Negative electrode active material and preparation method thereof, metal lithium negative electrode and metal lithium battery
By depositing metal lithium in NiO@NiOx co-doped carbon nanocage, the problems of poor deposition uniformity and circulation performance of metal lithium anode lithium are solved, and efficient battery circulation performance and safety improvement are achieved.
Patent Information
- Application Number
- CN202310558604.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-17
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-05-17
AI Technical Summary
The poor lithium deposition uniformity and poor circulation performance of metal lithium negative electrodes during charging and discharging lead to safety hazards and thermal runaway from the battery, making it difficult to achieve commercial application.
NiO@NiOx co-doped carbon nanocage is used as the negative electrode active material. By depositing metal lithium in its cage cavity, NiO and nitrogen oxide heteroatoms are used to improve lithium philtrum, inhibit the growth of lithium dendrites, and enhance the cycle life of the battery.
The uniform deposition and high circulation performance of metal lithium are achieved, the Coulombic efficiency and stability of the battery are improved, the risk of side reactions is reduced, and the safety of the battery is enhanced.
Smart Images

Figure CN119008943A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of electrochemical technology, and in particular to a negative electrode active material and a preparation method thereof, a metal lithium negative electrode and a metal lithium battery. Background Art
[0002] In recent years, lithium metal anodes have received extensive attention from battery researchers due to the characteristics of lithium metal such as high theoretical specific capacity and low electrode potential. However, there are also many problems. On the one hand, due to the high reactivity of lithium metal, it is easy to react with organic electrolytes, and a large amount of gas will be produced, which will lead to a decrease in the utilization rate of lithium metal and electrolyte, and it is easy to bring safety hazards. Secondly, after multiple charge and discharge of the battery, lithium dendrites will continue to grow on the surface of lithium metal. A large number of dendrites have a large stress on the diaphragm, causing the diaphragm to be pierced, thereby causing thermal runaway of the battery. In addition, the unlimited volume expansion of lithium metal will also lead to various problems such as lithium electrode pulverization, electrolyte consumption, and large-scale gas production. These problems make it difficult for lithium metal anodes to be commercially applied.
[0003] In order to solve the above problems, the main technical routes adopted in the prior art include: developing modified electrolytes, negative electrode surface passivation modification, and developing composite negative electrode materials. However, the methods of modified electrolytes and negative electrode surface passivation modification are often only applicable to battery systems with specific electrolytes and positive and negative electrodes. At the same time, the process is cumbersome and the cost is high. In the development of composite negative electrode materials, three-dimensional nanomaterials with a certain strength and stable structure are used as current collectors to form composite negative electrodes with metallic lithium. However, the carbon nanonetworks that are currently widely studied have poor lithium affinity, and metallic lithium is deposited on the surface, so that lithium is still in an exposed state, which is easy to react with the electrolyte, and the effect is not good in practical applications. Summary of the invention
[0004] The purpose of the present invention is to overcome the problems of poor uniformity of lithium deposition and poor cycle performance of metal lithium negative electrodes during the charge and discharge process in the prior art, and to provide a negative electrode active material and a preparation method thereof, a metal lithium negative electrode and a metal lithium battery. The negative electrode active material can deposit lithium uniformly and has excellent cycle performance.
[0005] In order to achieve the above-mentioned object, the first aspect of the present invention provides a negative electrode active material, the negative electrode active material comprises NiO@nitrogen-oxygen co-doped carbon nanocage, and metallic lithium filled in the cage cavity of the NiO@nitrogen-oxygen co-doped carbon nanocage;
[0006] The X-ray photoelectron spectroscopy shows that the molar content of nickel in the NiO@nitrogen-oxygen co-doped carbon nano cage is not less than 0.5%, and the molar content ratio of oxygen to nickel is 0.5-20:1.
[0007] A second aspect of the present invention provides a method for preparing a negative electrode active material, the method comprising:
[0008] (1) providing a homogeneous solution containing a Ni salt, ethylenediaminetetraacetic acid and a solvent, and then removing the solvent from the homogeneous solution to obtain a precursor; the mass ratio of the Ni salt to the ethylenediaminetetraacetic acid is 1:0.1-100;
[0009] (2) subjecting the precursor to a first pyrolysis under an inert atmosphere and / or a reducing atmosphere to obtain a first pyrolysis product;
[0010] (3) contacting the first pyrolysis product with an oxygen-containing acid and then drying it;
[0011] (4) Under an inert atmosphere, subjecting the product obtained in step (3) to a second pyrolysis to obtain NiO@nitrogen-oxygen co-doped carbon nanocages; the temperature of the second pyrolysis is 250-400° C.;
[0012] (5) depositing metallic lithium onto the NiO@nitrogen-oxygen co-doped carbon nanocage by electrodeposition.
[0013] The third aspect of the present invention provides a metal lithium negative electrode, the metal lithium negative electrode comprising a current collector and an active layer composited on the current collector, the active layer comprising an active material, a binder and an optional conductive agent;
[0014] The active material includes the negative electrode active material described in the first aspect or the negative electrode active material prepared by the preparation method described in the second aspect.
[0015] A fourth aspect of the present invention provides a metal lithium battery, which includes the metal lithium negative electrode described in the third aspect.
