Silicon carbide device and manufacturing method thereof
By correcting the photoresist layer and trench side walls of silicon carbide devices, the problems of low accuracy and rough side walls in the prior art are solved, the accuracy and performance of the device are improved, and the product yield is improved.
Patent Information
- Application Number
- CN202411472953.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-22
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-10-22
AI Technical Summary
The existing silicon carbide device manufacturing process is difficult to meet the high-precision requirements, especially when the device size is reduced, resulting in poor perpendicularity of the silicon carbide trench gate and rough side walls, affecting device accuracy and performance.
By correcting the patterned photoresist layer, its roughness is reduced, and the side walls of the silicon carbide trench formed by etching are corrected, and gases such as HBr and fluorine-based gas are used to reduce the roughness of the side walls. , improve the verticality and smoothness of the grooves.
It improves the transfer accuracy and performance of silicon carbide devices, reduces the resistance of the device, and improves product yield.
Smart Images

Figure CN119008400A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of semiconductor technology, and in particular to a silicon carbide device and a manufacturing method thereof. Background Art
[0002] Silicon carbide power metal oxide semiconductor field effect transistor (MOSFET) is a widely used semiconductor transistor that can be used as a switching device in high-power device applications. In order to obtain better performance and higher operating voltage, silicon carbide MOSFET adopts a silicon carbide trench gate structure to achieve lower on-resistance and improve device reliability and service life.
[0003] However, with the development of semiconductor technology, in order to improve the integration density, the characteristic size of silicon carbide devices has been continuously reduced, and the existing manufacturing process can hardly meet the high-precision requirements of silicon carbide devices. Summary of the invention
[0004] The following is a summary of the subject matter of the detailed description of the present disclosure. This summary is not intended to limit the scope of the claims.
[0005] In a first aspect, the present disclosure provides a method for manufacturing a silicon carbide device, comprising:
[0006] Providing a silicon carbide substrate, forming a photoresist layer on the silicon carbide substrate, and patterning the photoresist layer, wherein the patterned photoresist layer has a first roughness;
[0007] Performing a correction process on the patterned photoresist layer, so that the corrected photoresist layer has a second roughness, and the second roughness is smaller than the first roughness;
[0008] Etching the silicon carbide substrate according to the modified photoresist layer to form a plurality of silicon carbide grooves arranged at intervals, wherein the sidewalls of the silicon carbide grooves have a third roughness;
[0009] The sidewall of the silicon carbide trench is subjected to a modification process, and the modified sidewall of the silicon carbide trench has a fourth roughness, and the fourth roughness is smaller than the third roughness.
[0010] Optionally, the silicon carbide substrate is placed in a process chamber, and the steps of modifying the patterned photoresist layer, etching the silicon carbide substrate according to the modified photoresist layer, and modifying the sidewall of the silicon carbide trench are sequentially performed.
[0011] Optionally, performing a correction process on the patterned photoresist layer includes:
[0012] Under a first process condition, a first gas is used to process the patterned photoresist layer.
[0013] Optionally, the first gas includes HBr; and the first process conditions include:
[0014] Temperature 10℃-60℃; Pressure 1mtorr-100mtorr; Source power 100W-1000W; Bias power 10W-500W.
[0015] Optionally, the bias power of the first process condition is positively correlated with the thickness of the photoresist layer, and the source power of the first process condition is negatively correlated with the thickness of the photoresist layer.
[0016] Optionally, the sidewall of the silicon carbide trench is subjected to a modification process, comprising:
[0017] Under the second process condition, a second gas is used to process the sidewall of the silicon carbide trench; the second gas includes a fluorine-based gas.
[0018] Optionally, the second gas includes at least one of SF6, NF3, CF4, C2F6, C4F8, C5F8 and C4F6; and the second process conditions include:
[0019] Temperature 0℃-60℃; Pressure 10mtorr-1000mtorr; Source power 500W-3000W; Bias power 10W-1000W.
[0020] Optionally, the manufacturing method comprises:
[0021] Patterning the photoresist layer to form an initial photoresist pattern, wherein the initial photoresist pattern has a first characteristic size;
[0022] The patterned photoresist layer is modified to increase the characteristic size of the initial photoresist pattern to form a photoresist pattern with a second characteristic size, wherein the second characteristic size is greater than the first characteristic size.
