Passivating film preparation method and semiconductor device

By stepping deposition of ammonia-free silicon nitride, ammonia-containing silicon nitride, silicon oxide and silicon oxynitride film layers, the problem of insufficient leakage and breakdown voltage in the traditional passivation film preparation solution is solved, and the electrical performance of semiconductor devices is improved. Film density.

CN119008426APending Publication Date: 2024-11-22BEIJING NAURA MICROELECTRONICS EQUIP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310553241.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

When the traditional passivation film preparation scheme deposits a thicker film layer at high power, it is easy to reduce the leakage yield of the device, and the breakdown voltage of the SiNx film layer is insufficient, which is easy to break down, resulting in current collapse.

Method used

By using step-by-step deposition method, first deposit the ammonia-free silicon nitride film layer, then deposit the ammonia-silicon nitride film layer, and optionally deposit the silicon oxide and silicon nitride film layer. By adjusting the gas composition and compressive stress, H ion diffusion is reduced. Enhance the density of the film layer and water vapor barrier capability.

Benefits of technology

It improves the density and breakdown voltage of the film layer, reduces the diffusion of H ions, avoids device leakage, enhances passivation effect, and improves the electrical performance of semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008426A_ABST
    Figure CN119008426A_ABST
Patent Text Reader

Abstract

The invention discloses a passive film preparation method and a semiconductor device, and the method comprises the steps: depositing a first film layer on a substrate through first deposition gas, the first deposition gas comprises SiH4 and N2, and the first film layer is ammonia-free silicon nitride; a second film layer is deposited on the first film layer through second deposition gas, the second deposition gas comprises SiH4, N2 and NH3, and the second film layer is ammonia silicon nitride. A high-quality passivation film can be formed, electric leakage of the semiconductor device is avoided, and the electric leakage yield of the semiconductor device is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductor technology, and in particular to a passivation film preparation method and a semiconductor device. Background Art

[0002] AlGaN / GaN high electron mobility transistor (HEMT), the heterojunction material surface of this type of device has surface states caused by crystal defects. The existence of these surface states will cause the device to produce current collapse when it is used in high-frequency and high-power applications, greatly reducing the output power of the device. Surface passivation measures can effectively suppress the current collapse phenomenon. Growing a passivation layer on the material surface can not only compensate for the occurrence of this phenomenon, but also weaken the influence of the ambient atmosphere on the electrical characteristics of the device.

[0003] The dielectric films commonly used for AlGaN / GaN HEMT surface passivation include SiNx (silicon nitride) and SIO2 (silicon dioxide). Among them, SiO2 is the earliest film used for passivation film. The interface state of the outermost layer is good, but compared with the SiNx film layer, SiO2 has a lower dielectric breakdown strength and carries a lower high-power voltage. It is easy to be broken down, resulting in leakage, and the passivation effect is not ideal. SiNx deposited by PECVD (plasma enhanced chemical vapor deposition) has a lower dielectric constant and a higher breakdown voltage strength. It is widely used in passivation films. At the same time, the H element contained in its film layer can diffuse to the Si-SiNx interface and effectively passivate the interface, further enhancing the density of the film layer. Using traditional SiNx deposition main gases, including SiH4, NH3 and N2, at 300°C, 500W, 1800A single-layer SiNx film is deposited to passivate the device surface.

[0004] AlGaN / GaN heterojunction materials mainly rely on polarization electric fields to induce two-dimensional electron gas. This characteristic causes charge damage on the AlGaN surface and the AlGaN / GaN interface, which has a significant impact on the channel charge. During the device passivation film coating process, excessive PECVD power will damage the device surface, resulting in a decrease in the device current, but too low PECVD power will reduce the density of the grown SiN film, thereby reducing the breakdown voltage of the film layer. Therefore, when the above passivation film preparation scheme uses excessively high power to deposit a thicker film thickness, it is easy to reduce the leakage yield of the device. Summary of the invention

[0005] In view of this, the present application provides a passivation film preparation method and a semiconductor device to solve the problem that the leakage yield of the device is easily reduced when a thicker film thickness is deposited at too high a power in a traditional passivation film preparation solution.

[0006] The present application provides a method for preparing a passivation film, comprising:

[0007] Depositing a first film layer on a substrate with a first deposition gas, wherein the first deposition gas comprises SiH4 and N2, and the first film layer is ammonia-free silicon nitride;

[0008] A second film layer is deposited on the first film layer using a second deposition gas, wherein the second deposition gas includes SiH4, N2 and NH3, and the second film layer is silicon nitride with ammonia.

[0009] Optionally, the passivation film preparation method further includes: depositing a third film layer on the second film layer using a third deposition gas, the third film layer being silicon oxide; the second film layer has compressive stress, and the compressive stress of the third film layer is smaller than that of the second film layer.

[0010] Optionally, the passivation film preparation method further includes: depositing a fourth film layer on the third film layer using a fourth deposition gas, the fourth film layer being silicon oxynitride; and the compressive stress of the fourth film layer is smaller than that of the third film layer.

[0011] Optionally, the fourth deposition gas includes NH 3, which is used to introduce Si—H bonds into the fourth film layer to enhance the water vapor barrier capability of the fourth film layer.