[0016] The negative electrode active material provided by the present invention includes NiO@nitrogen-oxygen co-doped carbon nanocage, and metallic lithium filled in the cage cavity of the NiO@nitrogen-oxygen co-doped carbon nanocage. On the one hand, the NiO@nitrogen-oxygen co-doped carbon nanocage has the characteristics of small particle size and large curvature. At the same time, by utilizing the NiO on its inner surface, the nucleation sites of metallic lithium can be increased, the lithium affinity can be improved, and it is beneficial to induce metallic lithium to enter the interior of the carbon nanocage for deposition. On the other hand, the presence of NiO and nitrogen-oxygen heteroatoms in the carbon nanocage can uniformly deposit metallic lithium, effectively inhibit the growth of metallic lithium dendrites during the charge and discharge process, and improve the battery cycle life. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 is a TEM image of the NiO@nitrogen and oxygen co-doped carbon nanocage prepared in Example 1;
[0018] Figure 2 is the XPS image of NiO@nitrogen and oxygen co-doped carbon nanocage prepared in Example 1;
[0019] Figure 3 is the XPS O1s spectrum of NiO@nitrogen and oxygen co-doped carbon nanocage prepared in Example 1;
[0020] Figure 4 This is a SEM image of the metal lithium negative electrode after cycling in Example 1. DETAILED DESCRIPTION
[0021] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0022] The first aspect of the present invention provides a negative electrode active material, the negative electrode active material comprising NiO@nitrogen-oxygen co-doped carbon nanocage, and metallic lithium filled in the cage cavity of the NiO@nitrogen-oxygen co-doped carbon nanocage;
[0023] The X-ray photoelectron spectroscopy shows that the molar content of nickel in the NiO@nitrogen-oxygen co-doped carbon nano cage is not less than 0.5%, and the molar content ratio of oxygen to nickel is 0.5-20:1.
[0024] In the present invention, it can be understood that the NiO@nitrogen-oxygen co-doped carbon nanocage has a hollow cage structure surrounded by a NiO@nitrogen-oxygen co-doped graphitized carbon layer, including NiO and a nitrogen-oxygen co-doped graphitized carbon layer, and the graphitized carbon layer refers to a carbon structure with a layered structure that can be clearly observed under a high-resolution transmission electron microscope, rather than an amorphous structure.
[0025] In the present invention, the "nitrogen" and "oxygen" in the term "NiO@nitrogen-oxygen co-doped carbon nanocage" refer to nitrogen and oxygen elements, that is, nitrogen and oxygen elements in various forms formed in the graphitized carbon layer during the preparation process of NiO@nitrogen-oxygen co-doped carbon nanocage. Through X-ray photoelectron spectroscopy testing and analysis based on the 2p orbital of Ni, it can be proved that NiO species exist in NiO@nitrogen-oxygen co-doped carbon nanocage. In addition, there may be Ni 2+ The Ni element exists in the form of NiO. According to the ion diffusion and fixation process during the preparation process, it can be inferred that the formed NiO is located on the inner surface of the nitrogen-oxygen co-doped carbon nanocage.
[0026] In the present invention, the “molar content of nickel” is the total content of nickel elements in all forms, the “molar content of oxygen” is the total content of oxygen elements in all forms, and similarly, the “molar content of nitrogen” is the total content of nitrogen elements in all forms.
[0027] The hollow carbon cages used as carriers of negative electrode lithium in the prior art have many problems, such as large particle size, poor lithium affinity, harsh preparation conditions, complex process, poor compatibility with existing battery systems, poor operability, etc. At the same time, the unmodified graphite hollow carbon cages have the characteristics of being lithium-phobic, and the outer shell layer has a high density, which is not conducive to the deposition of metallic lithium, resulting in poor cycle performance.
[0028] The negative electrode active material provided by the present invention includes NiO@nitrogen-oxygen co-doped carbon nanocage, and metallic lithium filled in the cage cavity of the NiO@nitrogen-oxygen co-doped carbon nanocage. On the one hand, the NiO@nitrogen-oxygen co-doped carbon nanocage has the characteristics of small particle size and large curvature. At the same time, by utilizing the NiO on its inner surface, the nucleation sites of metallic lithium can be increased, the lithium affinity is improved, and it is beneficial to induce metallic lithium to enter the interior of the carbon nanocage for deposition. On the other hand, the presence of NiO and nitrogen-oxygen heteroatoms in the carbon nanocage can uniformly deposit metallic lithium, effectively inhibit the growth of metallic lithium dendrites during the charge and discharge process, and improve the battery cycle life. In addition, the inventors of the present invention also found that the negative electrode active material can maintain a high coulombic efficiency during the cycle process. The reason for this may be that the SEI interface formed by the NiO-rich carbon nanocage during the lithium deposition process is more stable, which is beneficial to reduce the side reactions of metallic lithium and the electrolyte, thereby improving the coulombic efficiency.
[0029] According to the present invention, preferably, the molar content of carbon in the NiO@nitrogen-oxygen co-doped carbon nanocage measured by X-ray photoelectron spectroscopy is 50-88.5%, preferably 60-88%; the molar content of nickel is 0.5-10%, preferably 1-5%; the molar content of oxygen is 1-31%, preferably 5-15%; and the molar content of nitrogen is 1-10%, preferably 3-10%.
[0030] In the present invention, preferably, the oxygen content in the NiO@nitrogen-oxygen co-doped carbon nanocage is relatively high, and the oxygen content in the carbon cage or carbon hollow sphere used in the metal lithium negative electrode material disclosed in the prior art is relatively low. The inventors of the present invention have found in their research that co-doping the carbon nanocage with NiO, oxygen and nitrogen is beneficial to increasing the lithium affinity, thereby uniformly depositing metal lithium, and further controlling the molar content of nickel, oxygen and nitrogen in the carbon nanocage, which can improve the cycle stability of the metal lithium negative electrode active material.
