereby significantly improving the mechanical strength of the enameled copper flat wire.

[0018] Preferably, in step S11, the mass ratio of silica to epoxy silane coupling agent is 1:0.2-0.5. Preferably, in step S12, the mass ratio of coupling agent-modified silica to hyperbranched polyethyleneimine is ≤1:0.4.

[0019] In order to ensure the improvement effect of hyperbranched polyethyleneimine on the mechanical strength of the polyimide enameled wire, the mass ratio of the coupling agent modified silica to the hyperbranched polyethyleneimine is controlled to be less than or equal to 1:0.4. Within this range, a sufficient amount of hyperbranched polyethyleneimine molecules are grafted on the surface of the silica nanoparticles, thereby significantly enhancing the mechanical strength of the polyimide enameled wire.

[0020] Preferably, in step S12, the mass ratio of the coupling agent-modified silica to the hyperbranched polyethyleneimine is ≥1:0.6.

[0021] In the technical solution of the present invention, as described above, hyperbranched polyethyleneimine is grafted onto the surface of silica particles to improve the mechanical strength of the enameled copper flat wire. However, experimental studies have found that hyperbranched polyethyleneimine has a negative effect on the corona resistance of the enameled copper flat wire, reducing the corona resistance of the enameled copper flat wire. In order to solve this problem, the present invention controls the mass ratio of coupling agent modified silica to hyperbranched polyethyleneimine to be ≥1:0.6. Experimental studies have found that within this range, hyperbranched polyethyleneimine will not have a significant effect on the corona resistance of the enameled copper flat wire. Therefore, the present invention strictly controls the mass ratio of coupling agent modified silica to hyperbranched polyethyleneimine to be ≥1:0.6.

[0022] Preferably, the mass ratio of the aromatic polyimide to the modified silica nanoparticles is 1:0.03-0.08. Preferably, in step S3, the baking curing temperature is 310-330°C.

[0023] A polyimide high-strength corona-resistant frequency-conversion enameled copper rectangular wire is prepared by the method described above.

[0024] The present invention has the following beneficial effects:

[0025] 1) Doping silicon dioxide nanoparticles in polyimide resin. Silica nanoparticles are inorganic insulating nanoparticles that can effectively improve the corona resistance of enameled copper flat wire;

[0026] 2) Using a silane coupling agent to perform organic modification on the surface of nano-silicon dioxide to prevent the agglomeration of the silicon dioxide nanoparticles, the silicon dioxide nanoparticles can be effectively dispersed in the polyimide resin material, thereby improving the effect of nano-silicon dioxide on the corona resistance of the enameled copper flat wire;

[0027] 3) The numerous branched structures of hyperbranched polyethyleneimine are interlaced and interspersed in the polyimide resin to form a tree-like skeleton reinforcement structure, which significantly improves the mechanical strength of the enameled copper flat wire. DETAILED DESCRIPTION

[0028] The present invention is further described in detail below in conjunction with specific embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.

[0029] Unless otherwise specified, the raw materials used in the examples of the present invention are all commercially available or available to those skilled in the art; unless otherwise specified, the methods used in the examples of the present invention are all methods known to those skilled in the art.

[0030] Example 1

[0031] A method for preparing a polyimide high-strength corona-resistant frequency-conversion enameled copper flat wire comprises the following steps:

[0032] S1, preparation of modified silica nanoparticles;

[0033] S2, adding a polyimide resin having a solid content of 30 wt% to an organic solvent of cresol and anhydrous ethanol in a volume ratio of 5:3 at a mass volume ratio of 1 g / 300 mL, stirring and dissolving, to obtain a polyimide insulating resin solution; blending modified silica nanoparticles with the polyimide insulating resin solution, wherein the mass ratio of polyimide to modified silica nanoparticles is 1:0.07, to obtain a wire enamel;

[0034] S3, coating the wire enamel on the surface of the copper flat wire, and baking and curing the wire, wherein the baking and curing temperature is 330° C., to obtain the product.

