Iron-based nanocrystalline soft magnetic alloy and preparation method and application thereof

By optimizing the formulation and heat treatment process of iron-based nanocrystal soft magnetic alloy, the problem that the saturated magnetic induction strength and permeability of iron-based nanocrystal soft magnetic alloy in the current transformer cannot meet the requirements at the same time, and high initial magnetic conductivity is achieved The combination of rate and saturated magnetic induction strength improves the stability and temperature stability of the transformer.

CN119008161APending Publication Date: 2024-11-22HENAN XJ INSTR
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411229391.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The saturated magnetic induction strength and permeability of iron-based nanocrystalline soft magnetic alloy cannot meet the requirements of the current transformer at the same time, resulting in a narrow measurement range and poor operating stability of the transformer.

Method used

Through the optimized formulation design, the chemical composition of the iron-based nanocrystalline soft magnetic alloy is Si 6.8~7.2%, B 2.2~2.8%, Cu 1.2~1.8%, Nb 5.7~6.3%, Fe 81.9~84.1%, and heat treatment and The transverse magnetic field treatment improves the initial magnetic permeability and saturated magnetic induction strength while reducing the residual magnetic induction strength.

Benefits of technology

The high initial magnetic permeability and saturated magnetic induction strength of iron-based nanocrystalline soft magnetic alloy are achieved, which reduces the residual magnetic induction strength of the iron core, improves the operating stability and temperature stability of the transformer, and reduces error fluctuations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008161A_ABST
    Figure CN119008161A_ABST
Patent Text Reader

Abstract

The invention relates to an iron-based nanocrystalline soft magnetic alloy and a preparation method and application thereof, and belongs to the technical field of magnetic alloy materials. According to the magnetic core made of the iron-based nanocrystalline soft magnetic alloy, the initial relative permeability mu i is about 300000, the saturation flux density Bs is about 1.2 T, and the residual flux density is about 0.28 T; the initial magnetic conductivity of the magnetic core has a temperature coefficient of about + 0.06% / DEG C at a general use environment temperature of-40 DEG C to 70 DEG C. By adjusting the formula and the treatment process of the iron-based nanocrystalline magnetically soft alloy, the initial permeability is improved while the saturation flux density of the material is not reduced, and the residual magnetic flux density of the iron core can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an iron-based nanocrystalline soft magnetic alloy and a preparation method and application thereof, belonging to the technical field of magnetic alloy materials. Background Art

[0002] The accuracy and measurement limit of the standard current transformer are mainly determined by the core material performance and excitation current of the transformer. The initial magnetic permeability of the core material determines the excitation current of the transformer coil winding. The higher the initial magnetic permeability, the smaller the excitation current. However, the saturation magnetic induction intensity of the core with high initial magnetic permeability is relatively low. The low saturation magnetic induction intensity of the core will narrow the measurement range of the current transformer. Therefore, the two parameters of initial magnetic permeability and saturation magnetic induction intensity are both interrelated and contradictory. The residual magnetic induction intensity of the core material affects the operating stability of the transformer. When residual magnetism is generated in the core during operation, the excitation current will increase and the error characteristics will deteriorate. Therefore, the smaller the residual magnetic induction intensity of the core material, the better the operating stability of the transformer.

[0003] Iron-based nanocrystalline alloys have excellent soft magnetic properties such as high magnetic permeability, low coercivity, high electrical conductivity, and low loss. They have good application prospects in many soft magnetic electronic devices such as mutual inductors, transformers, switching power supplies, and motors. The preparation method of iron-based nanocrystalline alloys is as follows: using a smelting process, mainly iron elements, adding an alloy composed of a small amount of Nb, Cu, Si, and B elements, and obtaining an amorphous material through a rapid solidification process, and then obtaining a microcrystalline and nanocrystalline material with a diameter of 10 to 20 nm dispersed on the matrix through heat treatment, which is an iron-based nanocrystalline alloy. For example, Chinese patent document CN117637282A discloses a method for preparing an iron-based nanocrystalline soft magnetic alloy. The method for preparing an iron-based nanocrystalline soft magnetic alloy disclosed in the patent document specifically includes the following steps: S1, placing the prepared raw materials into a vacuum induction furnace for uniform melting, and then pouring them into a cooling casting plate to form a master alloy; S2, placing the master alloy in step S1 into a medium-frequency induction melting furnace of a spray belt equipment for secondary uniform melting, and adding a slag remover after the master alloy is completely melted into molten steel; S3, introducing the molten steel in step S2 into a tundish, and spraying it through the slit of the nozzle onto a copper roller rotating at a high speed of 25m / s to form a continuous amorphous strip with a width of 33-34mm and a thickness of 20-24μm; S4, subjecting the continuous amorphous strip in step S3 to heat treatment, during which a transverse magnetic field is applied.