[0031] In a further preferred embodiment, the molar ratio of oxygen to nitrogen in the NiO@nitrogen-oxygen co-doped carbon nanocage is 2.5-6:1 as measured by X-ray photoelectron spectroscopy. For example, it can be any ratio such as 2.5:1, 3:1, 3.5:1, 4:1, 4.5:1, 5:1, 5.5:1, 6:1, or a range therebetween. In the above preferred case, it is beneficial to further improve the cycle life of the negative electrode material.
[0032] Preferably, the molar ratio of oxygen to nickel in the NiO@nitrogen-oxygen co-doped carbon nanocage measured by X-ray photoelectron spectroscopy is 5-10:1, for example, it can be any ratio of 5:1, 5.5:1, 6:1, 6.5:1, 7:1, 7.5:1, 8:1, 8.5:1, 9:1, 9.5:1, 10:1, etc., or a range therebetween. In the above preferred case, it is beneficial to further improve the cycle life and coulombic efficiency of the negative electrode active material.
[0033] According to the present invention, preferably, the oxygen species in the NiO@nitrogen-oxygen co-doped carbon nanocage measured by X-ray photoelectron spectroscopy include carboxyl oxygen, hydroxyl oxygen and ether oxygen. In the present invention, the terms "carboxyl oxygen", "hydroxyl oxygen" and "ether oxygen" have conventional meanings in the art, specifically referring to: carboxyl oxygen is an oxygen species determined by a characteristic peak corresponding to a binding energy of 533-534 eV in the X-ray photoelectron spectrum; hydroxyl oxygen is an oxygen species determined by a characteristic peak corresponding to a binding energy of 531-532 eV in the X-ray photoelectron spectrum; ether oxygen is an oxygen species determined by a characteristic peak corresponding to a binding energy of 530-530.9 eV in the X-ray photoelectron spectrum.
[0034] Preferably, the molar ratio of carboxyl oxygen, hydroxyl oxygen and ether oxygen is 1-2:1-5:1-2. For example, it can be 1:1:1, 1:2:1, 1:3:1, 1:4:1, 1:5:1, 1:1:2, 1:2:2, 1:3:2, 1:4:2, 1:5:2 and other specific ratios, preferably 1-1.5:1-1.8:1. The molar content of carboxyl oxygen, hydroxyl oxygen and ether oxygen is calculated by peak area of X-ray photoelectron spectroscopy.
[0035] In the present invention, the X-ray photoelectron spectroscopy analysis was tested on an ESCALab250 X-ray photoelectron spectrometer equipped with ThermoAvantage V5.926 software from Thermo Scientific. The excitation source was monochromatic AlKα X-ray with an energy of 1486.6 eV and a power of 150 W. The penetration energy used for narrow scanning was 30 eV. The basic vacuum during the analysis test was 6.5×10 -10 The electron binding energy was calibrated with the C1s peak (284.6 eV) of elemental carbon. The data were processed on Thermo Avantage software, and the sensitivity factor method was used for quantitative analysis in the analysis module.
[0036] According to the present invention, preferably, the diameter of the NiO@nitrogen-oxygen co-doped carbon nanocage is 2-50 nm, preferably 10-50 nm, and more preferably 10-30 nm; the NiO@nitrogen-oxygen co-doped carbon nanocage has a smaller diameter and a larger curvature, which is beneficial to the transport and deposition of metallic lithium.
[0037] Preferably, the thickness of the cage wall of the NiO@nitrogen and oxygen co-doped carbon nanocage is 1-50 nm, preferably 1-30 nm, and more preferably 1-20 nm.
[0038] In the present invention, the diameter of the NiO@nitrogen-oxygen co-doped carbon nanocage and the thickness of the cage wall of the NiO@nitrogen-oxygen co-doped carbon nanocage can be measured by high-resolution transmission electron microscopy images. The model of the high-resolution transmission electron microscope used is JEM-2100 (Japan Electron Co., Ltd.), and the high-resolution transmission electron microscope test conditions are: the acceleration voltage is 200kV.
[0039] According to the present invention, the NiO@nitrogen-oxygen co-doped carbon nanocage has a loose and porous cage wall, which is conducive to the filling and deposition of metallic lithium. Preferably, the pore volume of the cage wall of the NiO@nitrogen-oxygen co-doped carbon nanocage is 0.1-1 cm 3 / g, preferably 0.1-0.5cm 3 / g.
[0040] Preferably, the specific surface area of the NiO@nitrogen-oxygen co-doped carbon nanocage is 50-1000 m 2 / g, preferably 200-800m 2 / g, more preferably 300-600m 2 / g.
[0041] In the present invention, the pore structure properties of the material are detected by the BET test method. Specifically, the Quantachrome AS-6B analyzer is used for the measurement, and the BET specific surface area of the material is obtained by the Brunauer-Emmett-Taller (BET) method.
[0042] According to the present invention, preferably, based on the total amount of the NiO@nitrogen and oxygen co-doped carbon nanocages and metallic lithium, the content of metallic lithium is 2-90wt%, preferably 2-50wt%.
