Coil component
By setting a void in the coil component and forming a metal oxide distribution using the heat during calcination, the problem of stress instability between the conductor layer and the magnetic body layer is solved, and the position stability and electromagnetic performance of the coil are improved.
Patent Information
- Application Number
- CN202411106186.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2020-02-25
- Filing Date
- 2021-02-23
- Publication Date
- 2024-11-22
AI Technical Summary
In the existing coil components, the stress between the conductor layer and the magnetic body layer is unstable, resulting in unstable coil position.
By providing a void between the magnetic layer and the coil wiring, and forming a region containing metal oxides on the side of the void, the metal oxide is melted by the heat during calcination to form an island-shaped or strip-shaped metal oxide distribution. Ensure uniformity and stability of the void.
The stress between the magnetic layer and the coil wiring is alleviated, the position stability of the coil is improved, and the unevenness of impedance and inductance values is suppressed, ensuring high-quality electromagnetic performance.
Smart Images

Figure CN119008194A_ABST
Abstract
Description
[0001] This application is a divisional application of patent application 202110200611.0 (application date: February 23, 2021, invention name: coil component). Technical Field
[0002] The present invention relates to a coil component and a method for manufacturing the same. Background Art
[0003] As a conventional coil component, there is a coil component described in Japanese Patent Application Laid-Open No. 11-219821 (Patent Document 1). In Patent Document 1, a gap is provided to relieve stress between a conductor layer and a magnetic layer, and the gap is provided over the entire circumference of the conductor layer.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 11-219821 Summary of the invention
[0007] In the coil component described in Patent Document 1, the conductor layer and the magnetic layer forming the coil are not in direct contact, and the position of the coil in such a coil component may be unstable.
[0008] An object of the present invention is to provide a coil component in which the position of the coil is stabilized while relieving stress.
[0009] In order to solve the above-mentioned problems, a coil component as one embodiment of the present disclosure includes a unit body and a coil provided in the unit body.
[0010] The unit cell has a plurality of stacked magnetic layers.
[0011] The coil has a plurality of stacked coil wires.
[0012] The magnetic layers and coil wiring are stacked alternately.
[0013] There is a gap between the magnetic layer and the coil wiring.
[0014] Part of the coil wiring is in contact with the magnetic layer.
[0015] A region containing a metal oxide exists in a part of the surface of the coil wiring on the gap portion side.
[0016] According to the above embodiment, the stress between the magnetic layer and the coil wiring is relieved by providing a gap between the magnetic layer and the coil wiring. In addition, since at least a portion of the coil wiring is in contact with the magnetic layer, the position of the coil wiring is more stable than when there is a gap around the entire circumference of the coil wiring.
[0017] In one embodiment of the coil component, the melting point of the metal contained in the metal oxide is 850° C. or lower.
[0018] According to the above embodiment, the metal is melted before the sintering of the conductor paste that becomes the coil wiring is completed, and the cavity portion can be easily formed.
[0019] In one embodiment of the coil component, the metal oxide includes at least one of an oxide of Cu, an oxide of Zn, an oxide of Bi, and an oxide of Sn.
[0020] The metal contained in the metal oxide in the above embodiment is a metal that can melt at a temperature lower than the sintering temperature of the coil conductor paste of the coil wiring, and / or a metal that can be used as a material constituting the magnetic layer. According to such a form, the above metal melts during the heating to the sintering temperature, and a gap portion can be easily formed, and / or the same material as the magnetic layer can be used, so the metal oxide formed by protruding from the coil wiring is absorbed by the magnetic layer of the unit body during calcination and integrated, which can suppress the unevenness of the size of the gap portion, and help suppress the unevenness of the impedance value and inductance value of the coil component.
[0021] In one embodiment of the coil component, the shape of the region containing the metal oxide includes at least one of an island shape and a strip shape.
[0022] According to the above embodiment, since the regions containing the metal oxide are dotted or dispersed on the surface of the coil wiring, the voids can be uniformly formed on the surface of the coil wiring.
[0023] In one embodiment of the coil component, the shape of the region containing the metal oxide includes an island shape, and an equivalent circle diameter of the island shape has a diameter of 0.1 μm or more.
[0024] In the above embodiment, since the equivalent circle diameter of the island shape is 0.1 μm or more, the amount of metal used for forming the cavity can be ensured to be constant. As a result, the cavity can be easily formed.
[0025] In the above-described embodiment, the ratio of the region containing the metal oxide (also referred to as “coverage”) is 10% to 80% with respect to the surface area of the coil wiring.
[0026] According to the above embodiment, when the gap is formed by melting the metal that is the raw material of the metal oxide, the gap can be reliably formed on the surface of the coil wiring by making the proportion of the area containing the metal oxide 10% or more. In addition, the proportion of the area containing the metal oxide does not necessarily need to be formed on the entire surface of the coil wiring, and from the viewpoint of forming the gap, 80% is sufficient.