[0004] Chinese patent document CN117888028A discloses an iron-based nanocrystalline soft magnetic material, which is composed of the following components: Si7.7%, B 2.0%, Cu 1.3%, Nb 5.6%, Fe balance, but the patent document does not provide relevant performance test results of the iron-based nanocrystalline soft magnetic material.

[0005] Chinese patent document CN114914049A discloses an ultra-fine crystal iron core with stable performance for current transformers, and the ultra-fine crystal iron core disclosed in the patent document includes the following chemical components in weight percentage: Nb 2.8-3.8%, B 8.2-10.0%, Si 11.5-14.0%, Cu 0.81-1.5%, and the balance is Fe and inevitable impurities. Chinese patent document CN113990597A discloses a high initial magnetic permeability amorphous nanocrystalline alloy, and the high initial magnetic permeability amorphous nanocrystalline alloy disclosed in the patent document is composed of the following elements in weight percentage: Si: 7%-10%, B: 1.5%-2.5%, Nb: 5.0%-6.0%, Cu: 1.0-1.5%, inevitable impurities <0.1%, and the balance is Fe. Although the iron-based nanocrystalline soft magnetic alloy disclosed in the above document has a high saturation magnetic induction intensity or a high initial magnetic permeability, it is impossible to make the saturation magnetic induction intensity and the magnetic permeability meet the use requirements of the current transformer at the same time. Summary of the invention

[0006] The purpose of the present invention is to provide an iron-based nanocrystalline soft magnetic alloy, which can solve the problem that the saturation magnetic induction intensity and magnetic permeability of the current iron-based nanocrystalline soft magnetic alloy cannot simultaneously meet the use requirements of the current transformer.

[0007] The second object of the present invention is to provide a method for preparing an iron-based nanocrystalline soft magnetic alloy, which can solve the problem that the saturation magnetic induction intensity and magnetic permeability of the currently prepared iron-based nanocrystalline soft magnetic alloy cannot simultaneously meet the use requirements of the current transformer.

[0008] The third purpose of the present invention is to provide an application of an iron-based nanocrystalline soft magnetic alloy as a magnetic core material, which can solve the problem that the saturation magnetic induction intensity and magnetic permeability of the current iron-based nanocrystalline soft magnetic alloy cannot simultaneously meet the use requirements when used as a magnetic core material.

[0009] In order to achieve the above objectives, the technical solution adopted by the iron-based nanocrystalline soft magnetic alloy of the present invention is:

[0010] An iron-based nanocrystalline soft magnetic alloy is composed of the following elements in percentage by mass: 6.8-7.2% silicon, 2.2-2.8% boron, 1.2-1.8% copper, 5.7-6.3% niobium, and 81.9-84.1% iron.

[0011] The iron-based nanocrystalline soft magnetic alloy of the present invention is obtained by optimizing the formula design of conventional nanocrystalline materials. Compared with conventional nanocrystalline materials, the magnetic permeability of the iron-based nanocrystalline soft magnetic alloy of the present invention is further improved. The initial relative magnetic permeability μi of the magnetic core made of the iron-based nanocrystalline soft magnetic alloy of the present invention is about 300000, the saturation magnetic induction intensity Bs is about 1.2T, and the residual magnetic induction intensity is about 0.28T; the initial magnetic permeability of the magnetic core has a temperature coefficient of about +0.06% / °C at a general use environment temperature of -40°C to 70°C.

[0012] The technical solution adopted by the method for preparing the iron-based nanocrystalline soft magnetic alloy of the present invention is:

[0013] A preparation method of an iron-based nanocrystalline soft magnetic alloy comprises the following steps: subjecting an amorphous alloy material to heat treatment and transverse magnetic field treatment to obtain an iron-based nanocrystalline soft magnetic alloy; the amorphous alloy material is composed of the following elements in percentage by mass: 6.8-7.2% silicon, 2.2-2.8% boron, 1.2-1.8% copper, 5.7-6.3% niobium, and 81.9-84.1% iron.