[0043] A second aspect of the present invention provides a method for preparing a negative electrode active material, the method comprising:
[0044] (1) providing a homogeneous solution containing a Ni salt, ethylenediaminetetraacetic acid and a solvent, and then removing the solvent from the homogeneous solution to obtain a precursor; the mass ratio of the Ni salt to the ethylenediaminetetraacetic acid is 1:0.1-100;
[0045] (2) subjecting the precursor to a first pyrolysis under an inert atmosphere and / or a reducing atmosphere to obtain a pyrolysis product;
[0046] (3) contacting the pyrolysis product with an oxygen-containing acid and then drying it;
[0047] (4) Under an inert atmosphere, subjecting the product obtained in step (3) to a second pyrolysis to obtain NiO@nitrogen-oxygen co-doped carbon nanocages; the temperature of the second pyrolysis is 250-400° C.;
[0048] (5) depositing metallic lithium onto the NiO@nitrogen-oxygen co-doped carbon nanocage by electrodeposition.
[0049] In the present invention, a precursor prepared by reacting a Ni salt and ethylenediaminetetraacetic acid in a solvent is first pyrolyzed at a relatively low temperature, and then contacted with an oxygen-containing acid so that the nickel exists in the form of a nickel acid salt. Then, a second pyrolysis is performed so that at least a portion of the nickel acid salt is converted into nickel oxide, which is attached to the inner surface of the nitrogen-oxygen co-doped carbon nanocage.
[0050] According to a specific embodiment of the present invention, in step (3), the product obtained by contacting the first pyrolysis product with the oxygen-containing acid is directly dried after optional solid-liquid separation. The present invention does not include a washing step, so that at least part of the nickel oxygen-containing acid salt is retained in the carbon cage.
[0051] According to the present invention, preferably, in step (1), the mass ratio of the Ni salt to EDTA is 1:0.5-50, preferably 1:0.5-5.
[0052] The present invention has no particular limitation on the specific method of forming the homogeneous solution in step (1), for example, the homogeneous solution may be formed by heating, preferably by heating and stirring. The present invention also has no particular limitation on the heating temperature and stirring rate, as long as the homogeneous solution can be formed.
[0053] According to the present invention, preferably, the Ni salt and ethylenediaminetetraacetic acid are dissolved in a solvent to form a homogeneous solution. The present invention has no particular limitation on the type of the solvent, which is subject to the ability to form a homogeneous solution. Preferably, the solvent is water and / or ethanol, more preferably water; the present invention has no particular limitation on the amount of the solvent, which is also subject to the ability to form a homogeneous solution.
[0054] In the present invention, the solvent in the homogeneous solution can be removed by existing techniques known to those skilled in the art, and the present invention has no particular limitation on this. For example, the solvent in the homogeneous solution can be removed by heating and evaporating to dryness.
[0055] In the present invention, there is no particular limitation on the specific type of the Ni salt. Preferably, the Ni salt is selected from organic acid salts and / or inorganic salts of Ni; preferably, the organic acid salt of Ni is an organic carboxylate free of heteroatoms, preferably nickel acetate; preferably, the inorganic salt of Ni is at least one of nickel chloride, nickel carbonate and basic nickel carbonate.
[0056] In the present invention, preferably, the temperature of the first pyrolysis is not higher than 450°C. In the prior art, in order to ensure that the carbon coating has a high degree of graphitization, the calcination or heat treatment temperature generally used is not less than 600°C. A high degree of graphitization is conducive to improving the conductivity of the material. However, the inventors of the present invention have found in their research that a lower calcination temperature can increase the oxygen content in the material. Under the synergistic effect of NiO and oxygen and nitrogen atoms, it is conducive to improving the lithium affinity, further uniform deposition of metallic lithium, and further helping to improve the cycle performance of the metallic lithium negative electrode. Preferably, in step (2), the first pyrolysis conditions include: a heating rate of 0.5-30°C / min, preferably 1-10°C / min; a temperature of 350-450°C, preferably 350-400°C; for example, it can be a specific temperature of 350°C, 360°C, 370°C, 380°C, 390°C, 400°C, or a temperature range between two points. Preferably, the constant temperature time is 20-600min, preferably 60-480min. The use of the above preferred first pyrolysis conditions is conducive to taking into account the appropriate graphitization degree and oxygen doping amount of the NiO@nitrogen-oxygen co-doped carbon nanocages, further improving the cycle life of the negative electrode active material.
[0057] In the present invention, preferably, in step (2), the inert atmosphere is provided by at least one of nitrogen, argon, neon and helium. Preferably, the reducing atmosphere is hydrogen.
[0058] In step (2) of the present invention, the first pyrolysis product is contacted with an acid and then dried, so that nickel is attached to the inner surface of the nitrogen-oxygen co-doped carbon nanocage in the form of nickel oxyacid salt.
[0059] In a further preferred embodiment, the product obtained by contacting the pyrolysis product with the acid is directly dried after optional solid-liquid separation, without a washing step, to minimize the loss of Ni element. The solid-liquid separation can be carried out in a conventional manner in the art, as long as the remaining acid is removed, for example, solid-liquid separation can be carried out by filtering, suction filtration, centrifugation, etc.
[0060] According to the present invention, preferably, in step (3), the oxygen-containing acid is provided by an aqueous solution of nitric acid; the concentration of the aqueous solution of nitric acid is 0.5-2 mol / L, preferably 0.5-1 mol / L. The present invention has no particular limitation on the amount of the oxygen-containing acid, as long as it can fully convert nickel into an oxygen-containing acid salt of nickel, and those skilled in the art can select it according to actual conditions.
[0061] Preferably, in step (3), the contacting temperature is 20-110°C, preferably 60-90°C; and the contacting time is 0.1-48h, preferably 4-12h.