[0027] According to the above embodiment, the maximum thickness of the cavity is in the range of 0.5 μm to 8.0 μm.
[0028] According to the above embodiment, the presence of the gap portion can provide a stress relief effect. Also, since the thickness of the gap portion is within a specific range, the coil component can ensure an impedance value and an inductance value.
[0029] According to the above embodiment, the gap portion exists on one surface of the coil wiring in the stacking direction.
[0030] According to the above embodiment, the gap portion is provided on one side in the stacking direction, thereby achieving the effect of relaxing stress. In addition, since the magnetic layer is provided on the other side in the stacking direction, the position of the coil conductor is stabilized, and the coil component can ensure the impedance value and inductance value.
[0031] According to the above embodiment, the method for manufacturing a coil component includes the following steps:
[0032] A step of forming a layer containing a metal on the magnetic sheet which becomes a magnetic layer after calcination,
[0033] a step of forming a coil conductor paste layer which becomes a coil wiring after firing on the layer containing the metal, and
[0034] A step of melting the metal contained in the metal-containing layer by firing to form a gap between the coil wiring and the magnetic layer and providing a region containing a metal oxide on the surface of the coil wiring.
[0035] According to the above embodiment, since the heat during firing is utilized to melt the metal contained in the metal-containing layer, the cavity portion is easily formed.
[0036] According to the coil component of the present invention, stress can be relaxed and the position of the coil can be stabilized. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 It is a perspective view showing the first embodiment of the coil component.
[0038] Figure 2 yes Figure 1 X-X cross-sectional view of the coil component.
[0039] Figure 3 This is an exploded top view of the coil component.
[0040] Figure 4 yes Figure 2 An enlarged cross-sectional view of the area around the coil wiring.
[0041] Figure 5A It is an explanatory diagram for explaining an example of a method for manufacturing a coil component.
[0042] Figure 5B It is an explanatory diagram for explaining an example of a method for manufacturing a coil component.
[0043] Figure 5C It is an explanatory diagram for explaining an example of a method for manufacturing a coil component.
[0044] Figure 5D It is an explanatory diagram for explaining an example of a method for manufacturing a coil component.
[0045] Fig. 6A It is an explanatory diagram for explaining an example of a method for manufacturing a coil component.
[0046] Figure 6B It is an explanatory diagram for explaining an example of a method for manufacturing a coil component.
[0047] Figure 7 It is an enlarged cross-sectional view of the vicinity of the coil wiring of the coil component according to the second embodiment.
[0048] Fig. 8A It is an explanatory diagram of the surface of the coil wiring in Example 1, and is an explanatory diagram showing that copper oxide and zinc oxide are formed on the surface of the coil wiring.
[0049] Figure 8B It only means Fig. 8A Illustration of copper oxide in .
[0050] Figure 8C It only means Fig. 8A Illustration of zinc oxide in .
[0051] Fig. 9 It is an explanatory diagram of the surface of the coil wiring in Example 2, and is an explanatory diagram showing that copper oxide is formed on the surface of the coil wiring.
[0052] Fig.10 It is an explanatory diagram of the surface of the coil wiring in Example 3, and is an explanatory diagram showing that zinc oxide is formed on the surface of the coil wiring.
[0053] Fig.11 This is an explanatory diagram of the surface of the coil wiring in Example 4, and is an explanatory diagram showing that copper oxide is formed in a strip shape on the surface of the coil wiring.
[0054] Explanation of symbols
[0055] 1 Coil components
[0056] 10 units
[0057] 111st magnetic layer
[0058] 12 Second magnetic layer
[0059] 15 The first end face of the unit
[0060] The second end face of the 16-unit body
[0061] 17 units side view
[0062] 20 coils
[0063] 21 Coil wiring
[0064] 31 1st external electrode
[0065] 32 2nd external electrode
[0066] 41 Layer containing metal
[0067] 51 gap
[0068] 61 1st lead conductor layer
[0069] 62 2nd lead conductor layer
[0070] 71 Region containing metal oxides
[0071] 71a, 71b Metal oxides
[0072] 211 magnetic sheet
[0073] 212 Magnetic paste layer
[0074] 221 coil conductor paste layer
[0075] 261 1st lead conductor paste layer
[0076] T height direction
[0077] WWidth direction
[0078] L Length direction DETAILED DESCRIPTION
[0079] Hereinafter, a coil component as one embodiment of the present disclosure will be described in detail by way of the illustrated embodiment. It should be noted that the drawings include some schematic diagrams and may not reflect actual dimensions and ratios.