[0023] Optionally, the first roughness includes line width roughness and line edge roughness.
[0024] In a second aspect, the present disclosure provides a silicon carbide device, which is manufactured using the method for manufacturing the silicon carbide device as described in the first aspect.
[0025] The silicon carbide device and the manufacturing method thereof disclosed in the present invention perform correction processing on the patterned photoresist layer to reduce the roughness of the patterned photoresist layer, improve the transfer accuracy of etching a silicon carbide substrate to form a silicon carbide groove, and improve the verticality of the silicon carbide groove; and perform correction processing on the sidewall of the silicon carbide groove after etching to form the silicon carbide groove to reduce the roughness of the sidewall of the silicon carbide groove, which can reduce the film layer defects formed on the surface of the sidewall of the silicon carbide groove, reduce the resistance of the silicon carbide device, and improve the performance and product yield of the silicon carbide device. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the technical solutions in the embodiments of the present disclosure or the conventional technology, the drawings required for use in the embodiments or the conventional technology descriptions will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present disclosure, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0027] Figure 1 is a process flow chart of a method for manufacturing a silicon carbide device provided in an embodiment;
[0028] Figure 2 is a schematic diagram of forming a photoresist layer on a silicon carbide substrate and patterning the photoresist layer provided in an embodiment;
[0029] Figure 3 A schematic diagram of a patterned photoresist layer after correction processing provided in an embodiment;
[0030] Figure 4 is a schematic diagram of a hard mask layer patterned according to a modified photoresist layer provided in an embodiment;
[0031] Figure 5 is a schematic diagram of a silicon carbide substrate after patterning to form silicon carbide trenches in one embodiment;
[0032] Figure 6 is a schematic diagram of a side wall of a silicon carbide trench after a modification process is performed in one embodiment;
[0033] Figure 7 A schematic diagram of patterning a photoresist layer to form an initial photoresist pattern having a first feature size in one embodiment;
[0034] Figure 8 It is a schematic diagram of performing a correction process on a patterned photoresist layer to form a photoresist pattern with a second characteristic size in one embodiment;
[0035] Fig. 9 is a schematic diagram of a silicon carbide substrate after patterning to form silicon carbide trenches according to an embodiment;
[0036] Fig.10 FIG. 1 is a schematic diagram of a sidewall of a silicon carbide trench after being modified in one embodiment. DETAILED DESCRIPTION
[0037] In order to facilitate understanding of the present application, the present application will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present application are given in the drawings. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present application more thorough and comprehensive.
[0038] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0039] It should be understood that when an element or layer is referred to as "on ...", "adjacent to ...", "connected to" or "coupled to" other elements or layers, it can be directly on, adjacent to, connected to or coupled to other elements or layers, or there can be intervening elements or layers. On the contrary, when an element is referred to as "directly on ...", "directly adjacent to ...", "directly connected to" or "directly coupled to" other elements or layers, there are no intervening elements or layers. It should be understood that although the terms first, second, third, etc. can be used to describe various elements, components, regions, layers, doping types and / or parts, these elements, components, regions, layers, doping types and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer, doping type or part from another element, component, region, layer, doping type or part. Therefore, without departing from the teachings of the present invention, the first element, component, region, layer, doping type or portion discussed below may be represented as a second element, component, region, layer or portion; for example, the first doping type may be referred to as the second doping type, and similarly, the second doping type may be referred to as the first doping type; the first doping type and the second doping type are different doping types, for example, the first doping type may be P-type and the second doping type may be N-type, or the first doping type may be N-type and the second doping type may be P-type.
[0040] Spatially relative terms such as "under," "beneath," "below," "under," "above," "above," and the like may be used herein to describe the relationship of an element or feature shown in the figures to other elements or features. It should be understood that, in addition to the orientations shown in the figures, spatially relative terms also include different orientations of the device in use and operation. For example, if the device in the accompanying drawings is flipped, an element or feature described as "under other elements" or "under it" or "under it" will be oriented as being "above" the other elements or features. Thus, the exemplary terms "under" and "under" may include both upper and lower orientations. In addition, the device may also include additional orientations (e.g., rotated 90 degrees or other orientations), and the spatial descriptors used herein are interpreted accordingly.