[0035] Preparation of modified silica nanoparticles:

[0036] S11, ethanol and water are mixed in a ratio of 10:1 to form a mixed solution, 2 g of silica is added to the mixed solution of 300 mL of ethanol and water, and the mixture is stirred and mixed evenly, and then epoxy silane coupling agent KH-560 is added, and the mass ratio of silica to epoxy silane coupling agent is 1:0.4, and the mixture is heated to 50° C. and stirred for reaction for 3 hours, and coupling agent-modified silica is obtained after separation;

[0037] S12, adding 1.5 g of hyperbranched polyethyleneimine into 500 mL of deionized water, stirring to dissolve, forming a hyperbranched polyethyleneimine solution, adding coupling agent modified silica to the hyperbranched polyethyleneimine solution, the mass ratio of coupling agent modified silica to hyperbranched polyethyleneimine is 1:0.5, heating to 80°C, stirring to react for 3 hours, and separating to obtain modified silica nanoparticles.

[0038] Example 2

[0039] A method for preparing a polyimide high-strength corona-resistant frequency-conversion enameled copper flat wire comprises the following steps:

[0040] S1, preparation of modified silica nanoparticles;

[0041] S2, adding a polyimide resin having a solid content of 30 wt% to an organic solvent of cresol and anhydrous ethanol in a volume ratio of 5:3 at a mass volume ratio of 1 g / 300 mL, stirring and dissolving, to obtain a polyimide insulating resin solution; blending modified silica nanoparticles with the polyimide insulating resin solution, wherein the mass ratio of polyimide to modified silica nanoparticles is 1:0.04, to obtain a wire enamel;

[0042] S3, coating the wire enamel on the surface of the copper flat wire, and baking and curing the wire, wherein the baking and curing temperature is 310° C., to obtain the product.

[0043] Preparation of modified silica nanoparticles:

[0044] S11, ethanol and water are mixed in a ratio of 10:1 to form a mixed solution, 2 g of silica is added to the mixed solution of 300 mL of ethanol and water, and the mixture is stirred and mixed evenly, and then epoxy silane coupling agent KH-560 is added, and the mass ratio of silica to epoxy silane coupling agent is 1:0.25, and the mixture is heated to 50° C. and stirred for reaction for 3 h, and coupling agent-modified silica is obtained after separation;

[0045] S12, adding 1.5 g of hyperbranched polyethyleneimine into 500 mL of deionized water, stirring to dissolve, forming a hyperbranched polyethyleneimine solution, adding coupling agent modified silica to the hyperbranched polyethyleneimine solution, the mass ratio of coupling agent modified silica to hyperbranched polyethyleneimine is 1:0.45, heating to 80°C, stirring to react for 3 hours, and separating to obtain modified silica nanoparticles.

[0046] Example 3

[0047] A method for preparing a polyimide high-strength corona-resistant frequency-conversion enameled copper flat wire comprises the following steps:

[0048] S1, preparation of modified silica nanoparticles;

[0049] S2, adding a polyimide resin having a solid content of 30 wt% to an organic solvent of cresol and anhydrous ethanol in a volume ratio of 5:3 at a mass volume ratio of 1 g / 300 mL, stirring and dissolving, to obtain a polyimide insulating resin solution; blending modified silica nanoparticles with the polyimide insulating resin solution, wherein the mass ratio of polyimide to modified silica nanoparticles is 1:0.05, to obtain a wire enamel;

[0050] S3, coating the wire enamel on the surface of the copper flat wire, and baking and curing the wire, wherein the baking and curing temperature is 320° C., to obtain the product.

[0051] Preparation of modified silica nanoparticles:

[0052] S11, ethanol and water are mixed in a ratio of 10:1 to form a mixed solution, 2 g of silica is added to the mixed solution of 300 mL of ethanol and water, and the mixture is stirred and mixed evenly, and then epoxy silane coupling agent KH-560 is added, the mass ratio of silica to epoxy silane coupling agent is 1:0.35, and the mixture is heated to 50° C. and stirred for reaction for 3 h, and coupling agent-modified silica is obtained after separation;

[0053] S12, adding 1.5 g of hyperbranched polyethyleneimine into 500 mL of deionized water, stirring to dissolve, forming a hyperbranched polyethyleneimine solution, adding coupling agent modified silica to the hyperbranched polyethyleneimine solution, the mass ratio of coupling agent modified silica to hyperbranched polyethyleneimine is 1:0.48, heating to 80°C, stirring to react for 3 hours, and separating to obtain modified silica nanoparticles.