[0012] Optionally, the fourth deposition gas further includes N2O, and the stress of the fourth film layer is adjusted by adjusting the ratio of NH3 / N2O.

[0013] Optionally, before depositing the first film layer on the substrate with the first deposition gas, the passivation film preparation method further includes: introducing the first process gas into the process chamber to perform plasma bombardment cleaning on the surface to be deposited of the first film layer; the first process gas includes N2 and NH3.

[0014] Optionally, the ratio of N2 to NH3 in the first process gas ranges from 20:1 to 50:1.

[0015] Optionally, process parameters for introducing the first process gas into the process chamber include: a gas pressure range in the process chamber of 2000-2300 mT, a power supply power of 250-300 W, a flow range of N2 of 4000-5000 sccm, and a flow range of NH3 of 200-250 sccm.

[0016] Optionally, after depositing a second film layer on the first film layer with a second deposition gas, the passivation film preparation method further includes: introducing a second process gas into a process chamber, the second process gas including an oxygen-containing gas; the oxygen-containing gas is used to perform plasma bombardment on the second film layer to remove dangling bonds on the surface of the second film layer.

[0017] Optionally, after depositing a third film layer on the second film layer with a third deposition gas, the passivation film preparation method further includes: introducing the second process gas into the process chamber to perform plasma bombardment on the third film layer to remove dangling bonds on the surface of the third film layer.

[0018] Optionally, after depositing a fourth film layer on the third film layer with a fourth deposition gas, the passivation film preparation method further includes: introducing the second process gas into the process chamber to perform plasma bombardment on the fourth film layer to remove surface defects of the fourth film layer.

[0019] Optionally, the second process gas further includes a purge gas for removing particles on the surface of the film layer; wherein the ratio of the purge gas to the oxygen-containing gas is in the range of 50:1 to 60:1.

[0020] Optionally, the process parameters for introducing the second process gas into the process chamber include: the gas pressure range in the process chamber is 2000-2300mT, the power supply power includes 250-300W, the flow range of the purge gas is 4000-5000sccm, and the flow range of the oxygen-containing gas is 80-100sccm.

[0021] Optionally, the thickness of the first film layer is in the range of 300-400A; and / or the refractive index of the first film layer is in the range of 1.95-2.05.

[0022] Optionally, process parameters for depositing the first film layer include: the gas pressure range in the process chamber is 1500-2000mT, the power supply power includes 250-300W, the flow range of N2 is 5000-6000sccm, and the flow range of SiH4 is 100-200sccm.

[0023] Optionally, the thickness of the second film layer is in the range of 600-700 Å; and / or the refractive index of the second film layer is in the range of 1.95-2.05.

[0024] Optionally, the process parameters for depositing the second film layer include: the gas pressure range in the process chamber is 1500~2000mT, the power supply power includes 250~300W, the flow range of N2 is 5000-6000sccm, the flow range of SiH4 is 100-200sccm, and the flow range of NH3 is 100-200sccm.

[0025] Optionally, the thickness of the third film layer is in the range of 4000-5000A; and / or the refractive index of the third film layer is in the range of 1.455-1.465.

[0026] Optionally, the process parameters for depositing the third film layer include: the gas pressure range in the process chamber is 1500-2000mT, the power supply power includes 250-300W, the flow range of N2 is 5000-6000sccm, the flow range of SiH4 is 100-200sccm, and the flow range of N2O is 4000-5000sccm.

[0027] Optionally, the thickness of the fourth film layer is in the range of 2000-3000A; and / or the refractive index of the fourth film layer is in the range of 1.70-1.90.

[0028] Optionally, the process parameters for depositing the fourth film layer include: the gas pressure range in the process chamber is 1500~2000mT, the power supply power includes 250~300W, the flow range of N2 is 5000-6000sccm, the flow range of SiH4 is 100-200sccm, the flow range of N2O is 1000-2000sccm, and the flow range of NH3 is 100-200sccm.

[0029] The present application also provides a semiconductor device, comprising:

[0030] Semiconductor device film structure;

[0031] A passivation film is located on the surface of the film layer structure, and the passivation film is prepared by any of the above passivation film preparation methods.

[0032] The above-mentioned passivation film preparation method and semiconductor device of the present application are deposited in steps of a first film layer, a second film layer, a third film layer and a fourth film layer. In the first film layer close to the front-end structure of the semiconductor device, the amount of H is low, and it contains fewer Si-H bonds, more Si-Si bonds and Si-N bonds, which can reduce the escape phenomenon of H ions after annealing in the relevant film layer, can reduce the defects of the film, and can also ensure that H ions do not diffuse into the interior of the semiconductor device, thereby avoiding affecting the electrical properties of the semiconductor device. The second film layer has Si-H bonds, which can H-type the SiN film. The H ions in the second film layer can diffuse and capture O ions to form stable chemical bonds, play a role in passivating the surface, and realize the function of protecting the corresponding semiconductor device and avoiding leakage of the semiconductor device.

[0033] Furthermore, in the present application, the third film layer can enhance the passivation function through SiO2, and the Si-H bond is introduced into the fourth film layer to increase the proportion of H ions in the film layer, which can offset the O2 in the air and form a dense oxide film, further blocking water vapor in the air from entering the film layer, thereby avoiding leakage of semiconductor devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.