[0080] (First embodiment)
[0081] Figure 1It is a perspective view showing the first embodiment of the coil component. Figure 2 yes Figure 1 The XX cross-sectional view of the first embodiment shown is an LT cross-sectional view passing through the center in the W direction. Figure 3 It is an exploded top view of the coil component, and the figures from the bottom to the top are shown along the T direction. It should be noted that the L direction is the length direction of the coil component 1, the W direction is the width direction of the coil component 1, and the T direction is the height direction (first direction) of the coil component 1.
[0082] like Figure 1 to Figure 3 As shown, the coil component 1 includes a unit body 10 , a coil 20 provided inside the unit body 10 , and a first external electrode 31 and a second external electrode 32 provided on the surface of the unit body 10 and electrically connected to the coil 20 .
[0083] The coil component 1 is electrically connected to wiring of a circuit board (not shown) via first and second external electrodes 31 and 32. The coil component 1 is used as a noise reduction filter, for example, and can be used in electronic devices such as computers, DVD players, digital cameras, TVs, mobile phones, and automotive electronics.
[0084] The unit body 10 is formed in a substantially rectangular parallelepiped shape and has a first end face 15, a second end face 16 located opposite to the first end face 15, and four side faces 17 located between the first end face 15 and the second end face 16. The first end face 15 and the second end face 16 face each other in the L direction.
[0085] The unit body 10 includes a plurality of first magnetic layers 11 and second magnetic layers 12. The first magnetic layers 11 and the second magnetic layers 12 are alternately stacked in the T direction. The first magnetic layers 11 and the second magnetic layers 12 are made of, for example, a magnetic material such as a Ni-Cu-Zn ferrite material. The thickness of each of the first magnetic layer 11 and the second magnetic layer 12 is, for example, not less than 5 μm and not more than 30 μm. It should be noted that the unit body 10 may partially contain a non-magnetic layer.
[0086] The first external electrode 31 covers the entire surface of the first end face 15 of the unit cell 10 and the end of the side face 17 of the unit cell 10 on the first end face 15 side. The second external electrode 32 covers the entire surface of the second end face 16 of the unit cell 10 and the end of the side face 17 of the unit cell 10 on the second end face 16 side. The first external electrode 31 is electrically connected to the first end of the coil 20, and the second external electrode 32 is electrically connected to the second end of the coil 20.
[0087] The first external electrode 31 may be formed in an L shape on the first end surface 15 and one side surface 17 , and the second external electrode 32 may be formed in an L shape on the second end surface 16 and one side surface 17 .
[0088] The coil 20 is wound in a spiral shape along the T direction. The coil 20 is made of a conductive material such as Ag or Cu. The coil 20 includes a plurality of coil wires 21 and a plurality of lead conductor layers 61 and 62 .
[0089] The 2-layer first lead conductor layer 61, the plurality of coil wirings 21, and the 2-layer second lead conductor layer 62 are sequentially arranged along the T direction and are electrically connected sequentially through via conductors. The plurality of coil wirings 21 are sequentially connected in the T direction to form a spiral along the T direction. The 1st lead conductor layer 61 is exposed from the 1st end face 15 of the unit body 10 and connected to the 1st external electrode 31, and the 2nd lead conductor layer 62 is exposed from the 2nd end face 16 of the unit body 10 and connected to the 2nd external electrode 32. It should be noted that the number of layers of the 1st and 2nd lead conductor layers 61 and 62 is not particularly limited, and for example, each may be 1 layer.
[0090] The coil wiring 21 is provided on the first magnetic layer 11 and is provided on the same layer as the second magnetic layer 12. By adopting such a configuration, the thickness of the coil wiring 21 can be maintained, and the DC resistance value (Rdc) of the coil wiring 21 can be reduced. In other words, the shape of the cross section of the coil wiring 21, in other words, the shape of the cross section of the coil wiring 21 in the direction perpendicular to the extension direction can be made into a trapezoidal or other rectangular shape. It should be noted that, Figure 3 The second magnetic layer 12 is omitted.
[0091] Part of the coil wiring 21 is in contact with the magnetic layer. Specifically, the coil wiring 21 is in contact with the first magnetic layer 11 on its upper surface and in contact with the second magnetic layer 12 on its left and right surfaces. By adopting such a form, the position of the coil wiring 21 is stabilized compared to a case where the entire circumference of the coil wiring 21 is not in contact with the magnetic layer.
[0092] The coil wiring 21 is formed in a shape that is wound in a plane less than one turn. The lead conductor layers 61 and 62 are formed in a straight line shape. The thickness of the coil wiring 21 is, for example, 10 μm to 40 μm. The thickness of the first and second lead conductor layers 61 and 62 is, for example, 10 μm to 30 μm, but may be thinner than the thickness of the coil wiring 21.