[0014] The preparation method of the iron-based nanocrystalline soft magnetic alloy of the present invention performs heat treatment and transverse magnetic field treatment on the amorphous alloy material, which can further improve the initial magnetic permeability of the material, and at the same time make the change of the magnetic permeability of the material under different magnetic field strengths small, and make the magnetic permeability of the magnetic material gradually increase with the increase of temperature, so that when the iron-based nanocrystalline soft magnetic alloy is used in the iron core, it can offset a part of the adverse effect caused by the increase of the copper resistance of the coil with the increase of temperature, and reduce the fluctuation of the error of the mutual inductor with the change of temperature. The relative magnetic permeability of the iron-based nanocrystalline soft magnetic alloy prepared by the present invention can reach 300,000, and the saturation magnetic induction intensity can reach 1.2T. The present invention improves the initial magnetic permeability without reducing the saturation magnetic induction intensity of the material by adjusting the formula and processing technology of the iron-based nanocrystalline soft magnetic alloy, and can reduce the residual magnetic induction intensity of the iron core.

[0015] Preferably, the amorphous alloy material is prepared by a method comprising the following steps: mixing and melting iron powder and alloy raw materials to obtain a molten raw material, and then solidifying the molten raw material to obtain an amorphous alloy material; the alloy raw materials consist of silicon, boron, copper and niobium.

[0016] Preferably, the heat treatment method is as follows: the amorphous alloy material is heated to 475-485° C., kept warm for 1.5-2.5 hours, then continued to be heated to 558-568° C., kept warm for 2 hours to 2.5 hours, and then cooled to room temperature.

[0017] Preferably, the temperature of the transverse magnetic field treatment is 440-460° C., the magnetic field intensity is 1000 GS-3000 GS, and the time of the transverse magnetic field treatment is 0.5-1 h.

[0018] The technical solution adopted by the application of the iron-based nanocrystalline soft magnetic alloy of the present invention as a magnetic core material is:

[0019] An application of the above-mentioned iron-based nanocrystalline soft magnetic alloy as a magnetic core material.

[0020] The relative magnetic permeability of the iron-based nanocrystalline soft magnetic alloy of the present invention can reach 300,000, the saturation magnetic induction intensity can reach 1.2T, and the magnetic permeability gradually increases with the increase of temperature. When used in the iron core, it can offset part of the adverse effect caused by the increase of the coil copper resistance with the increase of temperature, so as to reduce the fluctuation of the mutual inductor error with temperature change. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 Schematic diagram of a static hysteresis loop and a basic magnetization curve of an iron-based nanocrystalline soft magnetic alloy according to Example 1 of the present invention;

[0022] Figure 2 It is a schematic diagram of a static hysteresis loop and a basic magnetization curve of the iron-based nanocrystalline soft magnetic alloy of Comparative Example 1 of the present invention;

[0023] Figure 3 Schematic diagram of the magnetic permeability variation curve of the iron-based nanocrystalline soft magnetic alloy at different temperatures in Example 1 of the present invention. DETAILED DESCRIPTION

[0024] The iron-based nanocrystalline soft magnetic alloy of the present invention is a pioneering invention. The iron-based nanocrystalline soft magnetic alloy of the present invention is composed of the following elements in mass percentage: 6.8-7.2% silicon, 2.2-2.8% boron, 1.2-1.8% copper, 5.7-6.3% niobium, and 81.9-84.1% iron. The preparation method of the iron-based nanocrystalline soft magnetic alloy of the present invention comprises the following steps: subjecting an amorphous alloy material to heat treatment and transverse magnetic field treatment to obtain an iron-based nanocrystalline soft magnetic alloy; the amorphous alloy material is composed of the following elements in mass percentage: 6.8-7.2% silicon, 2.2-2.8% boron, 1.2-1.8% copper, 5.7-6.3% niobium, and 81.9-84.1% iron.