[0041] When used herein, the singular forms "a", "an", and "said / the" may also include plural forms, unless the context clearly indicates otherwise. It should also be understood that when the terms "consisting of" and / or "comprising" are used in this specification, the presence of the features, integers, steps, operations, elements and / or parts can be determined, but the presence or addition of one or more other features, integers, steps, operations, elements, parts and / or groups is not excluded. At the same time, when used herein, the term "and / or" includes any and all combinations of the relevant listed items.
[0042] Embodiments of the invention are described herein with reference to cross-sectional views which are schematic diagrams of ideal embodiments (and intermediate structures) of the invention, such that variations in the shapes shown due to, for example, manufacturing techniques and / or tolerances are anticipated. Thus, embodiments of the invention should not be limited to the specific shapes of the regions shown herein, but rather include deviations in shapes due to, for example, manufacturing techniques. For example, an implanted region shown as a rectangle typically has rounded or curved features and / or an implant concentration gradient at its edges rather than a binary change from an implanted region to a non-implanted region. Similarly, a buried region formed by implantation may result in some implantation in the region between the buried region and the surface through which the implantation is performed. Thus, the regions shown in the figures are schematic in nature, their shapes do not represent the actual shape of the region of the device, and do not limit the scope of the invention.
[0043] With the advancement of semiconductor technology, the size of silicon carbide devices continues to decrease, and the requirements for the manufacturing process of silicon carbide devices are becoming higher and higher.
[0044] At present, the manufacturing process of silicon carbide devices is difficult to meet the high-precision requirements of silicon carbide devices. After analysis, it is believed that the reasons for the low manufacturing precision of silicon carbide devices include: the deviation of the pattern of the photoresist layer after patterning relative to the mask master, that is, the low precision of the pattern of the photoresist layer, which may cause deviation when the pattern is transferred according to the etching substrate of the photoresist layer, affecting the precision of the silicon carbide device; and in order to make the silicon carbide trench gate of the silicon carbide MOSFET, the etching substrate has a high aspect ratio, and the etching process is difficult to ensure high-precision etching, resulting in poor verticality of the formed silicon carbide trench gate or rough sidewalls of the silicon carbide trench gate, affecting the precision and device performance of the silicon carbide device.
[0045] In view of this, the present disclosure provides a silicon carbide device and a manufacturing method thereof, wherein after patterning a photoresist layer, the patterned photoresist layer is corrected to reduce the roughness of the corrected photoresist layer; after etching a silicon carbide substrate according to the corrected photoresist layer to form a silicon carbide groove, the sidewall of the silicon carbide groove is corrected to reduce the roughness of the sidewall of the silicon carbide groove. The roughness of the sidewall of the silicon carbide groove is reduced, the film layer defects formed on the surface of the sidewall of the silicon carbide groove are reduced, the resistance of the silicon carbide device is reduced, and the performance and product yield of the silicon carbide device are improved.
[0046] According to an exemplary embodiment, the present disclosure provides a method for manufacturing a silicon carbide device, such as Figure 1 As shown, the following steps are included:
[0047] Step S11: providing a silicon carbide substrate, forming a photoresist layer on the silicon carbide substrate, and patterning the photoresist layer, wherein the patterned photoresist layer has a first roughness;
[0048] Step S12: performing a correction process on the patterned photoresist layer, wherein the corrected photoresist layer has a second roughness, and the second roughness is smaller than the first roughness;
[0049] Step S13: etching the silicon carbide substrate according to the modified photoresist layer to form a plurality of silicon carbide grooves arranged at intervals, wherein the sidewalls of the silicon carbide grooves have a third roughness;
[0050] Step S14: performing a correction process on the sidewall of the silicon carbide trench, wherein the sidewall of the silicon carbide trench after correction has a fourth roughness which is smaller than the third roughness.