[0062] Preferably, in step (3), the drying is used to remove the clear water introduced by the acid in the product. The drying method can be atmospheric drying or reduced pressure drying, and the drying conditions can be any feasible existing technology, preferably, the drying is carried out at 80-140°C.
[0063] In the present invention, the second pyrolysis in step (4) is used to thermally decompose the nickel oxygenate to form NiO. The present invention has a wide range of conditions for the second pyrolysis, as long as the above-mentioned purpose can be achieved.
[0064] Preferably, in step (4), the second pyrolysis conditions include: a heating rate of 0.5-15°C / min, preferably 1-10°C / min; a temperature of 250-350°C, preferably 300-350°C; and a constant temperature time of 20-600min, preferably 60-480min.
[0065] According to the present invention, preferably, in step (5), based on the total amount of the NiO@nitrogen and oxygen co-doped carbon nanocages and metallic lithium, the content of the deposited metallic lithium is 2-90wt%, preferably 2-50wt%.
[0066] In the invention, there is no particular requirement for the specific method of the electrodeposition, and the electrodeposition method conventional in the art can be used. Preferably, the electrodeposition is selected from constant direct current electrodeposition and / or pulse electrodeposition.
[0067] The present invention has no particular limitation on the specific conditions of the constant direct current electrodeposition and / or pulse electrodeposition, and the conventional operating conditions in the art can be used as long as the above-mentioned deposition amount of metallic lithium can be met. Preferably, the electrodeposition is constant direct current electrodeposition, and the current of the constant direct current electrodeposition can be 0.5-5 mA / cm 2 .
[0068] The third aspect of the present invention provides a metallic lithium negative electrode, which comprises a current collector and an active layer composited on the current collector, wherein the active layer comprises an active material, a binder and an optional conductive agent; the active material comprises the negative electrode active material described in the first aspect or the negative electrode active material prepared by the preparation method described in the second aspect.
[0069] In the present invention, the content of the binder and the conductive agent in the active layer has a wide range of choices, and those skilled in the art can select according to needs. Preferably, based on the total mass of the active layer, the content of the active material is 50-95wt%, preferably 70-95wt%; the content of the binder is 1-50wt%, preferably 2-20wt%; the content of the conductive agent is 0-10wt%, preferably 5-10wt%.
[0070] In the present invention, the binder can be any binder known in the art that can be used for metal lithium batteries, for example, it can be selected from fluorine-containing resins and / or polyolefin compounds. Preferably, the binder is selected from at least one of polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), sodium carboxymethyl cellulose, polyvinyl alcohol, styrene-butadiene rubber emulsion and acrylonitrile copolymer aqueous dispersion, preferably polyvinylidene fluoride.
[0071] In the present invention, the conductive agent can be any conductive agent known to those skilled in the art. Preferably, the conductive agent is selected from at least one of conductive carbon black (Super-P), acetylene black, nickel powder, copper powder and conductive graphite, preferably conductive carbon black.
[0072] In the present invention, there is no particular limitation on the composite method, and it can be carried out by conventional operations in the art. For example, the active layer can be composited on the current collector by coating or calendering.
[0073] According to the present invention, there is no particular limitation on the material and shape of the current collector, for example, it can be selected from any conventional flat current collector in the art. Preferably, the material of the current collector is selected from at least one of copper, titanium, nickel, iron and cobalt.
[0074] Preferably, the thickness of the current collector is 2-200 μm, preferably 2-100 μm.
[0075] In the present invention, there is no particular limitation on the thickness of the negative electrode active layer, and those skilled in the art can select the thickness according to actual needs.
[0076] A fourth aspect of the present invention provides a metal lithium battery, wherein the metal lithium battery comprises the metal lithium negative electrode described in the third aspect.
[0077] In the present invention, there is no special limitation on the specific structure and composition of the metal lithium battery, and any conventional assembly method in the art can be adopted. For example, the metal lithium battery includes a pole core and a non-aqueous electrolyte, the pole core and the non-aqueous electrolyte are sealed in a battery housing, the pole core includes a positive electrode, a negative electrode and a diaphragm, and the diaphragm is located between the positive electrode and the negative electrode.
[0078] The non-aqueous electrolyte and the separator may be the non-aqueous electrolyte and the separator applicable to metal lithium batteries conventionally used in the art. The specific composition and dosage thereof are well known to those skilled in the art and will not be described in detail here.
[0079] In the present invention, the selection range of the active material in the positive electrode of the metal lithium battery is relatively wide, and any conventional positive electrode active material in the art can be used, and those skilled in the art can select it according to actual needs. For example, the active material can be at least one of lithium iron phosphate, lithium cobalt oxide and ternary positive electrode material.
[0080] Preferably, the metal lithium battery is any one of a lithium sulfur battery, a lithium oxygen battery, a lithium iodine battery, a lithium selenium battery, a lithium tellurium battery, a lithium oxygen battery and a lithium carbon dioxide battery.
[0081] The present invention will be described in detail below through examples.
[0082] In the following examples, unless otherwise specified, the raw materials used were commercially available.
[0083] The growth of metallic lithium dendrites was characterized by scanning electron microscopy (SEM). The model of the scanning electron microscope used was Hitachi S-4800 cold field scanning emission electron microscope. The test conditions of the scanning electron microscope were: the powder sample was fixed on the sample stage for observation by conductive glue, and the acceleration voltage was 5kV.
[0084] The surface morphology of the material was characterized by high-resolution transmission electron microscopy (HRTEM). The model of the high-resolution transmission electron microscope used was JEM-2100 (JEOL Ltd.), and the test conditions of the high-resolution transmission electron microscope were: the acceleration voltage was 200 kV.