[0025] The iron-based nanocrystalline soft magnetic alloy of the present invention is obtained by optimizing the formula design of conventional nanocrystalline materials. Compared with conventional nanocrystalline materials, the magnetic core rate of the iron-based nanocrystalline soft magnetic alloy of the present invention is further improved. The initial relative magnetic permeability μi of the magnetic core made of the iron-based nanocrystalline soft magnetic alloy of the present invention is about 300000, the saturation magnetic induction intensity Bs is about 1.2T, and the residual magnetic induction intensity is about 0.28T; the initial magnetic permeability of the magnetic core has a temperature coefficient of about +0.06% / °C at a general use environment temperature of -40°C to 70°C.

[0026] The preparation method of the iron-based nanocrystalline soft magnetic alloy of the present invention performs heat treatment and transverse magnetic field treatment on the amorphous alloy material, which can further improve the initial magnetic permeability of the material, and at the same time make the change of the magnetic permeability of the material under different magnetic field strengths small, and at the same time make the magnetic permeability of the magnetic material gradually increase with the increase of temperature, so that when the iron-based nanocrystalline soft magnetic alloy is used in the iron core, it can offset a part of the adverse effect caused by the increase of the copper resistance of the coil with the increase of temperature, and reduce the fluctuation of the error of the mutual inductor with the change of temperature. The relative magnetic permeability of the iron-based nanocrystalline soft magnetic alloy prepared by the present invention can reach 300,000, and the saturation magnetic induction intensity can reach 1.2T. The present invention improves the initial magnetic permeability without reducing the saturation magnetic induction intensity of the material by adjusting the formula and processing technology of the iron-based nanocrystalline soft magnetic alloy, and can reduce the residual magnetic induction intensity of the iron core.

[0027] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0028] 1. The specific embodiments of the iron-based nanocrystalline soft magnetic alloy and the preparation method thereof of the present invention are as follows:

[0029] Example 1

[0030] The iron-based nanocrystalline soft magnetic alloy of the present embodiment is composed of the following elements in percentage by mass: 7% silicon, 2.5% boron, 1.5% copper, 6% niobium, and 83% iron.

[0031] Example 2

[0032] The iron-based nanocrystalline soft magnetic alloy of the present embodiment is composed of the following elements in percentage by mass: 6.8% silicon, 2.2% boron, 1.2% copper, 5.7% niobium, and 84.1% iron.

[0033] Example 3

[0034] The iron-based nanocrystalline soft magnetic alloy of the present embodiment is composed of the following elements in percentage by mass: 7.2% silicon, 2.8% boron, 1.8% copper, 6.3% niobium, and 81.9% iron.

[0035] The preparation method of the iron-based nanocrystalline soft magnetic alloy of Examples 1-3 specifically comprises the following steps:

[0036] After the iron powder is melted, the alloy raw material is added, and then stirred evenly to obtain a molten raw material, and then the molten raw material is rapidly solidified to obtain an amorphous alloy material, and then the amorphous alloy material is subjected to heat treatment and transverse magnetic field treatment to obtain an iron-based nanocrystalline soft magnetic alloy. Among them, the alloy raw material is composed of silicon, boron, copper and niobium elements, and the cooling end point of rapid solidification is room temperature. The method of heat treating the amorphous alloy material is as follows: the amorphous alloy material is heated to 480°C, kept warm for 2h, and then continued to be heated to 563°C, kept warm for 2h, and then cooled to room temperature; the temperature of the transverse magnetic field treatment is 450°C, the time is 0.5h, and the magnetic field intensity is 1200GS.

[0037] In other embodiments, the heat treatment method is as follows: the amorphous alloy material is heated to 475 or 485°C, kept warm for 2 or 2.5 hours, then continued to be heated to 558 or 568°C, kept warm for 2.1 or 2.5 hours, and then cooled to room temperature; the temperature of the transverse magnetic field treatment is 440 or 460°C, the time is 0.7 or 1 hour, and the magnetic field strength is 1000 or 3000GS.

[0038] Comparative Example 1

[0039] The iron-based nanocrystalline soft magnetic alloy of this comparative example is composed of the following elements in percentage by mass: 7.5% silicon, 1.5% boron, 2% copper, 5.5% niobium, and 83.5% iron.

[0040] 2. Specific examples of the application of the iron-based nanocrystalline soft magnetic alloy of the present invention as a magnetic core material are as follows:

[0041] Any of the iron-based nanocrystalline soft magnetic alloys of Examples 1-3 can be used as a magnetic core material (magnetic core material of a current transformer).

