Method for improving magnetic performance of SmCo5 material
By adding high-purity Cu powder to SmCo5 magnetic powder and performing vacuum annealing, the problem of powder agglomeration in the traditional annealing process was solved, the magnetic properties of SmCo5 material were improved and the production cost was reduced.
Patent Information
- Application Number
- CN202310547400.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-16
- Publication Date
- 2024-11-22
AI Technical Summary
Traditional annealing processes cause SmCo5 materials to agglomerate at high temperatures, affecting the orientation of magnetic powder particles, reducing the magnetic properties of bonded magnets, and also increasing costs.
Add up to 5 wt% of high-purity Cu powder to SmCo5 magnetic powder, and perform high-energy ball milling in an Ar atmosphere. Then, perform vacuum annealing with the annealing temperature reduced to 500-650℃ to avoid powder agglomeration.
It effectively improves the coercivity and remanent magnetization of SmCo5 materials, reduces production costs, avoids powder agglomeration, and enhances magnetic properties.
Smart Images

Figure CN119008157A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rare earth permanent magnetic material preparation, in particular to a method for improving the magnetic properties of SmCo5 material. Background Art
[0002] With the advancement of science and technology and the development of industry, magnetic materials, as a very important functional material, are widely used in medical, energy, automobile and communication fields. As a major country in the research and development and production of electric vehicles, magnetic materials are the key parts of electric vehicle generators, which are crucial to the high integration and lightweight of electric vehicles. In order to meet the increasing requirements of industrial applications, the performance and production process of magnetic materials have always received much attention.
[0003] SmCo5 material is a high-performance rare earth permanent magnetic material with advantages such as wide range of raw materials, low price and high cost performance. As one of the highest-yield permanent magnetic materials, it is widely used in many fields. According to the different molding of SmCo5 material magnetic powder, its application can be mainly divided into bonded magnets and sintered magnets. Among them, bonded magnets have the advantages of low production cost and good plasticity, and are widely used in many industrial fields as bonded magnets. The production process of bonded magnets mainly includes pretreatment, mixing, high-temperature pre-sintering, crushing, annealing and molding. For example, the Chinese invention patent with authorization number CN1145538C carried out annealing heat treatment at 900℃×3 hours, and after quenching and rapid cooling, anisotropic bonded magnets were made by bonding method. The intrinsic properties of bonded magnet powder largely determine the magnetic properties of the bonded magnet produced in the end, and the essential properties of the magnetic powder in the general bonded magnet production process are basically consistent with the properties of the magnetic powder after annealing. The magnetic powder that has been pre-burned at high temperature will produce a large number of lattice defects during the crushing process, which will reduce the magnetic properties of the magnetic powder. The annealing step after crushing is to eliminate the lattice defects and restore the magnetic properties of the magnetic powder. The traditional annealing process requires a higher annealing temperature (850-950℃) to restore the magnetic properties of the magnetic powder, which greatly increases the production cost of bonded magnets and easily causes the magnetic powder to agglomerate during the annealing process. If the annealing temperature is too low, the lattice defects of the magnetic powder may not be completely eliminated, thereby failing to achieve the effect of improving the magnetic properties of the magnetic powder.
[0004] In addition, the traditional annealing process easily causes the magnetic powder to agglomerate, which will prevent the magnetic powder particles from preferentially orienting along the magnetic field direction during the subsequent molding process, thus reducing the orientation degree of the magnetic powder particles in the resulting bonded magnet and failing to effectively improve the magnetic properties of the molded magnet. Therefore, it is necessary to find a suitable annealing temperature and use modification methods to effectively restore the magnetic properties of the magnetic powder. Summary of the invention
[0005] In order to solve the problems of the prior art, the purpose of the present invention is to overcome the shortcomings of the existing technology and provide a method for improving the magnetic properties of SmCo5 materials. Compared with traditional SmCo5 materials, the annealing temperature is greatly reduced, which effectively prevents the agglomeration of powders annealed at high temperatures from affecting the orientation of magnetic particles, and improves the comprehensive magnetic properties of SmCo5 materials.