[0051] The method for manufacturing the silicon carbide device of the present embodiment performs correction processing on the patterned photoresist layer to reduce the roughness of the patterned photoresist layer, improves the pattern transfer accuracy of etching a silicon carbide substrate to form a silicon carbide groove, and improves the verticality of the silicon carbide groove; and after etching to form the silicon carbide groove, performs correction processing on the sidewall of the silicon carbide groove to reduce the roughness of the sidewall of the silicon carbide groove, which can reduce the film layer defects formed on the surface of the sidewall of the silicon carbide groove, reduce the resistance of the silicon carbide device, and improve the performance and product yield of the silicon carbide device.
[0052] In step S11, refer to Figure 2 A hard mask layer 20 is formed on the silicon carbide substrate 10 , and the material of the hard mask layer 20 may include at least one of silicon oxide, silicon nitride, silicon oxynitride or silicon oxycarbide.
[0053] A photoresist is coated on the silicon carbide substrate 10 and baked to form a photoresist layer 30. The photoresist layer 30 is exposed and developed according to a mask master (not shown in the figure), and the design pattern of the mask master is transferred to the photoresist layer 30 by patterning the photoresist layer 30, and a photoresist pattern 30a is formed on the photoresist layer 30.
[0054] A photolithography machine is used to expose the photoresist layer 30. Due to the limitation of the photolithography machine, the sidewalls of the patterned photoresist layer 30 are rough. For example, the dimensional accuracy of the photoresist pattern 30a is low, the verticality of the sidewalls of the photoresist pattern 30a is low, and the sidewalls of the photoresist pattern 30a are rough.
[0055] In this embodiment, the patterned photoresist layer 30 has a first roughness Ra1, wherein the first roughness includes line width roughness and line edge roughness.
[0056] Line Width Roughness (LWR) refers to the deviation of the line width of the photoresist pattern 30 a from the size value of the mask due to edge roughness.
[0057] Line Edge Roughness (LER) refers to the roughness of the edge of the photoresist pattern 30 a.
[0058] In step S12, refer to Figure 3 The patterned photoresist layer 30 is subjected to a correction treatment, including: using a first gas to treat the patterned photoresist layer 30 under a first process condition. The first gas includes HBr; the first process condition includes: a temperature of 10° C. to 60° C.; a pressure of 1 mtorr to 100 mtorr; a source power of 100 to 1000 W; and a bias power of 10 W to 500 W.
[0059] Specifically, the silicon carbide substrate 10 is placed in a process chamber (not shown in the figure), and the process chamber is a process chamber for dry etching the silicon carbide substrate 10 .
[0060] After the process chamber is evacuated, the process chamber is adjusted to the first process condition, the temperature is 10°C-60°C, for example, the temperature can be 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C or 60°C; the pressure is 1mtorr-100mtorr, for example, the pressure can be 1mtorr, 15mtorr, 30mtorr, 45mtorr, 50mtorr torr, 65mtorr, 80mtorr, 90mtorr or 100mtorr; source power 100W-1000W, for example, the source power can be 100W, 200W, 400W, 500W, 800W or 1000W; bias power 10W-500W, for example, the bias power can be 10W, 50W, 100W, 200W, 300W, 400W or 500W.
[0061] Then, a first gas is introduced into the process chamber, wherein the first gas includes HBr. The flow rate of the first gas is 35 nm / min-60 nm / min. For example, the flow rate of the first gas can be 35 nm / min, 38 nm / min, 40 nm / min, 42 nm / min, 45 nm / min, 48 nm / min, 50 nm / min, 52 nm / min, 55 nm / min, 58 nm / min or 60 nm / min.
[0062] In some examples, during the process of modifying the patterned photoresist layer 30 , the first gas may be introduced into the process chamber in a pulsed manner to flexibly control the progress of modifying the patterned photoresist layer 30 .
[0063] Under the first process condition, the first gas is ionized to generate bromine plasma, and the process chamber applies bias power to the bromine plasma, so that the bromine plasma bombards the patterned photoresist layer 30 in a direction perpendicular to the silicon carbide substrate 10, corrects the side wall of the patterned photoresist layer 30, removes the rough part of the side wall of the photoresist layer 30, corrects the defects of the side wall of the photoresist layer 30, and improves the dimensional accuracy of the corrected photoresist layer 30.
[0064] In this embodiment, the modified photoresist layer 30 has a second roughness Ra2, which is smaller than the first roughness Ra1. In addition, the dimensional accuracy of the modified photoresist layer 30 is greater than that of the photoresist layer 30 before modification; the dimensional accuracy includes the verticality and / or angle accuracy of the sidewall.