[0042] Experimental example

[0043] In order to evaluate the magnetic properties of the iron-based nanocrystalline soft magnetic alloys of each embodiment and comparative example, the static hysteresis loop and basic magnetization curve of the iron-based nanocrystalline soft magnetic alloys of each embodiment and comparative example were tested respectively. The static hysteresis loop and basic magnetization curve of the iron-based nanocrystalline soft magnetic alloys of Example 1 and Comparative Example 1 are as follows: Figure 1-2 As shown ( Figure 1 The MeasurementResult in the table represents the test result). The magnetic permeability of the iron-based nanocrystalline soft magnetic alloy of Example 1 at different temperatures was also tested. The relationship between the relative temperature change rate of the magnetic permeability and the temperature is shown in FIG. Figure 3 And the characteristic parameters of the iron-based nanocrystalline soft magnetic alloys of various embodiments and comparative examples are summarized in Table 1. Figure 1-2In the figure, μi represents the initial relative magnetic permeability, Bs represents the saturation magnetic induction intensity, μm represents the maximum magnetic permeability, Br represents the residual magnetic induction intensity, Hc represents the coercive force, Hi represents the magnetic field intensity corresponding to the initial magnetic permeability, and Hs represents the saturation magnetic induction intensity.

[0044] Table 1 Characteristic parameters of the iron-based nanocrystalline soft magnetic alloys of the embodiments and comparative examples

[0045] Soft magnetic alloy Initial magnetic permeability Saturation magnetic induction Residual magnetic induction Coercivity Curie temperature Example 1 300,000 1.2T 0.28T 0.3a / m 570℃ Example 2 280,000 1.22T 0.35T 0.4a / m 570℃ Example 3 295,000 1.15T 0.3T 0.4a / m 570℃ Comparative Example 1 200,000 1.2T 0.77T 0.7a / m 570℃

[0046] As can be seen from Table 1, the iron-based nanocrystalline soft magnetic alloy prepared by the specific formula of the present invention has the advantages of high initial magnetic permeability and low coercive force (about 0.3A / m); when used as an iron core, the mutual inductor can have the characteristics of small initial error and good linearity; at the same time, the iron-based nanocrystals have the advantages of high saturation magnetic induction intensity (about 1.2T) and high Curie temperature (about 570°C), which can make the mutual inductor have the characteristics of strong overload capacity and good temperature stability.

Claims

1. An iron-based nanocrystalline soft magnetic alloy, characterized in that: It is composed of the following elements in the following mass percentages: silicon 6.8-7.2%, boron 2.2-2.8%, copper 1.2-1.8%, niobium 5.7-6.3%, and iron 81.9-84.1%.

2. A method for preparing an iron-based nanocrystalline soft magnetic alloy, characterized in that: The following steps are involved: The amorphous alloy material is subjected to heat treatment and transverse magnetic field treatment to obtain an iron-based nanocrystalline soft magnetic alloy; The amorphous alloy material is composed of the following elements in percentage by mass: 6.8-7.2% silicon, 2.2-2.8% boron, 1.2-1.8% copper, 5.7-6.3% niobium, and 81.9-84.1% iron.

3. The method for preparing the iron-based nanocrystalline soft magnetic alloy according to claim 2, characterized in that: The amorphous alloy material is prepared by a method comprising the following steps: mixing and melting iron powder and alloy raw materials to obtain a molten raw material, and then solidifying the molten raw material to obtain the amorphous alloy material; The alloy raw materials are composed of silicon, boron, copper and niobium.

4. The method for preparing the iron-based nanocrystalline soft magnetic alloy according to claim 2 or 3, characterized in that: The heat treatment method is as follows: the amorphous alloy material is heated to 475-485°C, kept warm for 1.5-2.5 hours, then continued to be heated to 558-568°C, kept warm for 2 hours to 2.5 hours, and then cooled to room temperature.

5. The method for preparing the iron-based nanocrystalline soft magnetic alloy according to claim 2 or 3, characterized in that: The temperature of the transverse magnetic field treatment is 440-460° C., the magnetic field intensity is 1000 GS-3000 GS, and the time of the transverse magnetic field treatment is 0.5-1 h.

6. Use of the iron-based nanocrystalline soft magnetic alloy as claimed in claim 1 as a magnetic core material.