[0093] There is a gap 51 in the unit cell 10. The gap 51 exists between the magnetic layer and the coil wiring 21. Specifically, the gap 51 exists between the first magnetic layer 11 and the coil wiring 21. By providing the gap 51, the stress generated by the difference in thermal expansion coefficient between the coil wiring 21 and the first magnetic layer 11 can be suppressed, the degradation of the inductance (impedance value) caused by the internal stress can be eliminated, and a high impedance value (inductance value) can be ensured.
[0094] In addition, the gap portion 51 exists on one side of the stacking direction of the coil wiring 21. Specifically, it is provided in a manner of contacting the lower surface of the coil wiring 21. The gap portion 51 exists on one side of the stacking direction of the coil wiring 21, and the first magnetic layer 11 exists on the other side. By adopting such a form, the position of the coil wiring 21 is stabilized, and a high impedance value (inductance value) can be ensured.
[0095] The maximum thickness of the gap 51 is, for example, 0.5 μm to 8.0 μm. The gap 51 having such a maximum thickness can fully exert the stress relaxation effect and also ensure a high impedance value (inductance value) of the coil component because the thickness of the gap is within a specific range.
[0096] Figure 4 express Figure 2 An enlarged cross-sectional view of the coil wiring 21 and its vicinity. Figure 4 As shown, a region 71 containing a metal oxide exists in a part of the surface of the coil wiring 21 on the side of the cavity 51 .
[0097] The region 71 containing metal oxide may be a region composed only of metal oxide, and the region 71 containing metal oxide may contain inevitable impurities.
[0098] The metal oxide-containing region 71 includes a first metal oxide 71 a and a second metal oxide 71 b. The first metal oxide 71 a and the second metal oxide 71 b are compounds containing different metals.
[0099] The first metal oxide 71a is an oxide of Cu. Since Cu is a metal that can be used as a material for constituting a magnetic layer, the same material as the magnetic layer can be used. Since the metal oxide formed by protruding from the coil wiring is absorbed by the magnetic layer of the unit body during calcination and integrated, it is possible to suppress the unevenness of the size of the gap portion, which helps to suppress the unevenness of the impedance value and inductance value of the coil component. Examples of Cu oxides include CuO, Cu 2 O.
[0100] The second metal oxide 71b is an oxide of Zn. Zn is a metal that can be used as a material for constituting a magnetic layer. Therefore, the same material as the magnetic layer can also be used. Since the metal oxide formed by protruding from the coil wiring is absorbed and integrated by the magnetic layer of the unit body during calcination, the unevenness of the size of the gap portion can be suppressed, which helps to suppress the unevenness of the impedance value and inductance value of the coil component. In addition, the heat of calcination can be used to melt Zn, making it easier to form the gap portion. In addition, the melting point of Zn is 419°C, that is, Zn is a metal with a melting point of less than 850°C. Therefore, when Zn is used, the metal melts before the sintering of the conductor paste that becomes the coil wiring is completed, and the formation of the gap portion becomes easier. As an oxide of Zn, for example, ZnO can be cited.
[0101] The shape of the region 71 containing the metal oxide includes at least one of an island shape and a band shape. Since the region 71 containing the metal oxide has the above-mentioned shape and is spread or dispersed on the surface of the coil wiring, a gap portion can be uniformly formed on the surface of the coil wiring. In addition, since the region 71 containing the metal oxide is spread or dispersed, when the gap portion 51 is formed by melting the metal that becomes the raw material of the metal oxide, the gap portion 51 with a stable shape can be uniformly formed.
[0102] Here, the band shape refers to a thin and continuous shape with a constant width, for example, a long rectangular strip. The constant width means that the width is generally constant. In the case of a band shape, the region 71 containing the metal oxide may be a straight line or a curved line.
[0103] Island-like refers to a shape having a circular, elliptical and / or a shape close to these shapes, and refers to a shape from which an equivalent circle diameter can be obtained. In the case of an island-like shape, the regions 71 containing metal oxides may be separated from each other, or may not be completely separated, and the regions 71 containing metal oxides may be in contact with each other in a portion. In addition, the regions 71 containing metal oxides may be mixed with the regions 71 having an island-like shape and the regions 71 having a band-like shape, or a plurality of regions 71 having an island-like shape may be connected with the region 71 having a band-like shape.
[0104] When the region 71 containing metal oxide is in an island shape, the equivalent circle diameter of the region 71 containing metal oxide may be 0.1 μm or more. Since the equivalent circle diameter of the island shape is 0.1 μm or more, the amount of metal used in forming the gap 51 can be ensured to be constant. As a result, the formation of the gap 51 becomes easy.