[0054] Example 4

[0055] A method for preparing a polyimide high-strength corona-resistant frequency-conversion enameled copper flat wire comprises the following steps:

[0056] S1, preparation of modified silica nanoparticles;

[0057] S2, adding a polyimide resin having a solid content of 30 wt% to an organic solvent of cresol and anhydrous ethanol in a volume ratio of 5:3 at a mass volume ratio of 1 g / 300 mL, stirring and dissolving, to obtain a polyimide insulating resin solution; blending modified silica nanoparticles with the polyimide insulating resin solution, wherein the mass ratio of polyimide to modified silica nanoparticles is 1:0.08, to obtain a wire enamel;

[0058] S3, coating the wire enamel on the surface of the copper flat wire, and baking and curing the wire, wherein the baking and curing temperature is 330° C., to obtain the product.

[0059] Preparation of modified silica nanoparticles:

[0060] S11, ethanol and water are mixed in a ratio of 10:1 to form a mixed solution, 2 g of silica is added to the mixed solution of 300 mL of ethanol and water, and the mixture is stirred and mixed evenly, and then epoxy silane coupling agent KH-560 is added, and the mass ratio of silica to epoxy silane coupling agent is 1:0.5, and the mixture is heated to 50° C. and stirred for reaction for 3 h, and coupling agent-modified silica is obtained after separation;

[0061] S12, adding 1.5 g of hyperbranched polyethyleneimine into 500 mL of deionized water, stirring to dissolve, forming a hyperbranched polyethyleneimine solution, adding coupling agent modified silica to the hyperbranched polyethyleneimine solution, the mass ratio of coupling agent modified silica to hyperbranched polyethyleneimine is 1:0.6, heating to 80°C, stirring to react for 3 hours, and separating to obtain modified silica nanoparticles.

[0062] Example 5

[0063] A method for preparing a polyimide high-strength corona-resistant frequency-conversion enameled copper flat wire comprises the following steps:

[0064] S1, preparation of modified silica nanoparticles;

[0065] S2, adding a polyimide resin having a solid content of 30 wt% to an organic solvent of cresol and anhydrous ethanol in a volume ratio of 5:3 at a mass volume ratio of 1 g / 300 mL, stirring and dissolving, to obtain a polyimide insulating resin solution; blending modified silica nanoparticles with the polyimide insulating resin solution, wherein the mass ratio of polyimide to modified silica nanoparticles is 1:0.03, to obtain a wire enamel;

[0066] S3, coating the wire enamel on the surface of the copper flat wire, and baking and curing the wire, wherein the baking and curing temperature is 310° C., to obtain the product.

[0067] Preparation of modified silica nanoparticles:

[0068] S11, ethanol and water are mixed in a ratio of 10:1 to form a mixed solution, 2 g of silica is added to the mixed solution of 300 mL of ethanol and water, and the mixture is stirred and mixed evenly, and then epoxy silane coupling agent KH-560 is added, the mass ratio of silica to epoxy silane coupling agent is 1:0.2, and the mixture is heated to 50° C. and stirred for reaction for 3 h, and coupling agent-modified silica is obtained after separation;

[0069] S12, adding 1.5 g of hyperbranched polyethyleneimine into 500 mL of deionized water, stirring to dissolve, forming a hyperbranched polyethyleneimine solution, adding coupling agent modified silica to the hyperbranched polyethyleneimine solution, the mass ratio of coupling agent modified silica to hyperbranched polyethyleneimine is 1:0.4, heating to 80°C, stirring to react for 3 hours, and separating to obtain modified silica nanoparticles.

[0070] Comparative Example 1

[0071] The difference between Comparative Example 1 and Example 1 is that:

[0072] The modified silica nanoparticles were replaced with ordinary silica nanoparticles.

[0073] The remaining steps are the same as those in Example 1.

[0074] Comparative Example 2

[0075] The difference between Comparative Example 2 and Example 1 is:

[0076] The S12 step is omitted in the preparation process of modified silica nanoparticles.

[0077] The remaining steps are the same as those in Example 1.

[0078] Comparative Example 3

[0079] The difference between Comparative Example 3 and Example 4 is that:

[0080] The mass ratio of coupling agent modified silica to hyperbranched polyethyleneimine is 1:0.7.