[0035] Figure 1 This is a schematic diagram of the semiconductor device structure during the research process;

[0036] Figure 2 This is a schematic diagram of a process for preparing a passivation film according to an embodiment of the present application;

[0037] Figure 3a and Figure 3b is a schematic diagram of the structure of each film layer in one embodiment of the present application;

[0038] Figure 4 is a schematic diagram of the structure of a semiconductor device according to an embodiment of the present application;

[0039] Figure 5 is a schematic flow chart of a method for preparing a passivation film according to another embodiment of the present application;

[0040] Figure 6 It is a performance comparison analysis diagram of an embodiment of the present application. DETAILED DESCRIPTION

[0041] The technical solutions in the embodiments of the present application are clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present application. In the absence of conflict, the following embodiments and their technical features can be combined with each other.

[0042] The first aspect of the present application provides a passivation film preparation method, which is mainly used to form a passivation film on the surface of a semiconductor device such as AlGaN / GaN HEMT. The structure of the above semiconductor device can refer to Figure 1 As shown, the structure includes a substrate (such as a silicon substrate, etc.), a GaN (gallium nitride) buffer layer, an AlGaN (aluminum gallium nitride) barrier layer and a GaN cap layer.

[0043] refer to Figure 2 As shown, the passivation film preparation method includes steps S110 to S140.

[0044] S110, reference Figure 3a As shown, the first deposition gas is deposited on the substrate ( Figure 3aThe first film layer 211 is deposited on the substrate (not shown), the first deposition gas includes SiH4 (silane) and N2 (nitrogen), and the first film layer is ammonia-free silicon nitride. The substrate is not limited to being in direct contact with the substrate, and other layers may be included between the substrate and the first film layer 211. For example, the above steps may form the first film layer 211 directly on the surface of the substrate, and for another example, the above steps may also form the first film layer 211 on the surface of other film layers above the substrate.

[0045] In step S110, radio frequency power can be applied to the process chamber so that the first deposition gas forms a plasma. In step S110, SiH4 and N2 are used as the main deposition gases, and NH3 (ammonia) is not introduced. The deposited first film layer 211 can also be called an ammonia-free SiNx layer, where SiNx can represent silicon nitride, and x can represent the content of the N element in the first film layer 211. In the above-mentioned first film layer 211, the amount of H (hydrogen) is relatively low, that is, it contains fewer Si-H bonds, more Si-Si bonds and Si-N bonds, and the density of the film layer is higher, thereby reducing the escape phenomenon of H ions in the relevant film layer after annealing, which can reduce the defects of the film; at the same time, it also ensures that H ions do not diffuse into the interior of the semiconductor device where the substrate is located, thereby avoiding affecting the electrical properties of the semiconductor device.

[0046] Optionally, the thickness of the first film layer 211 is in the range of 300 to 400 Å.

[0047] Optionally, the refractive index of the first film layer 211 is in the range of 1.95-2.05; for example, the refractive index of the first film layer 211 may be 1.95, 2.0 or 2.05. The stress corresponding to the first film layer 211 is compressive stress.

[0048] Optionally, the process parameters for depositing the first film layer 211 include: the pressure in the process chamber is in the range of 1500-2000 mT, the power is in the range of 250-300 W, the flow rate of N2 is in the range of 5000-6000 sccm, and the flow rate of SiH4 is in the range of 100-200 sccm. The process chamber may include a PECVD chamber.

[0049] S120, depositing a second film layer 212 on the first film layer 211 with a second deposition gas, wherein the second deposition gas includes SiH4, N2 and NH3, and the second film layer is silicon nitride containing ammonia.

[0050] In step S120, RF power may be applied to the process chamber to form a plasma from the second deposition gas. In step S120, NH3 is introduced into the second deposition gas, and the deposited second film layer 212 may also be called an ammonia SiNx layer. Si-H bonds exist in the second film layer 212, which can H-type the SiN film. The H ions in the second film layer 212 can diffuse and capture O ions to form stable chemical bonds, thereby passivating the surface.

[0051] Optionally, the thickness of the second film layer 212 is in the range of 600 Å to 700 Å.

[0052] Optionally, the refractive index of the second film layer 212 is in the range of 1.95-2.05; for example, the refractive index of the second film layer 212 may be 1.95, 2.0 or 2.05. The stress corresponding to the second film layer 212 is a slightly smaller compressive stress.

[0053] Optionally, the process parameters for depositing the second film layer 212 include: the gas pressure range in the process chamber is 1500-2000mT, the power includes 250-300W, the flow range of N2 is 5000-6000sccm, the flow range of SiH4 is 100-200sccm, and the flow range of NH3 is 100-200sccm.