[0085] The pore structure properties of the material were detected by the BET test method, which was specifically measured using a Quantachrome AS-6B analyzer, and the specific surface area of the material was obtained by the Brunauer-Emmett-Taller (BET) method.
[0086] The composition and valence state changes of each element on the surface of the material were determined by X-ray photoelectron spectroscopy (XPS). The X-ray photoelectron spectroscopy analysis was carried out on an ESCALab250 X-ray photoelectron spectrometer equipped with Thermo Avantage V5.926 software from Thermo Scientific. The excitation source was monochromatic Al Kα X-ray with an energy of 1486.6 eV and a power of 150 W. The penetration energy used for narrow scanning was 30 eV. The basic vacuum during the analysis was 6.5×10 -10 The electron binding energy was calibrated with the C1s peak (284.3 eV) of elemental carbon. The data were processed on Thermo Avantage software, and the sensitivity factor method was used for quantitative analysis in the analysis module.
[0087] The electrochemical performance of the metallic lithium anode was tested by a LAND CT2001A tester.
[0088] Example 1
[0089] (1) 14.67 g of basic nickel carbonate, 20.46 g of ethylenediaminetetraacetic acid (EDTA), and 100 mL of deionized water were mixed, stirred at 80° C. to obtain a homogeneous solution, and then heated and evaporated to obtain a solid precursor.
[0090] (2) placing the precursor obtained in step (1) in a porcelain boat, then placing the porcelain boat in the constant temperature zone of a tubular furnace, introducing nitrogen at a flow rate of 80 mL / min, and heating to 350°C at a rate of 10°C / min. After keeping the constant temperature for 2 hours, stopping heating, and cooling to room temperature under a nitrogen atmosphere to obtain a first pyrolysis product.
[0091] (3) The first pyrolysis product is added to an aqueous solution containing 1 M nitric acid, stirred at 90°C for 4 hours, and then filtered to collect the filtrate. The filter cake is then dried in a constant temperature oven at 120°C for 6 hours to obtain a nitrogen-oxygen co-doped carbon nanocage containing Ni(NO3)2.
[0092] (4) The nitrogen-oxygen co-doped carbon nanocage containing Ni(NO3)2 obtained in step (3) is placed in a porcelain boat, and then the porcelain boat is placed in the constant temperature zone of a tubular furnace, nitrogen is introduced at a flow rate of 80 mL / min, and the temperature is increased to 350°C at a rate of 10°C / min for a second pyrolysis. After keeping the temperature constant for 2 hours, the heating is stopped, and the mixture is cooled to room temperature under a nitrogen atmosphere to obtain NiO@nitrogen-oxygen co-doped carbon nanocage.
[0093] TEM images of NiO@nitrogen and oxygen co-doped carbon nanocages Figure 1 As shown in the figure, it can be seen that NiO@nitrogen-oxygen co-doped carbon nanocage has a hollow cage structure, which indicates that NiO is attached to the inner surface of the nitrogen-oxygen co-doped carbon nanocage.
[0094] The diameter of the NiO@nitrogen-oxygen co-doped carbon nanocage is 10 nm, and the thickness of the cage wall is 2 nm. The specific surface area of the NiO@nitrogen-oxygen co-doped carbon nanocage is 343.7 m 2 / g, the pore volume of the cage wall is 0.26cm 3 / g.
[0095] The XPS picture of this material is as follows Figure 2 As shown, the material contains carbon, nickel, oxygen and nitrogen. In the NiO@nitrogen-oxygen co-doped carbon nanocage, the molar content of carbon is 84.8%, the molar content of nickel is 1.2%, the molar content of oxygen is 10.5% and the molar content of nitrogen is 3.5%. The ratio of the molar content of oxygen to nickel is 8.75, and the ratio of the molar content of oxygen to nitrogen is 3. The XPS spectrum is analyzed based on the 2p orbital of Ni, proving the presence of NiO species in the material.
[0096] Figure 3 The XPS O1s peak spectrum of the NiO@nitrogen-oxygen co-doped carbon nanocage is shown in Figure 1. Through XPS data analysis, it can be found that the oxygen species in the NiO@nitrogen-oxygen co-doped carbon nanocage include carboxyl oxygen, hydroxyl oxygen and ether oxygen. The characteristic peaks of carboxyl oxygen, hydroxyl oxygen and ether oxygen are located at 533.4 eV, 532.0 eV and 530.7 eV, respectively. The molar content ratio of carboxyl oxygen: hydroxyl oxygen and ether oxygen is 1.06:1.51:1.
[0097] (5) depositing metallic lithium onto the NiO@nitrogen-oxygen co-doped carbon nanocage by constant direct current deposition, with the total amount of the NiO@nitrogen-oxygen co-doped carbon nanocage and metallic lithium being the basis, and the content of the deposited metallic lithium being 10 wt %, and the specific method comprising:
[0098] S1. Grind NiO@nitrogen-oxygen co-doped carbon nanocage and conductive agent Super-P in a mortar for 15 minutes. After grinding evenly, add NMP solution of binder PVDF (mass fraction 5%) according to the proportion. The mass ratio of NiO@nitrogen-oxygen co-doped carbon nanocage, conductive agent and binder is 8:1:1. Stir on a magnetic stirrer for 6 hours; evenly apply the obtained paste slurry on a 9μm thick current collector copper foil with a coating thickness of 75μm; then dry it in a vacuum drying oven at 60℃ for 20 hours for use. The dried electrodes are made into circular pole pieces with a diameter of 12mm respectively; and maintained at a pressure of 8MPa for 30-180 seconds.