[0105] Here, the equivalent circle diameter refers to the equivalent circle diameter of the island shape in the SEM (scanning electron microscope) image of the surface observed from the gap 51 side of the coil wiring 21. For example, for the above-mentioned equivalent circle diameter, a specific range (e.g., 15μm×25μm) is photographed with SEM at 5000 times on the surface of the gap 51 side of the coil wiring 21 of the coil component 1, and the SEM image is analyzed using image analysis software (e.g., A-Zou Kun (registered trademark) manufactured by Asahi Kasei Engineering Corporation), and the equivalent circle diameter can be obtained for the island shape. As a metal oxide, when there are multiple types, it is required regardless of the type of metal oxide. It should be noted that the type of metal oxide can be identified by elemental analysis using EDS (energy dispersive X-ray spectrometer).
[0106] The ratio of the region 71 containing the metal oxide (also referred to as "coverage") to the surface area of the coil wiring 21 (the total value of the area of the surface exposed in the void 51 of the coil wiring 21 and the area of the region 71 containing the metal oxide) can be 10% to 80%. When the void 51 is formed by melting the metal that serves as the raw material of the metal oxide, the ratio of the region 71 containing the metal oxide is set to 10% or more, so that the void 51 can be reliably formed on the surface of the coil wiring 21. In addition, the ratio of the region 71 containing the metal oxide does not necessarily need to be formed on the entire surface of the coil wiring, and from the viewpoint of forming the void, 80% is sufficient.
[0107] Here, the ratio of the region 71 containing the metal oxide can be obtained by photographing a specific range (e.g., 15 μm×25 μm) at 5000 times with an SEM on the surface observed from the gap 51 side of the coil wiring 21 of the coil component 1, analyzing the SEM image using image analysis software (e.g., A-Zou Kun (registered trademark) manufactured by Asahi Kasei Engineering Corporation), and calculating the ratio of the area of the region 71 containing the metal oxide to the total value of the area of the surface exposed in the gap 51 of the coil wiring 21 and the area of the region 71 containing the metal oxide. It should be noted that when there are multiple types of metal oxides, the region 71 containing the metal oxide refers to all the regions containing the metal oxide.
[0108] Next, use Figure 5A to Figure 5D and Figure 6A to Figure 6B An example of a method for manufacturing the coil component 1 will be described. It should be noted that the method for manufacturing the coil component 1 is not limited to the following method, and other manufacturing methods may be used.
[0109] Figure 5A to Figure 5D The cross section along the width direction of the coil wiring 21 , in other words, the cross section perpendicular to the extending direction of the coil wiring 21 is shown.
[0110] First, the magnetic sheet 211 is prepared. The magnetic sheet 211 can be produced, for example, by molding a magnetic paste containing a magnetic ferrite material into a sheet shape and processing it by punching etc. as needed. In addition, a through hole is formed by laser irradiation at a predetermined location of the magnetic sheet 211.
[0111] As a method of processing the magnetic slurry into a sheet, for example, a doctor blade method is mentioned. The thickness of the obtained sheet is, for example, 15 μm or more and 25 μm or less.
[0112] The composition of the magnetic ferrite material is not particularly limited. For example, a ferrite containing Fe 2 O 3 , ZnO, CuO and NiO. Magnetic ferrite materials contain Fe 2 O 3 , ZnO, CuO and NiO, regarding their contents, for example, Fe 2 O 3 The above-mentioned magnetic ferrite material may further contain additives. Examples of the additives include Mn, 3 O 4 、Co 3 O 4 SnO 2 、Bi 2 O 3 、SiO 2 .
[0113] The magnetic ferrite material is mixed and crushed by a wet method using a commonly used method, and then dried. The dried product obtained by drying is pre-calcined at 700° C. to 800° C., specifically, 700° C. to 720° C. to form a raw material powder. It should be noted that the raw material powder (pre-calcined powder) may contain inevitable impurities.
[0114] A water-based acrylic binder and a dispersant are added to the raw material powder, and mixed and crushed by a wet method to prepare a magnetic slurry. The mixed and crushed in the wet method can be carried out, for example, by adding partially stabilized zirconia (PSZ) balls to a pot mill. It should be noted that the magnetic sheet 211 becomes the first magnetic layer 11 after calcination.
[0115] As shown below, a metal-containing layer 41 is formed on the magnetic sheet 211. The metal contained in the metal-containing layer 41 is a raw material of a metal oxide, and in this embodiment, contains Cu and Zn. The metal-containing layer 41 can be composed of at least one selected from metal resinates, metal salts, and composite materials of metals and resins.
[0116] The metal-containing layer 41 can be formed by applying a solution containing at least one of a metal resinate, a metal salt, and a composite material of metal and resin by a spray method or the like, and then drying it at 70° C. to 100° C. as required. At this time, a mask or the like can be used as required. A plurality of solutions containing at least one of a metal resinate, a metal salt, and a composite material of metal and resin can be used, or only one can be used. For example, in the case of two kinds, two metal resinate solutions can be used in combination, or both a metal resinate solution containing one side and a solution containing a metal salt containing the other side can be used.