[0065] In order to ensure the dimensional accuracy of the photoresist pattern 30a, avoid the size increase of the photoresist pattern 30a caused by bromine plasma bombardment, and ensure that the photoresist pattern 30a and the pattern of the mask master have high accuracy, the bias power of the first process condition is set to 10W-500W in this embodiment.
[0066] In order to ensure the dimensional accuracy of the photoresist pattern 30a and avoid the bromine plasma bombarding the photoresist layer 30 for too long, which causes the size of the photoresist pattern 30a to increase, the time for the correction treatment of the patterned photoresist layer 30 is 10s-18s. For example, the correction treatment of the patterned photoresist layer 30 can be performed for 10s, 12s, 14s, 15s, 17s, 18s or 20s.
[0067] In some embodiments, the bias power of the first process condition is positively correlated with the thickness of the photoresist layer 30 , and the source power of the first process condition is negatively correlated with the thickness of the photoresist layer 30 .
[0068] In one example, the thickness of the patterned photoresist layer 30 is 500 nm, the bias power of the first process condition is 500 W, and the source power is 100 W. In another example, the thickness of the patterned photoresist layer 30 is 100 nm, the bias power of the first process condition is 10 W, and the source power is 1000 W.
[0069] In some embodiments, the first roughness Ra1 of the patterned photoresist layer 30 is 3nm, and the thickness of the patterned photoresist layer 30 is 200nm. After the process chamber is evacuated, the process chamber is adjusted to a temperature of 10°C-60°C; a pressure of 1mtorr-100mtorr; a source power of 100-1000W; a bias power of 10W-500W, and then a first gas is introduced into the process chamber, and the first gas corrects the patterned photoresist layer 30, and the processing time is 15s. The corrected photoresist layer 30 has a second roughness Ra2, and the second roughness Ra2=1nm.
[0070] In step S13 , in the process chamber, the silicon carbide substrate 10 is etched according to the modified photoresist layer 30 to form a plurality of silicon carbide trenches 11 .
[0071] In this embodiment, refer to Figure 4 , the hard mask layer 20 is etched according to the modified photoresist layer 30 , and the photoresist pattern 30 a is transferred to the hard mask layer 20 to obtain a patterned hard mask layer 20 .
[0072] Then, the photoresist layer 30 is removed by etching in the process chamber.
[0073] Next, refer to Figure 5, the silicon carbide substrate 10 is etched using the patterned hard mask layer 20 as a mask. Specifically, before etching the silicon carbide substrate 10, the process chamber is evacuated. Then, an etching gas is introduced into the process chamber, and the process conditions of the process chamber are adjusted. The plasma generated by the ionized etching gas bombards the silicon carbide substrate 10 exposed by the patterned hard mask layer 20 to form a plurality of spaced silicon carbide grooves 11. The sidewalls of the silicon carbide grooves 11 have a third roughness Ra3.
[0074] In this embodiment, a dry process is used to etch the silicon carbide substrate 10 to form the silicon carbide groove 11. The etching process is anisotropic etching. The etching speed in the direction perpendicular to the silicon carbide substrate 10 is greater than the etching speed in the horizontal direction, ensuring that the sidewalls of the formed silicon carbide groove 11 have high verticality.
[0075] In step S14, refer to Figure 6 After etching to form the silicon carbide trench 11, the sidewall of the silicon carbide trench 11 is modified in the above-mentioned process chamber.
[0076] The sidewall of the silicon carbide trench 11 is subjected to a modification process, including: using a second gas to process the sidewall of the silicon carbide trench 11 under a second process condition.
[0077] The second gas includes at least one of SF6, NF3, CF4, C2F6, C4F8, C5F8 and C4F6; in one example, the second gas includes SF6; in another example, the second gas includes NF3; in yet another example, the second gas includes CF4; in a fourth example, the second gas includes a mixed gas of SF6 and NF3.