[0054] The inventors analyzed the relevant traditional solutions and found that too high PECVD power will damage the device surface, resulting in a decrease in the current of the device. Too low PECVD power will reduce the density of the grown SiNx film, thereby reducing the breakdown voltage of the film layer. In addition, there are many Si-H bonds in the SINx film layer. Although it can combine with O ions to form stable chemical bonds and increase the passivation performance of the film layer, it cannot prevent H ions from diffusing into the device, causing leakage of the capacitor inside the device, which will damage the continuous aging state of the device. In the above-mentioned passivation film preparation method provided in the present application, the first film layer 211 and the second film layer 212 are deposited step by step. In the first film layer 211 close to the front-end structure of the semiconductor device, the H content is low, containing fewer Si-H bonds, and containing more Si-Si bonds and Si-N bonds. The density of the film layer is higher, which can reduce the escape phenomenon of H ions after annealing in the relevant film layer, can reduce the defects of the film, and can also ensure that H ions do not diffuse into the interior of the semiconductor device, thereby avoiding affecting the electrical properties of the semiconductor device. The second film layer 212 has Si-H bonds, which can H-type the SiN film. The H ions in the second film layer 212 can diffuse and capture O ions to form stable chemical bonds, play a role in passivating the surface, and realize the function of protecting the corresponding semiconductor device and avoiding leakage of the semiconductor device.

[0055] In one embodiment, reference Figure 3b As shown, the passivation film preparation method further includes: depositing a third film layer 213 on the second film layer 212 with a third deposition gas to enhance the passivation function. In this embodiment, radio frequency power can be applied to the process chamber to form a plasma with the third deposition gas. Optionally, the third deposition gas includes SiH4, N2O and N2, and the third film layer is silicon oxide (SiO2).

[0056] The second film layer 212 has compressive stress, and the compressive stress of the third film layer 213 is smaller than that of the second film layer 212 , which can improve the adhesion between the third film layer 213 and the second film layer 212 and make the film layer subsequently formed on the third film layer 213 more closely fit the third film layer 213 .

[0057] Optionally, the thickness of the third film layer 213 is in the range of 4000 to 5000 Å.

[0058] Optionally, the refractive index of the third film layer 213 is in the range of 1.455-1.465; for example, the refractive index of the third film layer 213 may be 1.455, 1.46 or 1.465.

[0059] Optionally, the process parameters for depositing the third film layer 213 include: the gas pressure range in the process chamber is 1500-2000mT, the power includes 250-300W, the flow range of N2 is 5000-6000sccm, the flow range of SiH4 is 100-200sccm, and the flow range of N2O is 4000-5000sccm.

[0060] In one example, if Figure 3b As shown, the passivation film preparation method further includes: depositing a fourth film layer 214 on the third film layer 213 with a fourth deposition gas, wherein the fourth film layer is silicon oxynitride. In this embodiment, radio frequency power can be applied to the process chamber to form a plasma in the fourth deposition gas.

[0061] Among them, the compressive stress of the fourth film layer 214 is smaller than that of the third film layer 213, which can improve the adhesion between the fourth film layer 214 and the third film layer 213, and can also make other film layers subsequently formed on the fourth film layer 214 more closely fit the fourth film layer 214, thereby improving the reliability of the final semiconductor device.

[0062] Optionally, the fourth deposition gas includes NH3, which is used to introduce Si-H bonds into the fourth film layer 214 to enhance the water vapor barrier capability of the fourth film layer 214. Specifically, Si-H bonds are introduced into SiO2 in the fourth film layer 214 to increase the proportion of H ions in the film layer, which can offset O2 in the air and form a dense oxide film, thereby preventing water vapor in the air from entering the film layer and avoiding leakage of the semiconductor device.

[0063] Optionally, the fourth deposition gas further includes N2O, so as to adjust the stress of the fourth film layer by adjusting the ratio of NH3 / N2O, thereby ultimately achieving the purpose of stress matching between film layers.

[0064] Furthermore, the fourth deposition gas includes SiH4, N2O, NH3 and N2, and it adopts SiH4, N2O, NH3 and N2 as main gas deposition, and the obtained fourth film layer 214 can be called SiOxNy layer, SiOxNy can represent silicon oxynitride layer, x can represent the content of O element in the fourth film layer 214, and y can represent the content of N element in the fourth film layer 214.

[0065] Optionally, the fourth film layer 214 has a thickness ranging from 2000 to 3000 Å.

[0066] Optionally, the refractive index of the fourth film layer 214 is in the range of 1.70-1.90; for example, the refractive index of the fourth film layer 214 may be 1.70, 1.80 or 1.90.

[0067] Optionally, the process parameters for depositing the fourth film layer 214 include: the gas pressure range in the process chamber is 1500-2000mT, the power supply power includes 250-300W, the flow range of N2 is 5000-6000sccm, the flow range of SiH4 is 100-200sccm, the flow range of N2O is 1000-2000sccm, and the flow range of NH3 is 100-200sccm.

[0068] refer to Figure 4As shown, the first film layer 211, the second film layer 212, the third film layer 213 and the fourth film layer 214 can form a passivation layer 210, and the passivation layer 210 covers the surface of semiconductor devices such as HEMT 220 to form a new semiconductor device. In the passivation layer 210, the refractive index of the first film layer 211 and the second film layer 212 at the bottom can both be 2.0, which is easy to debug and evaluate, the refractive index of the third film layer 213 in the middle can be 1.46, and the refractive index of the fourth film layer 214 formed last can be 1.8, which is convenient for FTIR (Fourier Transform Infrared Spectroscopy) testing, and is conducive to the rapid implementation and evaluation of corresponding debugging. Since the film layer with compressive stress can give the device a sense of pressure, the above-mentioned film layers are all compressive stress, and it is not easy to warp upward at the edge of the film layer, thereby avoiding the peeling phenomenon at the edge of the film layer after the deposition of multiple film layers; the lowest first film layer 211 has the largest compressive stress, and bears the downward pressure generated by the continuous increase in the thickness of the subsequent film layers. The compressive stress of each film layer formed later gradually decreases, which is beneficial to the flattening of the film layer and can ensure that the surface warping can match the upper device when the final film layer is thicker; in this way, the stress characteristics between each film layer can better ensure the adhesion of each film layer to the upper and lower layers of the semiconductor device, thereby ensuring that the film layer does not fall off and bubbling occurs during the aging process of the semiconductor device, and the performance of the resulting semiconductor device can be further improved.