[0099] S2. Use the electrode sheet prepared as above as positive electrode, metallic lithium as negative electrode, Celgard membrane as separator, select 1 mol / L lithium bis(trifluoromethylsulfonate)imide as electrolyte, 1% lithium nitrate as additive, solvent volume ratio DOL (1,3-dioxolane): DME (ethylene glycol dimethyl ether) = 1:1, and assemble into CR2032 button battery.
[0100] S3, using the LAND CT2001A charge and discharge instrument of Wuhan Lanbo Electronics Co., Ltd. to perform constant DC deposition, the conditions include: at a constant current of 1mA / cm 2 Discharge for 4 hours under the conditions.
[0101] The battery is then disassembled in a glove box, and the pole piece is taken out, wherein the active material includes NiO@nitrogen-oxygen co-doped carbon nanocage and metallic lithium filled in the cage cavity of the NiO@nitrogen-oxygen co-doped carbon nanocage.
[0102] Electrochemical performance evaluation
[0103] The electrode obtained in the above-mentioned constant direct current deposition is used as a metal lithium negative electrode. In the metal lithium negative electrode, based on the total weight of the active layer, the content of the metal lithium negative electrode active material is 80.16% by weight, the content of the binder PVDF is 9.92% by weight, and the content of the conductive agent Super-P is 9.92% by weight. Metal lithium is used as the counter electrode, Celgard membrane is used as the diaphragm, 1 mol / L lithium bis(trifluoromethylsulfonate)imide is selected as the electrolyte, 1% lithium nitrate is used as the additive, and the solvent volume ratio DOL (1,3-dioxolane): DME (ethylene glycol dimethyl ether) = 1:1 is assembled into a CR2032 button cell. The battery is subjected to a constant current charge and discharge test using the Landian LAND CT2001A charge and discharge instrument of Wuhan Rambo Electronics Co., Ltd. At 25°C, the constant current is 1mA / cm 2 The charge and discharge were performed for 1 h each under the above conditions, and the above charge and discharge process was repeated, and the cycle was maintained at a stable overpotential. When the overpotential suddenly changed or continued to increase, the cycle was terminated and the cycle time was recorded. The results are shown in Table 1.
[0104] The cycled battery was disassembled, the negative electrode was taken out, the lithium salt and lithium nitrate on the surface of the electrode were cleaned with DME, and the lithium deposition morphology was observed by SEM test. The SEM test results of Example 1 are as follows: Figure 4 As shown, the deposition of metallic lithium is relatively uniform and smooth.
[0105] Example 2
[0106] (1) 12.1 g of basic nickel carbonate, 20.46 g of ethylenediaminetetraacetic acid (EDTA), and 100 mL of deionized water were mixed, stirred at 80° C. to obtain a homogeneous solution, and then heated and evaporated to obtain a solid precursor.
[0107] (2) placing the precursor obtained in step (1) in a porcelain boat, then placing the porcelain boat in the constant temperature zone of a tubular furnace, introducing nitrogen at a flow rate of 80 mL / min, and heating to 400°C at a rate of 10°C / min. After keeping the constant temperature for 2 hours, stopping heating, and cooling to room temperature under a nitrogen atmosphere to obtain a first pyrolysis product.
[0108] (3) The first pyrolysis product is added to an aqueous solution containing 1 M nitric acid, stirred at 90°C for 4 hours, and then filtered to collect the filtrate. The filter cake is then dried in a constant temperature oven at 120°C for 6 hours to obtain a nitrogen-oxygen co-doped carbon nanocage containing Ni(NO3)2.
[0109] (4) The nitrogen-oxygen co-doped carbon nanocage containing Ni(NO3)2 obtained in step (3) is placed in a porcelain boat, and then the porcelain boat is placed in the constant temperature zone of a tubular furnace, nitrogen is introduced at a flow rate of 80 mL / min, and the temperature is increased to 350°C at a rate of 10°C / min. After keeping the constant temperature for 2 hours, the heating is stopped and the mixture is cooled to room temperature under a nitrogen atmosphere to obtain NiO@nitrogen-oxygen co-doped carbon nanocage.
[0110] Through TEM, it can be seen that the NiO@nitrogen-oxygen co-doped carbon nanocage has a hollow cage structure. The diameter of the NiO@nitrogen-oxygen co-doped carbon nanocage is 10nm, and the thickness of the cage wall is 1.8nm. Through the BET test method, the specific surface area of the NiO@nitrogen-oxygen co-doped carbon nanocage is 310.2m 2 / g, and the pore volume of the cage wall is 0.34cm 3 / g.
[0111] The XPS test results of the material can prove that the material contains carbon, nickel, oxygen and nitrogen. In the NiO@nitrogen-oxygen co-doped carbon nanocage, the molar content of carbon is 87.1%, the molar content of nickel is 1%, the molar content of oxygen is 8.5% and the molar content of nitrogen is 3.4%. Among them, the molar content ratio of oxygen to nickel is 8.5, and the molar content ratio of oxygen to nitrogen is 2.5.
[0112] XPS data analysis shows that the oxygen species in the NiO@nitrogen-oxygen co-doped carbon nanocage include carboxyl oxygen, hydroxyl oxygen and ether oxygen, and the molar content ratio of carboxyl oxygen, hydroxyl oxygen and ether oxygen is 1.2:1.6:1.