[0078] The second process conditions include: temperature 0°C-60°C, for example, the temperature may be 0°C, 10°C, 20°C, 30°C, 40°C, 50°C or 60°C; pressure 10mtorr-1000mtorr, for example, the pressure may be 10mtorr, 50mtorr, 100mtorr, 300mtorr, 500mtorr, 700mtorr, 800mtorr or 1000mtorr; source power 500W-3000W, for example For example, the source power can be 500W, 800W, 1200W, 1500W, 1800W, 2200W, 2500W, 2800W or 3000W; the bias power is 10W-1000W. For example, the bias power can be 10W, 80W, 150W, 210W, 270W, 350W, 420W, 500W, 550W, 610W, 670W, 720W, 800W, 850W, 900W, 940W or 1000W.
[0079] The second gas dissociates under the second process condition to generate fluorine free radicals, which react with silicon atoms on the sidewalls of the silicon carbide groove 11 to generate gaseous products, and the reaction removes the rougher surface of the sidewalls of the silicon carbide groove 11 to correct the defects of the sidewalls of the silicon carbide groove 11 and improve the smoothness of the sidewalls of the silicon carbide groove 11. At the same time, compared with plasma etching, the reaction of free radicals is relatively mild, and will not form a strong bombardment to cause deformation of the silicon carbide lattice, and will not affect the original composition of the silicon carbide material. The sidewalls of the corrected silicon carbide grooves 11 have a fourth roughness Ra4, which is less than the third roughness Ra3.
[0080] In some embodiments, after the process chamber is evacuated, the process chamber is adjusted to a second process condition, and then a second gas is introduced into the process chamber, the second gas comprising SF6, and the flow rate of the second gas is 35 nm / min-60 nm / min.
[0081] Illustratively, the flow rate of the second gas may be 35 nm / min, 38 nm / min, 40 nm / min, 42 nm / min, 45 nm / min, 48 nm / min, 50 nm / min, 52 nm / min, 55 nm / min, 58 nm / min, or 60 nm / min.
[0082] In some embodiments, the sidewall of the silicon carbide groove 11 has a third roughness Ra3, and the third roughness Ra3=5nm. After evacuating the process chamber, adjust the process chamber to a temperature of 0°C-60°C; a pressure of 10mtorr-1000mtorr; a source power of 500W-3000W; a bias power of 10W-1000W, and then introduce a second gas into the process chamber. The second gas includes SF6, and the second gas corrects the sidewall of the silicon carbide groove 11. The processing time is 40s-60s. For example, the time for the second gas to correct the sidewall of the silicon carbide groove 11 can be 40s, 45s, 50s, 55s or 60s. The sidewall of the corrected silicon carbide groove 11 has a fourth roughness Ra4, and the fourth roughness Ra4=1.5nm.
[0083] In some embodiments, the bias power of the second process condition is defined according to the aspect ratio of the silicon carbide trench 11. The larger the aspect ratio of the silicon carbide trench 11, the larger the bias power is set to within the range of 10 W-1000 W. This is beneficial to increasing the line width of the trench and the verticality of the trench sidewall.
[0084] In some embodiments, the processing time for modifying the silicon carbide trench 11 is defined according to the aspect ratio of the silicon carbide trench 11 . The larger the aspect ratio of the silicon carbide trench 11 , the longer the processing time for modifying the silicon carbide trench 11 .
[0085] In the method for manufacturing the silicon carbide device of the present embodiment, the silicon carbide substrate 10 is placed in a process chamber, and the steps of correcting the patterned photoresist layer 30, etching the silicon carbide substrate 10 according to the corrected photoresist layer 30, and correcting the silicon carbide groove 11 are sequentially performed. In this way, there is no need to add new process equipment to correct the photoresist layer 30 and repair the silicon carbide groove 11. The operations of correcting the photoresist layer 30 and repairing the silicon carbide groove 11 can be performed on the original production line without additional equipment costs, and there is no need to transfer the silicon carbide substrate 10 between multiple reaction chambers, which saves operation procedures and reduces process difficulty.
[0086] In some embodiments, the target feature size of the silicon carbide trench 11 to be formed is W0. In step S11, referring to Figure 7 After forming a photoresist layer 30 on the silicon carbide substrate 10, the photoresist layer 30 is patterned to form an initial photoresist pattern 30b, the initial photoresist pattern 30b has a first feature size W1, the first feature size W1 is smaller than the target feature size W0, and the sidewall of the initial photoresist pattern 30b has a first roughness Ra1.