[0069] In this embodiment, the first film layer 211, the second film layer 212, the third film layer 213 and the fourth film layer 214 are deposited step by step. In the first film layer 211 close to the front-end structure of the semiconductor device, the H content is relatively low and contains fewer Si-H bonds, which can reduce the escape phenomenon of H ions in the relevant film layer after annealing, reduce the defects of the film, and ensure that H ions do not diffuse into the interior of the semiconductor device, thereby avoiding affecting the electrical properties of the semiconductor device. The second film layer 212 has Si-H bonds, which can H-type the SiN film. The H ions in the second film layer 212 can diffuse and capture O ions to form stable chemical bonds, which play a role in passivating the surface. The third film layer 213 can enhance the passivation function through SiO2. In the fourth film layer 214, Si-H bonds are introduced into SiO2 to increase the proportion of H ions in the film layer, which can offset O2 in the air and form a dense oxide film, further blocking water vapor in the air from entering the film layer to avoid leakage of the semiconductor device.

[0070] In one embodiment, before depositing the first film layer 211 on the substrate with the first deposition gas, the passivation film preparation method further includes: preheating the substrate, introducing the first process gas into the process chamber, and performing plasma bombardment cleaning on the surface to be deposited of the first film layer 211, so as to remove the oxide film layer and particles contaminated by the first film layer 211 and related structures in other previous processes, protect and passivate the structure formed in the previous process, and mitigate the loss of the structure formed in the previous process. The first process gas includes N2 and NH3.

[0071] In one example, the ratio of N2 to NH3 in the first process gas ranges from 20:1 to 50:1. The first process gas contains a large amount of N2. Although NH3 will dissociate H ions and react with the oxide film layer on the surface of the semiconductor device to obtain a certain amount of by-products, these by-products can be carried away by a large amount of N2. In other words, the ionized H ions in NH3 have almost no adhesion and penetration to the surface of the semiconductor device, and a large amount of N2 can also form an atmosphere passivation protection on the surface of the semiconductor device, which can effectively prevent H ions from entering the interior of the semiconductor device, enhance the protection and passivation of the surface of the semiconductor device layer by the plasma, and improve the roughness of the AlGaN surface and other film layers of the semiconductor device after the front-end etching.

[0072] In one example, the process parameters when the first process gas is introduced into the process chamber include: the gas pressure range in the process chamber is 2000-2300mT, the power includes 250-300W, the flow range of N2 is 4000-5000sccm, and the flow range of NH3 is 200-250sccm.

[0073] In one embodiment, after depositing the second film layer 212 on the first film layer 211 with a second deposition gas, the passivation film preparation method further includes: introducing a second process gas into the process chamber, wherein the second process gas includes an oxygen-containing gas; and the oxygen-containing gas is used to perform plasma bombardment on the second film layer to remove dangling bonds on the surface of the second film layer. Optionally, the oxygen-containing gas may include O2.

[0074] Optionally, the second process gas may further include a purge gas such as N 2 , etc. The purge gas is used to eliminate particles in and / or on the surface of the first film layer 211 and the second film layer 212 .

[0075] In this embodiment, after forming the second film layer 212, the second process gas is introduced into the process chamber, and the corresponding plasma bombards the second film layer 212, which can remove impurities such as dangling bonds on the surface of the second film layer 212, avoid the generation of gaps in the subsequent film layer deposition process, and can densify the relevant film layers. The second process gas can also include a purge gas such as N2, so that the process chamber is filled and pumped by the purge gas in the second process gas, remove byproducts in the deposition process, and optimize the overall environment of the process chamber.

[0076] In one example, after the third film layer 213 is deposited on the second film layer 212 with the third deposition gas, the passivation film preparation method further includes: introducing the second process gas into the process chamber to perform plasma bombardment on the third film layer 213 to remove dangling bonds on the surface of the third film layer 213. In this example, after the third film layer 213 is formed, the second process gas is introduced into the process chamber, and the corresponding plasma bombards the third film layer 213, which can remove impurities such as dangling bonds on the surface of the third film layer 213, avoid the generation of gaps in the subsequent film layer deposition process, and can densify the related film layers. The process chamber can also be filled and pumped by the purge gas in the second process gas to remove by-products in the deposition process and optimize the overall environment of the process chamber.

[0077] In one example, after depositing the fourth film layer 214 on the third film layer 213 with the fourth deposition gas, the passivation film preparation method further includes: introducing the second process gas into the process chamber, breaking down the second process gas to form plasma, and allowing the plasma to bombard the fourth film layer 214 to remove particles on the surface of the fourth film layer 214 and reduce surface defects of the fourth film layer 214. In this example, after forming the fourth film layer 214, the second process gas is introduced into the process chamber, and the corresponding plasma bombards the fourth film layer 214, which can remove particles on the surface of the fourth film layer 214 and consolidate the surface state of the film layer, thereby forming a film layer structure with low film layer particles and high passivation performance.