[0117] Metal resinate refers to an organic compound of a metal, that is, a compound containing a metal (e.g., Zn) and an organic group. Here, the organic group refers to a group containing a carbon atom. Examples of solvents contained in the metal resinate solution include isobutyl alcohol and butyl carbitol. The concentration of the metal contained in the metal resinate solution is, for example, 6% to 10% by weight, when converted into metal atoms, relative to the entire solution.
[0118] Examples of the metal salt include CuCl 2 (Melting point 498°C). It should be noted that CuCl 2 The melting point of CuCl is lower than the sintering temperature (e.g. 850°C) of the coil conductor paste that becomes the coil wiring. 2 When the molten metal is used, it melts during the calcination and a void portion can be easily formed.
[0119] As the solution containing the metal salt, an aqueous solution containing the metal salt can be used. It should be noted that the solution containing the metal salt can be any solution as long as the metal salt can be dissolved, for example, a solution containing a metal salt and an organic solvent, a solution containing a metal salt, an organic solvent and water,
[0120] The concentration of the metal contained in the solution containing the metal salt is, for example, 6% by weight to 10% by weight in terms of metal atoms relative to the entire solution.
[0121] The composite material of metal and resin is, for example, a material obtained by dispersing or dissolving metal powder or metal salt powder in resin. As the metal, for example, Zn can be mentioned, and as the metal salt, for example, CuCl can be mentioned. 2 .
[0122] The first conductive paste is formed into a coil conductor paste layer 221 by, for example, screen printing, in a manner overlapping the metal-containing layer 41. The first conductive paste can be, for example, a paste containing Ag powder, a solvent, a resin, and a dispersant. As the solvent, for example, eugenol can be mentioned, and as the resin, for example, ethyl cellulose can be mentioned. The preparation of the above-mentioned paste-like conductor composition can be carried out using a commonly used method. For example, it can be prepared by mixing Ag powder, a solvent, a resin, and a dispersant with a planetary mixer and then dispersing them with a three-roll mill. It should be noted that the coil conductor paste layer 221 becomes the coil wiring 21 after calcination.
[0123] Thereafter, a magnetic paste layer 212 is provided on the magnetic sheet 211 and on the same layer as the coil conductor paste layer 221. The magnetic paste layer 212 can be formed by screen printing the following magnetic paste. The magnetic paste layer 212 becomes the second magnetic layer 12 after being fired.
[0124] The magnetic paste is a paste-like composition containing a solvent, a raw material powder, a resin, and a plasticizer, and can be formed by kneading these with a planetary mixer and then dispersing them with a three-roll mill.
[0125] The raw material powder can be obtained by pre-calcining a magnetic ferrite material. The magnetic ferrite material can be the same as the magnetic ferrite material in the magnetic sheet. The pre-calcination of the magnetic ferrite material can be obtained by mixing and pulverizing the mixed material in a wet method using a commonly used method, and then drying the dried material, and pre-calcining the dried material at a temperature of 800° C. to 820° C. It should be noted that the raw material powder may contain inevitable impurities.
[0126] Through the above Figure 5A to Figure 5D According to the method shown, the coil wiring 21 is formed on the first magnetic layer 11 .
[0127] like Fig. 6A As shown, for the first lead conductor layer 61, first, a magnetic sheet 211 is prepared, and then, as shown in Figure 6B As shown, the second conductive paste is screen-printed on the magnetic sheet 211 to form the first lead conductor paste layer 261. The first lead conductor paste layer 261 becomes the first lead conductor layer 61 after firing. The second lead conductor layer 62 is also formed in the same manner as the first lead conductor layer 61.
[0128] The second conductive paste is a paste-like composition, and for example, a paste containing Ag powder, a solvent, a resin, and a dispersant can be used. Alternatively, the same material as the first conductive paste can be used.
[0129] These are bonded by heat and pressure to produce a laminated block.
[0130] Thereafter, the formed laminated body block is subjected to commonly performed operations, such as singulation, calcination, formation of external electrodes, etc., to form the coil component 1. The singulation, calcination, and formation of external electrodes can be performed using commonly performed methods. For example, the singulation can be performed by cutting the obtained laminated body block with a cutting machine or the like. As required, an arc is formed at a corner or the like by performing rotary drum grinding. The formation of the external electrode can be provided in the following manner: the exposed end face of the lead conductor layer is immersed in a layer obtained by stretching the Ag paste to a specified thickness, and the base electrode is formed by sintering at a temperature of about 800°C, and then a Ni film and a Sn film are sequentially formed on the base electrode by electroplating.