[0087] In step S12, refer to Figure 8 , the patterned photoresist layer 30 is corrected, the characteristic size of the initial photoresist pattern 30b is increased, and a photoresist pattern 30a having a second characteristic size W2 is formed, and the second characteristic size W2 is greater than the first characteristic size W1.
[0088] After the process chamber is evacuated, the process chamber is adjusted to the first process conditions, temperature 10°C-60°C; pressure 1mtorr-100mtorr; source power 100-1000W; bias power 10W-500W. Then, HBr gas is introduced into the process chamber, and the patterned photoresist layer 30 is processed for 15 seconds to form a photoresist pattern 30a with a second characteristic size W2, and the sidewall of the photoresist pattern 30a has a second roughness Ra2, and the second roughness Ra2=1nm.
[0089] In step S13, refer to Fig. 9 The silicon carbide substrate 10 is etched according to the photoresist pattern 30a having the second characteristic size W2 to form a silicon carbide trench 11. The silicon carbide trench 11 has the second characteristic size W2, and the sidewall of the silicon carbide trench 11 has a third roughness Ra3.
[0090] In step S14, refer to Fig. 9 , Fig.10After the process chamber is evacuated, the process chamber is adjusted to a temperature of 0°C-60°C; a pressure of 10mtorr-1000mtorr; a source power of 500W-3000W; and a bias power of 10W-1000W. Then, SF6 gas is introduced into the process chamber. SF6 generates fluorine free radicals. The fluorine free radicals react with silicon atoms on the side wall of the silicon carbide trench 11 to generate gaseous products. The reaction removes the rough surface of the side wall of the silicon carbide trench 11 (refer to Fig. 9 The dotted line portion is used to correct the defects of the sidewall of the silicon carbide trench 11. The corrected sidewall of the silicon carbide trench 11 has a fourth roughness Ra4, and the fourth roughness Ra4=1.5nm.
[0091] In some embodiments, the second feature size W2 is equal to the target feature size W0, and the silicon carbide trench 11 formed by etching the silicon carbide substrate 10 according to the photoresist pattern 30a has the target feature size W0.
[0092] In some other embodiments, the second characteristic size W2 is smaller than the target characteristic size W0, and the silicon carbide trench 11 formed by etching the silicon carbide substrate 10 according to the photoresist pattern 30a has the second characteristic size W2.
[0093] During the process of performing the correction treatment on the silicon carbide trench 11 , the silicon carbide trench 11 is made to have a target characteristic size W0 by correcting the treatment time of the silicon carbide trench 11 .
[0094] In this way, in the step of correcting the patterned photoresist layer 30, the correction time can be increased, the defective part of the side wall of the initial photoresist pattern 30a is removed, the characteristic size of the initial photoresist pattern 30a is increased to form the photoresist pattern 30a, and the side wall of the photoresist pattern 30a is ensured to be smooth and have high verticality, so as to improve the pattern transfer accuracy of etching the photoresist pattern 30a to form the silicon carbide groove 11, and improve the smoothness and verticality of the side wall of the silicon carbide groove 11; and after the silicon carbide groove 11 is formed, the side wall of the silicon carbide groove 11 is corrected to further increase the characteristic size of the silicon carbide groove 11 to the target characteristic size, and remove the defective part of the side wall of the silicon carbide groove 11 to make the groove wall of the silicon carbide groove 11 smooth, which can reduce the film layer defects formed on the surface of the side wall of the silicon carbide groove 11, reduce the resistance of the silicon carbide device, and improve the performance and product yield of the silicon carbide device.
[0095] According to an exemplary embodiment, the present disclosure further provides a silicon carbide device, which is manufactured using the method for manufacturing the silicon carbide device of the above embodiment. The silicon carbide device has a silicon carbide groove 11, and the groove wall of the silicon carbide groove 11 is smooth, which can reduce the film layer defects formed on the surface of the side wall of the silicon carbide groove 11, reduce the resistance of the silicon carbide device, and improve the performance and product yield of the silicon carbide device.