[0006] To achieve the above purpose, the specific technical solutions of the present invention are as follows:
[0007] A method for improving the magnetic properties of SmCo5 material comprises the following steps:
[0008] S1. Select SmCo5 magnetic powder and high purity Cu powder;
[0009] S2, the SmCo5 magnetic powder and the Cu powder are prepared in a mass ratio of 95-100:5-0, and preliminarily mixed to obtain a primary mixture;
[0010] S3, ball milling the primary mixed material in an Ar gas environment;
[0011] S4, after the ball milling treatment is completed, the material in the ball mill tank is taken out under an Ar gas environment to obtain a ball milled mixed material;
[0012] S5, placing the ball-milled mixture into a quartz glass tube with a bottom sealed at one end under an Ar gas environment, and then vacuum-sealing the tube to obtain a vacuum-sealed glass tube;
[0013] S6, annealing the vacuum sealed glass tube, and obtaining the annealed SmCo5 material after the annealing is completed.
[0014] Preferably, in the step S1, the particle size of the SmCo5 magnetic powder is 0.1-50 μm, and the purity of the high-purity Cu powder is 99.85% and the particle size is 1-75 μm.
[0015] Preferably, in the S3 step, the primary mixture and steel balls are placed in a ball mill in an Ar gas glove box, the steel balls have a diameter of 9 mm, and the ball-to-material ratio is 25:1. The ball mill is then tightened, and the ball mill is taken out of the glove box and finally placed in a high-energy ball mill for ball milling.
[0016] Further preferably, in the step S3, the parameters of the ball milling treatment are 1725 rotation speed and 3 hours.
[0017] Preferably, in the step S5, after the ball-milled mixture is loaded into the quartz glass tube, vacuuming and sealing are performed, and the vacuum degree in the quartz glass tube is 2×10 -4 Pa.
[0018] Preferably, in the step S6, the annealing procedure of the annealing treatment is: heating to an annealing temperature of 500-650°C at a heating rate of 25°C / min, keeping warm at the annealing temperature, taking out the vacuum-sealed glass tube, and naturally cooling to room temperature.
[0019] Further preferably, the annealing temperature is maintained for 30 minutes.
[0020] The SmCo5 material prepared by the above method for improving the magnetic properties of the SmCo5 material has a coercive force of 19.7 to 34.2 kOe.
[0021] Preferably, the SmCo5 material prepared by the above method for improving the magnetic properties of SmCo5 material has a residual magnetization intensity of 52.5 to 75.8 emu / g.
[0022] Preferably, the maximum magnetic energy product of the SmCo5 material prepared by the above method for improving the magnetic properties of the SmCo5 material is 7.9 to 15.9 MGOe.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] The present invention provides a method for improving the magnetic properties of SmCo5 material, by adding less than 5wt% of high-purity Cu powder into SmCo5 magnetic powder, performing high-energy ball milling treatment in an Ar gas environment, and then performing vacuum annealing treatment, wherein the annealing temperature is much lower than the annealing temperature used in the traditional SmCo5 material annealing process, thereby avoiding the occurrence of powder agglomeration.
[0025] The present invention provides a method for improving the magnetic properties of SmCo5 material. By using high-purity Cu powder to replace part of the SmCo5 magnetic powder, the cost is saved. Under the condition of a small decrease in residual magnetization intensity and maximum magnetic energy product, the increase in coercive force can reach 31%, effectively improving the comprehensive magnetic properties of the SmCo5 material. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 : is the demagnetization curve of the SmCo5 material prepared in Examples 1 to 4 of the present invention;
[0027] Figure 2 : is the demagnetization curve of the SmCo5 material prepared in Examples 5 to 8 of the present invention;
[0028] Figure 3 : is the demagnetization curve of the SmCo5 material prepared in Examples 9 to 12 of the present invention;
[0029] Figure 4 1 is the demagnetization curve of the SmCo5 material prepared in Examples 13 to 16 of the present invention;
[0030] Figure 5 These are TEM images of the SmCo5 materials prepared in Examples 11 and 14 of the present invention, where (a) is Example 11 and (b) is Example 14. DETAILED DESCRIPTION
[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] For ease of understanding, the nouns and abbreviations mentioned below are first explained:
[0033] SmCo5: Samarium cobalt, cobalt-samarium alloy, purchased from AlfaAesar.
[0034] Remanence: Short for residual magnetization.