[0131] The calcination can be performed at a temperature of 880°C to 920°C (temperature at which the magnetic slurry or magnetic paste that becomes the magnetic layer is sintered). It is believed that the metal or metal salt contained in the metal-containing layer 41 melts at a temperature below the temperature at which the sintering of the first conductive paste, such as Ag paste, is completed during the temperature rise during calcination. The temperature at which the sintering of Ag paste is completed is, for example, 850°C. In contrast, for example, the melting point of Zn is 419°C, so the metal resinate of Zn also melts at 419°C. In addition, CuCl 2 The melting point of Ag is 498° C. Therefore, both the metal and the metal salt melt at a temperature lower than the temperature at which the sintering of the Ag paste is completed.
[0132] As a result of the melting of the metal or metal salt as described above, the bonding strength of the portion where the metal-containing layer 41 exists between the coil wiring 21 and the first magnetic layer 11 or the second magnetic layer 12 decreases, and when the coil wiring 21 shrinks, a gap 51 is formed between the coil wiring 21 and the first magnetic layer 11 or the second magnetic layer 12. In addition, when the temperature is increased during calcination, at least a portion of the metal or metal salt contained in the metal-containing layer 41 is oxidized to form a metal oxide.
[0133] (Second embodiment)
[0134] Figure 7 The second embodiment of the coil component 1 of the present disclosure is shown, and an enlarged cross-sectional view of the coil wiring 21A and its vicinity is shown. In the second embodiment, the second magnetic layer 12 is not present, and the shape of the coil wiring 21A is different from that of the first embodiment.
[0135] In the second embodiment, the parts denoted by the same reference numerals as those in the first embodiment represent the same configurations. The description of the parts having the same configurations as those in the first embodiment may be omitted.
[0136] like Figure 7As shown, in the unit body 10A, the cross-section of the coil wiring 21A in the direction perpendicular to the extending direction is an oval shape. The upper surface of the coil wiring 21A contacts the first magnetic layer 11. It should be noted that the coil wiring 21A can be the same as the coil wiring 21 of the first embodiment except for its shape.
[0137] A region 71 containing a metal oxide exists in a part of the surface on the side of the cavity 51 of the lower surface of the coil wiring 21A. The region 71 containing a metal oxide includes a first metal oxide 71a and a second metal oxide 71b.
[0138] It should be noted that the present invention is not limited to the above-described embodiment, and design changes can be made within the scope of the gist of the present invention.
[0139] In the first embodiment, the first magnetic layer 11 is provided on the entire upper surface of the coil wiring 21, but it may be provided on only a portion of the upper surface. Similarly, in the above embodiment, the second magnetic layer 12 is provided on the entire left and right surfaces of the coil wiring 21, but it may be provided on only a portion thereof.
[0140] In the above-described first embodiment, the gap portion 51 is provided on the lower surface of the coil wiring 21 , but may be provided on the upper surface of the coil wiring 21 .
[0141] In the first embodiment, the gap 51 is provided between the coil wiring 21 and the first magnetic layer 11 , but may be provided between the coil wiring 21 and the second magnetic layer 12 , between the coil wiring 21 and the first magnetic layer 11 , and between the coil wiring 21 and the second magnetic layer 12 .
[0142] In the first embodiment, the first metal oxide 71a and the second metal oxide 71b are described as the metal oxides contained in the metal oxide-containing region 71, but the metal oxide may be a single compound (ie, only the first metal oxide 71a) or three or more compounds.
[0143] In the first embodiment described above, Cu and Zn are described as metals contained in the region 71 containing metal oxides, but Bi and Sn can be cited as metals other than Cu and Zn. In other words, the metal oxide may contain at least one of Cu oxide, Zn oxide, Bi oxide, and Sn oxide. Like Cu and Zn, Bi and Sn are also metals that can be used as materials constituting the magnetic layer, and the same material as the magnetic layer can also be used. Since the metal oxide formed by protruding from the coil wiring is absorbed and integrated by the magnetic layer of the unit body during calcination, the unevenness of the size of the gap portion can be suppressed, which helps to suppress the unevenness of the impedance value and inductance value of the coil component. In addition, the heat during calcination can be used to melt the above metals, making it easier to form the gap portion. In addition, since the melting point of Bi is 271°C and the melting point of Sn is 232°C, Bi and Sn are metals with a melting point of 850°C or less at the end of sintering of the conductor paste that becomes the coil wiring. Therefore, when these metals are used, the metal melts during the temperature rise period during calcination, making it easier to form the gap portion. Examples of Bi oxides include Bi 2 O 3 Examples of Sn oxides include SnO, SnO 4 SnO 3 .