[0096] Among them, the silicon carbide device of this embodiment can be a dynamic random access memory (DRAM), a static random access memory (SRAM), a flash EPROM, a ferroelectric random access memory (FeRAM), a magnetic random access memory (MRAM) or other types of memory.
[0097] In some embodiments, an electronic device is provided, including the silicon carbide device of the above embodiment or the silicon carbide device manufactured by the method for manufacturing the silicon carbide device of the above embodiment. The electronic device can be a storage device, a mobile phone, a computer, a tablet computer, a television, an artificial intelligence device, etc.
[0098] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features of the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0099] The above-described embodiments only express several implementation methods of the present disclosure, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present disclosure, and these all belong to the protection scope of the present disclosure. Therefore, the protection scope of the patent of the present disclosure shall be subject to the attached claims.
Claims
1. A method for manufacturing a silicon carbide device, characterized in that: include: Providing a silicon carbide substrate, forming a photoresist layer on the silicon carbide substrate, and patterning the photoresist layer, wherein the patterned photoresist layer has a first roughness; Performing a correction process on the patterned photoresist layer, so that the corrected photoresist layer has a second roughness, and the second roughness is smaller than the first roughness; Etching the silicon carbide substrate according to the modified photoresist layer to form a plurality of silicon carbide grooves arranged at intervals, wherein the sidewalls of the silicon carbide grooves have a third roughness; The sidewall of the silicon carbide trench is subjected to a modification process, and the modified sidewall of the silicon carbide trench has a fourth roughness, and the fourth roughness is smaller than the third roughness.
2. The method for manufacturing a silicon carbide device according to claim 1, characterized in that: The silicon carbide substrate is placed in a process chamber, and the steps of modifying the patterned photoresist layer, etching the silicon carbide substrate according to the modified photoresist layer, and modifying the sidewall of the silicon carbide trench are sequentially performed.
3. The method for manufacturing a silicon carbide device according to claim 1, characterized in that: The patterned photoresist layer is subjected to a correction process, comprising: Under a first process condition, a first gas is used to process the patterned photoresist layer.
4. The method for manufacturing a silicon carbide device according to claim 3, characterized in that: The first gas includes HBr; the first process conditions include: Temperature 10℃-60℃; Pressure 1mtorr-100mtorr; Source power 100W-1000W; Bias power 10W-500W.
5. The method for manufacturing a silicon carbide device according to claim 4, characterized in that: The bias power of the first process condition is positively correlated with the thickness of the photoresist layer, and the source power of the first process condition is negatively correlated with the thickness of the photoresist layer.
6. The method for manufacturing a silicon carbide device according to claim 1, characterized in that: The sidewall of the silicon carbide trench is corrected, comprising: Under the second process condition, a second gas is used to process the sidewall of the silicon carbide trench; the second gas includes a fluorine-based gas.
7. The method for manufacturing a silicon carbide device according to claim 6, characterized in that: The second gas includes at least one of SF6, NF3, CF4, C2F6, C4F8, C5F8 and C4F6; the second process conditions include: Temperature 0℃-60℃; Pressure 10mtorr-1000mtorr; Source power 500W-3000W; Bias power 10W-1000W.
8. The method for manufacturing a silicon carbide device according to claim 1, characterized in that: The production method comprises: Patterning the photoresist layer to form an initial photoresist pattern, wherein the initial photoresist pattern has a first characteristic size; The patterned photoresist layer is modified to increase the characteristic size of the initial photoresist pattern to form a photoresist pattern with a second characteristic size, wherein the second characteristic size is greater than the first characteristic size.
9. The method for manufacturing a silicon carbide device according to claim 1, characterized in that: The first roughness includes line width roughness and line edge roughness.
10. A silicon carbide device, characterized in that: The silicon carbide device is manufactured by the method for manufacturing a silicon carbide device according to any one of claims 1 to 9.
Citation Information
Patent Citations
Polysilicon etching method
CN105470120A
Semiconductor device forming method
CN106158595A
Pattern transfer method
CN106571291A
Etching method of silicon carbide groove and preparation method of silicon carbide device
CN114551227A
Cited By
Semiconductor structure forming method and semiconductor structure
CN119890041A
A semiconductor structure forming method and a semiconductor structure
CN119890041B