[0078] In one example, the second process gas also includes a purge gas, which is used to remove particles on the surface of the film layer; wherein the ratio of the purge gas to the oxygen-containing gas is in the range of 50:1 to 60:1. If the oxygen-containing gas includes O2, the purge gas includes N2, and the ratio of N2 to O2 is in the range of 50:1 to 60:1; the second process gas contains a large amount of N2, and a large amount of N2 is used to fill and pump the process chamber, which can purge the surface particles of the corresponding film layer after each deposition, thereby reducing the generation of particles in the deposition process; and the N2 in the second process gas can also promote the dissociation of O2 to form a mixed plasma of N2 and O2, thereby removing and passivating the dangling bonds on the surface of the corresponding film layer, and at the same time, the O ions can further react with the H ions on the surface of the SiON film layer (i.e., the fourth film layer 214), supplement the surface defects of the film layer, and reduce the escape of H ions during the later annealing process, thereby achieving the effect of reducing defects and reducing the roughness of the film layer.

[0079] In one example, the process parameters when the second process gas is introduced into the process chamber include: the gas pressure range in the process chamber is 2000-2300mT, the power supply power includes 250-300W, the flow range of the purge gas is 4000-5000sccm, and the flow range of the oxygen-containing gas is 80-100sccm.

[0080] In one example, the above passivation film preparation method can also refer to Figure 5 As shown, it includes steps S301 to S310.

[0081] S301, transporting the semiconductor device to be processed into a PECVD chamber through a transport mechanism for preheating.

[0082] S302, introducing a first process gas into the PECVD chamber for pre-deposition treatment.

[0083] S303, depositing an ammonia-free SiNx layer on the surface of the semiconductor device using a first deposition gas including SiH4 and N2.

[0084] S304 , an ammonia SiNx layer is deposited on the surface of the ammonia-free SiNx layer using a second deposition gas including SiH 4 , N 2 , and NH 3 .

[0085] S305, introducing a second process gas into the PECVD chamber, breaking down the second process gas to perform a second plasma treatment.

[0086] S306, depositing a SiO2 film layer on the surface of the ammonia-containing SiNx layer using a third deposition gas including SiH4, N2O and N2.

[0087] S307, introducing a second process gas into the PECVD chamber, breaking down the second process gas to perform a second plasma treatment.

[0088] S308, depositing a SiOxNy layer on the surface of the SiO2 film layer using a fourth deposition gas including SiH4, N2O, NH3 and N2.

[0089] S309, introducing a second process gas into the PECVD chamber for post-deposition treatment.

[0090] S310, performing other purges on the semiconductor device, and ending the process flow.

[0091] Among them, steps S303, S304, S306 and S308 are main deposition steps, and steps S305 and S307 are auxiliary deposition steps. The main deposition step can deposit the main passivation film layer, and the auxiliary deposition step is used to remove interface particles, improve the upper surface ion state between film layers, increase the adhesion of the film layer, and consolidate the passivation performance of the film layer, ensure the stress matching between the film layers, and avoid the occurrence of film layer splitting and other conditions. Further, when configuring the preparation parameters of the above-mentioned passivation film in the software interface, the various parameters involved in each step can be configured at one time to achieve an integrated formula. When depositing the formula, it only needs to be set once in the software interface before executing the deposition process, which can maintain the stability of the process environment temperature, so that each deposition step can avoid intermediate pauses, wherein N2 can be continuously output, stably filling and pumping the PECVD chamber to clean, and further reduce the particle size of the surface of the semiconductor device in the PECVD chamber.

[0092] Through the above steps S301 to S310, a passivation film layer with a total thickness of 7000A±100nm can be deposited on the surface of the corresponding semiconductor device, and the coating effect is good. The surface after passivation is flat and uniform. The inventor compares the stacked passivation film formed by the present application with the SiNx film layer formed by other schemes. The relevant comparison can be referred to Figure 6 As shown, compared with the SiNx film layer, the surface roughness of the laminated passivation film is reduced by 30%, and the surface particle state of the laminated passivation film has been greatly improved. It can be seen that the passivation film prepared by the passivation film preparation method of the present application has fewer film particles, can better control the generation of particles in the film layer and on the surface, and the roughness of the film layer surface is improved. Through the film layer interface treatment and surface passivation reaction, it can effectively isolate the oxygen and water vapor outside the device, and reduce the leakage probability of the corresponding semiconductor device.

[0093] The above analysis and characterization show that the above passivation film preparation method has the following advantages:

[0094] (1) Before deposition, the first process gas is introduced to perform surface treatment on the semiconductor device, wherein NH3 releases H ions after plasma bombardment and reacts with the oxide film layer of the semiconductor device. N2 promotes the dissociation of NH3 and takes away related by-products, thereby enhancing the surface protection and passivation of the device layer. This can effectively prevent H ions from entering the interior of the semiconductor device, enhance the protection and passivation of the surface of the semiconductor device layer by plasma, and improve the roughness of the film layer such as the AlGaN surface of the semiconductor device after the front-end etching.