[0144] In the above-mentioned first embodiment, Cu and Zn are described as the metal contained in the metal-containing layer 41 , but examples of metals other than Cu and Zn include Bi and Sn.
[0145] Bi and Sn are used, for example, as metal resinates and / or composite materials of metal and resin.
[0146] (Example)
[0147] Next, the surface of the coil wiring 21 viewed from the gap 51 side will be described using an embodiment.
[0148] It should be explained that Figures 8A to 8C , Figures 9-11 The figure is created from a SEM image obtained by cutting the coil component at a surface on the gap 51 side of the coil wiring 21 after the coil component is formed, and photographing the surface of the coil wiring 21 from a direction orthogonal to the gap 51 .
[0149] (Example 1)
[0150] The coil component of the first embodiment was produced. The metal-containing layer 41 was formed by applying a Zn resinate solution and then applying a CuCl 2 formed by an aqueous solution.
[0151] Fig. 8AIn FIG. 1 , the portion displayed in black is a region 71 containing a metal oxide, specifically, a region composed of copper oxide and zinc oxide. Fig. 8A The white portion of FIG. 2 is a portion exposed to the gap 51 of the coil wiring 21 . Fig. 8A In the graph, the ratio of the region 71 containing the metal oxide is 76%.
[0152] Figure 8B Only extract Fig. 8A The copper oxide is in the shape of islands.
[0153] Figure 8C Only extract Fig. 8A Figure 1. The shapes of zinc oxide are islands and bands. For example, Figure 8C In the figure, the portion marked with the symbol "I" is an island, and the portion marked with the symbol "B" is a band.
[0154] (Example 2)
[0155] In this embodiment, the metal contained in the region 71 containing the metal oxide is one kind of metal.
[0156] The metal-containing layer 41 is formed using CuCl 2 of aqueous solution.
[0157] Fig. 9 In FIG. 1 , the portion displayed in black is a region 71 containing a metal oxide, specifically, a region composed of copper oxide. Fig. 9 In the figure, the ratio of the region 71 containing the metal oxide is 14%, and the copper oxide is in the form of islands and strips. For example, Fig. 9 In the figure, the portion marked with the symbol "I" is an island, and the portion marked with the symbol "B" is a band.
[0158] (Example 3)
[0159] In this embodiment, the metal contained in the region 71 containing the metal oxide is one kind of metal.
[0160] The metal-containing layer 41 is formed using a Zn resinate solution.
[0161] Fig.10 In FIG. 1 , a portion displayed in black is a region 71 containing a metal oxide, specifically, a region composed of zinc oxide. Fig.10 In the figure, the ratio of the region 71 containing the metal oxide is 10%, and the shape of the zinc oxide is an island shape. In addition, the equivalent circle diameter of the zinc oxide is not less than 0.114 μm.
[0162] (Example 4)
[0163] In this embodiment, the metal contained in the region 71 containing the metal oxide is one kind of metal.
[0164] The metal-containing layer 41 is formed using CuCl 2 of aqueous solution.
[0165] Fig.11 In FIG. 1 , the portion displayed in black is a region 71 containing a metal oxide, specifically, a region composed of copper oxide. Fig.11 In the example, the ratio of the region 71 containing the metal oxide is 60%, and the copper oxide is in the form of islands and strips. Fig.11 In the figure, the portion marked with the symbol "I" is an island, and the portion marked with the symbol "B" is a band.
Claims
1. A coil component comprising a unit body and a coil arranged in the unit body, The unit cell has a magnetic layer, The coil has a plurality of stacked coil wires and a plurality of lead conductor layers. There is a gap between the magnetic layer and the coil wiring. A portion of the coil wiring is in contact with the magnetic layer, A region containing a metal oxide exists on a portion of the surface of the coil wiring on the side of the gap portion.
2. The coil component according to claim 1, wherein The melting point of the metal contained in the metal oxide is 850° C. or lower.
3. The coil component according to claim 1, wherein The metal oxide contains at least one of Cu oxide, Zn oxide, Bi oxide, and Sn oxide.
4. The coil component according to any one of claims 1 to 3, wherein The shape of the region containing the metal oxide includes at least one of an island shape and a strip shape.
5. The coil component according to claim 4, wherein The shape of the region containing the metal oxide includes an island shape, and an equivalent circle diameter of the island shape has a diameter of 0.1 μm or more.
6. The coil component according to any one of claims 1 to 5, wherein: The ratio of the region containing the metal oxide to the surface area of the coil wiring is 10% to 80%.
7. The coil component according to any one of claims 1 to 6, wherein: The maximum thickness of the void portion is in the range of 0.5 μm to 8.0 μm.
8. The coil component according to any one of claims 1 to 7, wherein The void portion exists on one surface of the coil wiring in the stacking direction.