[0035] The present invention provides an embodiment of a method for improving the magnetic properties of SmCo5 material, comprising the following seven steps:
[0036] S1. Select SmCo5 magnetic powder and high purity Cu powder;
[0037] S2, SmCo5 magnetic powder and Cu powder are prepared according to the mass ratio shown in Table 1, and preliminarily mixed to obtain a primary mixture;
[0038] S3, weighing 4 g of the primary mixed material and subjecting it to ball milling in an Ar gas environment;
[0039] S4, after the ball milling treatment is completed, the material in the ball mill tank is taken out under an Ar gas environment to obtain a ball milled mixed material;
[0040] S5. Under an Ar gas environment, weigh 0.5 g of the ball-milled mixture and put it into a quartz glass tube with a bottom sealed at one end, and then vacuum seal the tube to obtain a vacuum-sealed glass tube;
[0041] S6. Annealing the vacuum sealed glass tube to obtain an annealed SmCo5 material.
[0042] Furthermore, the particle size of the SmCo5 magnetic powder is 0.1 to 50 μm.
[0043] Furthermore, the purity of the high-purity Cu powder is 99.85%, and the particle size is 1-75 μm.
[0044] Furthermore, in step S3, the primary mixture and steel balls are placed in a ball mill in an Ar gas glove box, the steel balls have a diameter of 9 mm, and the ball-to-material ratio (mass ratio of steel balls to primary mixture) is 25:1, and then the ball mill is tightened, and then the ball mill is taken out of the glove box, and finally placed in a high-energy ball mill for ball milling. In this way, the ball mill is filled with Ar gas, which can be used as a protective gas in the subsequent ball milling process to protect the mixed powder from oxidation.
[0045] Specifically, in step S3, the purity of the Ar gas in the glove box is 99.999%.
[0046] Specifically, in step S3, a SPEX-8000D vibrating high-energy ball mill is used for ball milling. The ball mill is shaken thoroughly before being loaded onto the machine, and the ball mill is milled according to the setting program of 1725 r / min and 3 h.
[0047] Furthermore, in step S4, the ball mill jar is removed from the high-energy ball mill and placed in an Ar gas glove box. The ball mill jar is opened under an Ar gas environment and the materials therein are collected.
[0048] Furthermore, in step S5, after the ball-milled mixture is loaded into the quartz glass tube, the glass tube is assembled on a vacuum baffle and then assembled on a vacuum tube sealing device. -4 When Pa, the pipe sealing work is completed.
[0049] Specifically, in step S5, the dimensions of the quartz glass tube are: diameter d=10 mm, side wall thickness t=1 mm, and length L=300 mm.
[0050] Furthermore, in step S6, the vacuum-sealed glass tube is placed in a box-type resistance furnace for annealing treatment, and the annealing procedure is: heating to the annealing temperature at a heating rate of 25°C / min, keeping at the annealing temperature for 30 minutes, taking out the vacuum-sealed glass tube, and naturally cooling to room temperature.
[0051] Specifically, the annealing temperature during the annealing treatment is shown in Table 1.
[0052] Table 1 Mass ratio and process parameters of SmCo5 magnetic powder and Cu powder
[0053]
[0054] The SmCo5 materials with different Cu contents after vacuum annealing obtained in Examples 1 to 16 were tested for relevant magnetic performance parameters. The magnetization curves are shown in FIG. Figures 1 to 4 The specific magnetic properties are shown in Table 2:
[0055] Table 2 Magnetic properties of SmCo5 materials with different Cu contents obtained in Examples 1 to 16
[0056]
[0057] By comparing the magnetic properties of SmCo5 materials with different Cu contents after vacuum annealing, it can be found that the addition of Cu powder and the increase of annealing temperature can effectively improve the coercivity of SmCo5 materials after annealing, and there are differences in the improvement of the magnetic properties of SmCo5 materials with the addition of different Cu contents. It is worth noting that, in Examples 9 to 12, compared with Example 9, the SmCo5 material to which 1wt% Cu powder is added in Example 10 has a coercive force of 31.7kOe, a remanence of 65.4emu / g and a maximum magnetic energy product of 12.2MGOe, a coercive force increase of 21.5%, and only a slight decrease in remanence and maximum magnetic energy product, which are 1.8% and 2.4% respectively; in Example 11, after the addition of 3wt% high-purity Cu powder, the coercive force of the SmCo5 material reaches 34.2kOe, and compared with the performance of the SmCo5 magnetic powder without Cu, the absolute value of the coercive force increase is 8.1kOe, an increase of 31%, and the remanence of the magnetic powder is only slightly decreased, with a decrease of 10.4%, which greatly improves the anti-demagnetization ability and high-temperature performance of the magnetic powder. In Examples 13 to 16, compared with Example 13, the coercivity of the SmCo5 material with 1wt% Cu added in Example 14 is 31.4kOe, and the remanence is 62.5emu / g. The addition of 1wt% high-purity Cu powder can keep the remanence of the magnetic powder only decreased by 0.4emu / g, and can also effectively improve the coercivity of the magnetic powder after annealing, with an increase of 10.2%. It shows that by optimizing the annealing temperature and time, without significantly reducing the maximum magnetic energy product, the copper-containing SmCo5 material can have a higher coercivity and better comprehensive magnetic properties.