[0095] (2) The entire passivation film preparation process adopts step-by-step deposition. The main passivation film layer is deposited through the main deposition step, and the interface particles are removed in the secondary deposition step, which improves the upper surface ion state between the film layers, increases the adhesion of the film layer, and consolidates the passivation performance of the film layer, so that the stress between each film layer is more matched, which can avoid the occurrence of film layer splitting and other conditions.

[0096] (3) The ammonia-free SiNx layer is used as the bottom film layer, and the ammonia-containing SiNx layer, SiO2 film layer and SiOxNy film layer are sequentially included upwards. This structure is used as a new passivation film structure. The surface roughness of the obtained passivation film layer is improved, which can effectively isolate the oxygen and water vapor around the device and reduce the leakage probability of the corresponding semiconductor device.

[0097] (4) After the deposition of each film layer is completed, the second process gas is continuously introduced into the process chamber to further remove the particles of the film layer and consolidate the surface state of the film layer, thereby obtaining a film layer structure with low film layer particles and high passivation performance.

[0098] A second aspect of the present application further provides a semiconductor device, comprising:

[0099] Semiconductor device film structure;

[0100] A passivation film is located on the surface of the film layer structure, and the passivation film is prepared by the passivation film preparation method described in any of the above embodiments.

[0101] Specifically, the film layer structure of the semiconductor device is a high electron mobility transistor. In this case, the semiconductor device can be as follows: Figure 4 As shown, it includes a high electron mobility transistor 220 and a passivation film 210 located on the surface of the high electron mobility transistor 220 .

[0102] The film structure of the semiconductor device is described below by taking a high electron mobility transistor 220 as an example. The high electron mobility transistor 220 may include a transistor such as AlGaN / GaN HEMT; Figure 4 As shown, the high electron mobility transistor 220 may include structures such as a substrate, a GaN buffer layer, an AlGaN barrier layer, and a GaN cap layer. Functional regions such as a source, a drain, and a gate may also be provided in the high electron mobility transistor 220 .

[0103] The passivation film is prepared by the passivation film preparation method described in any of the above embodiments, and has all the beneficial effects of the passivation film preparation method described in any of the above embodiments, which will not be repeated here.

[0104] The above is a detailed introduction to a passivation film preparation method and a semiconductor device provided by the present application. This article uses specific examples to illustrate the principles and implementation methods of the present application. It should be noted that in the present application, the descriptions of each embodiment have their own emphasis. For parts that are not described or recorded in detail in a certain embodiment, please refer to the relevant descriptions of other embodiments.

[0105] Although the present application has been shown and described with respect to one or more implementations, equivalent variations and modifications will occur to those skilled in the art based on reading and understanding of this specification and the accompanying drawings. The present application includes all such modifications and variations and is limited only by the scope of the appended claims. In particular, with respect to the various functions performed by the above-mentioned components, the terms used to describe such components are intended to correspond to any component (unless otherwise indicated) that performs the specified function of the component (e.g., it is functionally equivalent), even if it is not structurally equivalent to the disclosed structure that performs the functions in the exemplary implementation of this specification shown herein.

[0106] That is, the above description is only an embodiment of the present application, and does not limit the patent scope of the present application. Any equivalent structure or equivalent process transformation made using the contents of the description and drawings of the present application, such as the mutual combination of technical features between the embodiments, or direct or indirect application in other related technical fields, are also included in the patent protection scope of the present application.

[0107] In addition, although the terms first, second, etc. may be used to describe various information in this article, this information should not be limited to these terms. These terms are only used to distinguish information of the same type from each other. The terms "first" and "second" should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more features. In the description of this application, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.

[0108] In this application, the word "exemplary" is used to mean "used as an example, illustration or description". Any embodiment described as "exemplary" in this application is not necessarily to be construed as being more preferred or more advantageous than other embodiments. In order to enable any technician in the field to implement and use the present application, the present application provides the above description. In the above description, various details are listed for the purpose of explanation. It should be understood that a person of ordinary skill in the art can recognize that the present application can be implemented without using these specific details. In other embodiments, well-known structures and processes will not be elaborated in detail to avoid unnecessary details that make the description of the present application obscure. Therefore, the present application is not intended to be limited to the embodiments shown, but is consistent with the widest range of principles and features disclosed in the present application.

Claims

1. A method for preparing a passivation film, It is characterized in that The steps include: A first film layer is deposited on the substrate using a first deposition gas, wherein the first deposition gas comprises SiH 4 and N 2 , the first film layer is ammonia-free silicon nitride; A second film layer is deposited on the first film layer using a second deposition gas, wherein the second deposition gas comprises SiH 4 、N 2 and NH 3 , the second film layer is ammonia silicon nitride.

2. The method for preparing a passivation film according to claim 1, It is characterized in that The passivation film preparation method also includes: Depositing a third film layer on the second film layer using a third deposition gas, wherein the third film layer is silicon oxide; The second film layer has compressive stress, and the compressive stress of the third film layer is smaller than that of the second film layer.

3. The method for preparing a passivation film according to claim 2, It is characterized in that The passivation film preparation method also includes: Depositing a fourth film layer on the third film layer using a fourth deposition gas, wherein the fourth film layer is silicon oxynitride; The compressive stress of the fourth film layer is smaller than that of the third film layer.