[0081] The remaining steps are the same as those in Example 4.

[0082] Comparative Example 4

[0083] The difference between Comparative Example 4 and Example 4 is that:

[0084] The mass ratio of coupling agent modified silica to hyperbranched polyethyleneimine is 1:0.8.

[0085] The remaining steps are the same as those in Example 4.

[0086] Performance Testing

[0087] 1. Mechanical strength test: Test the scratch resistance of the enameled wire paint film in accordance with GB / T4074.3-2008. The specific steps are: fix the sample on the tester, ensure that the sample is straightened and in good contact with the workbench, load the weight and enter the weight value, and the paint scraping device applies gradually increasing pressure to the sample until the paint film is scratched, and record the scratching force when the paint film is scratched.

[0088] 2. Corona resistance test: Place the enameled wire in an ambient temperature of 155°C, apply a voltage of 1500Vp to the surface of the enameled wire at a frequency of 50Hz, and the time it takes for the surface to break down and cause a short circuit is the corona resistance time of the enameled wire.

[0089]

[0090] The above are only preferred embodiments of the present invention. It should be noted that the above preferred embodiments should not be regarded as limiting the present invention, and the protection scope of the present invention should be based on the scope defined by the claims. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the spirit and scope of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.

Claims

1. A method for preparing a polyimide high-strength corona-resistant frequency-converting enameled copper rectangular wire, characterized in that: The following steps are involved: S1, preparation of modified silica nanoparticles; S2, blending the modified silica nanoparticles with a polyimide insulating resin solution to obtain a wire enamel; S3, coating the wire enamel on the surface of the copper flat wire, and baking and curing the wire.

2. The method for preparing a polyimide high-strength corona-resistant frequency conversion enameled copper rectangular wire according to claim 1, characterized in that: The preparation method of the modified silicon dioxide nanoparticles comprises the following steps: S11, adding silicon dioxide to a mixed solution of ethanol and water, stirring and mixing evenly, then adding an epoxy silane coupling agent, heating to react, and obtaining coupling agent-modified silicon dioxide through separation; S12, adding the coupling agent modified silica into the hyperbranched polyethyleneimine solution, heating to 80° C., stirring and reacting for 3 hours, and separating to obtain modified silica nanoparticles.

3. The method for preparing a polyimide high-strength corona-resistant frequency conversion enameled copper rectangular wire according to claim 2, characterized in that: In the step S11, the mass ratio of silicon dioxide to epoxy silane coupling agent is 1:0.2-0.

5.

4. The method for preparing a polyimide high-strength corona-resistant frequency conversion enameled copper rectangular wire according to claim 2, characterized in that: In the step S12, the mass ratio of the coupling agent modified silica to the hyperbranched polyethyleneimine is ≤1:0.

4.

5. The method for preparing a polyimide high-strength corona-resistant frequency conversion enameled copper rectangular wire according to claim 2, characterized in that: In the step S12, the mass ratio of the coupling agent modified silica to the hyperbranched polyethyleneimine is ≥1:0.

6.

6. The method for preparing a polyimide high-strength corona-resistant frequency conversion enameled copper rectangular wire according to claim 1, characterized in that: The mass ratio of the polyimide to the modified silicon dioxide nanoparticles is 1:0.03-0.

08.

7. The method for preparing a polyimide high-strength corona-resistant frequency conversion enameled copper rectangular wire according to claim 1, characterized in that: In the step S3, the curing temperature is 310-330°C.

8. A polyimide high-strength corona-resistant frequency conversion enameled copper rectangular wire, characterized in that: The method is prepared by any one of claims 1 to 7.

Citation Information

Patent Citations

  • Enameled wire containing nanometer stuffing

    CN101604562A

  • Preparation method for nanometer mesoporous particle modified corona resistance wire enamel

    CN102732147A

  • Fingerprint-resistant environmental-protection water-borne paint and preparation method thereof

    CN109207035A

  • Corona-resistant enameled wire for motor, preparation method of corona-resistant enameled wire and flat wire motor

    CN114724744A

  • Water-based paint based on epoxy resin emulsion modification and preparation process thereof

    CN116162390A