[0058] The TEM images of the SmCo5 materials prepared in Example 11 and Example 14 are as follows: Figure 5 As shown in the figure, it can be seen that after annealing, the particles of SmCo5 material are evenly distributed and no powder agglomeration occurs.
[0059] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is limited by the attached embodiments and their equivalents.
Claims
1. A method for improving the magnetic properties of SmCo5 material, characterized in that: The following steps are involved: S1. Select SmCo5 magnetic powder and high purity Cu powder; S2, the SmCo5 magnetic powder and the Cu powder are prepared in a mass ratio of 95-100:5-0, and preliminarily mixed to obtain a primary mixture; S3, ball milling the primary mixed material in an Ar gas environment; S4, after the ball milling treatment is completed, the material in the ball mill tank is taken out under an Ar gas environment to obtain a ball milled mixed material; S5, placing the ball-milled mixture into a quartz glass tube with a bottom sealed at one end under an Ar gas environment, and then vacuum-sealing the tube to obtain a vacuum-sealed glass tube; S6, annealing the vacuum sealed glass tube, and obtaining the annealed SmCo5 material after the annealing is completed.
2. The method for improving the magnetic properties of SmCo5 material according to claim 1, characterized in that: In the step S1, the particle size of the SmCo5 magnetic powder is 0.1-50 μm, the purity of the high-purity Cu powder is 99.85%, and the particle size is 1-75 μm.
3. The method for improving the magnetic properties of SmCo5 material according to claim 1, characterized in that: In the S3 step, the primary mixed material and steel balls are placed in a ball mill in an Ar gas glove box, the steel balls have a diameter of 9 mm, and the ball-to-material ratio is 25:
1. The ball mill is then tightened, and the ball mill is taken out of the glove box and finally placed in a high-energy ball mill for the ball milling treatment.
4. The method for improving the magnetic properties of SmCo5 material according to claim 3, characterized in that: In the step S3, the parameters of the ball milling treatment are 1725 r / min and 3 h.
5. The method for improving the magnetic properties of SmCo5 material according to claim 1, characterized in that: In the step S5, after the ball-milled mixture is loaded into the quartz glass tube, vacuumization and tube sealing are performed, and the vacuum degree in the quartz glass tube is 2×10 -4 Pa.
6. The method for improving the magnetic properties of SmCo5 material according to claim 1, characterized in that: In the step S6, the annealing procedure of the annealing treatment is: heating to an annealing temperature of 500-650°C at a heating rate of 25°C / min, keeping the temperature at the annealing temperature, taking out the vacuum-sealed glass tube, and naturally cooling it to room temperature.
7. The method for improving the magnetic properties of SmCo5 material according to claim 6, characterized in that: The annealing temperature is maintained for 30 min.
8. A SmCo5 material, prepared by the method for improving the magnetic properties of SmCo5 material according to any one of claims 1 to 7, characterized in that: The SmCo5 material has a coercive force of 19.7 to 34.2 kOe.
9. The SmCo5 material according to claim 8, characterized in that The SmCo5 material has a residual magnetization intensity of 52.5 to 75.8 emu / g.
10. The SmCo5 material according to claim 8, characterized in that The maximum magnetic energy product of the SmCo5 material is 7.9 to 15.9 MGOe.
Citation Information
Patent Citations
Fast quenching method for preparing anisotropic permanent-magnet SmCo5 material
CN1145538C