4. The method for preparing a passivation film according to claim 3, It is characterized in that The fourth deposition gas includes NH 3 , used to introduce Si-H bonds into the fourth film layer.

5. The method for preparing a passivation film according to claim 4, It is characterized in that The fourth deposition gas also includes N 2 O, by adjusting NH 3 / N 2 O ratio to adjust the stress of the fourth film layer.

6. The method for preparing a passivation film according to claim 1, It is characterized in that Before depositing the first film layer on the substrate with the first deposition gas, the passivation film preparation method further includes: A first process gas is introduced into the process chamber to perform plasma bombardment cleaning on the surface to be deposited of the first film layer; the first process gas comprises N 2 and NH 3 .

7. The method for preparing a passivation film according to claim 6, It is characterized in that The first process gas contains N 2 and NH 3 The ratio range includes: 20:1 to 50:

1.

8. The method for preparing a passivation film according to claim 6, It is characterized in that The process parameters when the first process gas is introduced into the process chamber include: the gas pressure in the process chamber is in the range of 2000 to 2300 mT, the power supply power is in the range of 250 to 300 W, N 2 The flow rate range is 4000-5000sccm, NH 3 The flow rate range is 200-250sccm.

9. The method for preparing a passivation film according to claim 3, It is characterized in that After depositing the second film layer on the first film layer with a second deposition gas, the passivation film preparation method further includes: introducing a second process gas into the process chamber, wherein the second process gas comprises an oxygen-containing gas; The oxygen-containing gas is used to perform plasma bombardment on the second film layer to remove dangling bonds on the surface of the second film layer.

10. The method for preparing a passivation film according to claim 9, It is characterized in that After depositing a third film layer on the second film layer with a third deposition gas, the passivation film preparation method further includes: The second process gas is introduced into the process chamber to perform plasma bombardment on the third film layer to remove dangling bonds on the surface of the third film layer.

11. The method for preparing a passivation film according to claim 9, It is characterized in that After depositing a fourth film layer on the third film layer with a fourth deposition gas, the passivation film preparation method further includes: The second process gas is introduced into the process chamber to perform plasma bombardment on the fourth film layer to remove surface defects of the fourth film layer.

12. The method for preparing a passivation film according to any one of claims 9 to 11, It is characterized in that The second process gas also includes a purge gas for removing particles on the surface of the film layer; wherein the ratio of the purge gas to the oxygen-containing gas is in the range of 50:1 to 60:

1.

13. The method for preparing a passivation film according to claim 12, It is characterized in that The process parameters when the second process gas is introduced into the process chamber include: the gas pressure range in the process chamber is 2000-2300mT, the power includes 250-300W, the flow range of the purge gas is 4000-5000sccm, and the flow range of the oxygen-containing gas is 80-100sccm.

14. The method for preparing a passivation film according to claim 1, It is characterized in that The thickness of the first film layer is in the range of 300-400 Å; and / or the refractive index of the first film layer is in the range of 1.95-2.

05.

15. The method for preparing a passivation film according to claim 1, It is characterized in that The process parameters for depositing the first film layer include: the pressure range of the process chamber is 1500-2000 mT, the power of the power source is 250-300 W, N 2 The flow rate range is 5000-6000sccm, SiH 4 The flow rate range is 100-200sccm.

16. The method for preparing a passivation film according to claim 1, It is characterized in that The thickness of the second film layer is in the range of 600-700 Å; and / or the refractive index of the second film layer is in the range of 1.95-2.

05.

17. The method for preparing a passivation film according to claim 1, It is characterized in that The process parameters for depositing the second film layer include: the pressure range of the process chamber is 1500-2000 mT, the power supply power is 250-300 W, N 2 The flow rate range is 5000-6000sccm, SiH 4 The flow rate range is 100-200sccm, NH 3 The flow rate range is 100-200sccm.

18. The method for preparing a passivation film according to claim 2, It is characterized in that The thickness of the third film layer is in the range of 4000-5000A; and / or the refractive index of the third film layer is in the range of 1.455-1.

465.

19. The method for preparing a passivation film according to claim 5, It is characterized in that The process parameters for depositing the third film layer include: the pressure range of the process chamber is 1500-2000 mT, the power supply power includes 250-300 W, N 2 The flow rate range is 5000-6000sccm, SiH 4 The flow rate range is 100-200sccm, N 2 The flow rate of O is in the range of 4000-5000 sccm.

20. The method for preparing a passivation film according to claim 3, It is characterized in that The thickness of the fourth film layer is in the range of 2000-3000A; and / or the refractive index of the fourth film layer is in the range of 1.70-1.

90.

21. The method for preparing a passivation film according to claim 5, It is characterized in that The process parameters for depositing the fourth film layer include: the pressure range of the process chamber is 1500-2000 mT, the power supply power includes 250-300 W, N 2 The flow rate range is 5000-6000sccm, SiH 4 The flow rate range is 100-200sccm, N 2 The flow rate range of O is 1000-2000sccm, NH 3 The flow rate range is 100-200sccm.

22. A semiconductor device, It is characterized in that include: Semiconductor device film structure; A passivation film located on the surface of the film layer structure, wherein the passivation film is prepared by the passivation film preparation method according to any one of claims 1 to 21.