[0113] (5) Depositing metallic lithium onto the NiO@nitrogen-oxygen co-doped carbon nanocage by constant direct current deposition according to the method in Example 1, with the total amount of the NiO@nitrogen-oxygen co-doped carbon nanocage and metallic lithium being the basis, and the content of the deposited metallic lithium being 10 wt %.
[0114] The electrochemical performance test was carried out according to the method in Example 1. The results are shown in Table 1.
[0115] Example 3
[0116] (1) 14.67 g of basic nickel carbonate, 20.46 g of ethylenediaminetetraacetic acid (EDTA), and 100 mL of deionized water were mixed, stirred at 80° C. to obtain a homogeneous solution, and then heated and evaporated to obtain a solid precursor.
[0117] (2) placing the precursor obtained in step (1) in a porcelain boat, then placing the porcelain boat in the constant temperature zone of a tubular furnace, introducing nitrogen at a flow rate of 80 mL / min, and heating to 300°C at a rate of 10°C / min. After keeping the constant temperature for 2 hours, stopping heating, and cooling to room temperature under a nitrogen atmosphere to obtain a first pyrolysis product.
[0118] (3) The first pyrolysis product is added to an aqueous solution containing 1 M nitric acid, stirred at 90°C for 4 hours, and then filtered to collect the filtrate. The filter cake is then dried in a constant temperature oven at 120°C for 6 hours to obtain a nitrogen-oxygen co-doped carbon nanocage containing Ni(NO3)2.
[0119] (4) The nitrogen-oxygen co-doped carbon nanocage containing Ni(NO3)2 obtained in step (3) is placed in a porcelain boat, and then the porcelain boat is placed in the constant temperature zone of a tubular furnace, nitrogen is introduced at a flow rate of 80 mL / min, and the temperature is increased to 300°C at a rate of 10°C / min. After keeping the constant temperature for 2 hours, the heating is stopped, and the mixture is cooled to room temperature under a nitrogen atmosphere to obtain NiO@nitrogen-oxygen co-doped carbon nanocage.
[0120] Through TEM, it can be seen that the NiO@nitrogen-oxygen co-doped carbon nanocage has a hollow cage structure. The diameter of the NiO@nitrogen-oxygen co-doped carbon nanocage is 10nm and the thickness of the cage wall is 3nm. Through the BET test method, the specific surface area of the NiO@nitrogen-oxygen co-doped carbon nanocage is 410m 2 / g, the pore volume of the cage wall is 0.21cm 3 / g.
[0121] The XPS test results of the material can prove that the material contains carbon, nickel, oxygen and nitrogen. In the NiO@nitrogen-oxygen co-doped carbon nanocage, the molar content of carbon is 61.5%, the molar content of nickel is 5%, the molar content of oxygen is 29.8% and the molar content of nitrogen is 3.7%. Among them, the molar content ratio of oxygen to nickel is 5.96, and the molar content ratio of oxygen to nitrogen is 8.
[0122] XPS data analysis shows that the oxygen species in the NiO@nitrogen-oxygen co-doped carbon nanocage include carboxyl oxygen, hydroxyl oxygen and ether oxygen, and the molar content ratio of carboxyl oxygen, hydroxyl oxygen and ether oxygen is 1.1:1.3:1.
[0123] (5) Depositing metallic lithium onto the NiO@nitrogen-oxygen co-doped carbon nanocage by constant direct current deposition according to the method in Example 1, with the total amount of the NiO@nitrogen-oxygen co-doped carbon nanocage and metallic lithium being the basis, and the content of the deposited metallic lithium being 10 wt %.
[0124] The electrochemical performance test was carried out according to the method in Example 1. The results are shown in Table 1.
[0125] Example 4
[0126] The method of Example 1 is followed, except that in step (3), the pyrolysis product obtained in step (2) is added to an aqueous solution containing 2M nitric acid and stirred at 90°C for 12 hours.
[0127] The prepared NiO@nitrogen-oxygen co-doped carbon nanocage has a carbon molar content of 86%, a nickel molar content of 0.5%, an oxygen molar content of 10%, and a nitrogen molar content of 3.5%, wherein the molar content ratio of oxygen to nickel is 20, and the molar content ratio of oxygen to nitrogen is 2.86.
[0128] XPS data analysis shows that the oxygen species in the NiO@nitrogen-oxygen co-doped carbon nanocage include carboxyl oxygen, hydroxyl oxygen and ether oxygen, and the molar content ratio of carboxyl oxygen, hydroxyl oxygen and ether oxygen is 1:2:1.
[0129] Metal lithium was deposited on the NiO@nitrogen-oxygen co-doped carbon nanocage by constant direct current deposition, with the total amount of the NiO@nitrogen-oxygen co-doped carbon nanocage and metal lithium as the basis, and the content of the deposited metal lithium was 10wt%. The electrochemical performance test was carried out according to the method in Example 1. The results are shown in Table 1.
[0130] Example 5
[0131] The method of Example 1 is followed, except that in step (2), the first pyrolysis temperature is increased to 1100°C.
[0132] The prepared NiO@nitrogen-oxygen co-doped carbon nanocage has a molar content of carbon of 96.4%, a molar content of nickel of 1.2%, a molar content of oxygen of 1.05% and a molar content of nitrogen of 1.35%, wherein the ratio of the molar content of oxygen to nickel is 0.88, and the ratio of the molar content of oxygen to nitrogen is 0.78.
[0133] XPS data analysis shows that the oxygen species in the NiO@nitrogen-oxygen co-doped carbon nanocage include carboxyl oxygen, hydroxyl oxygen and ether oxygen, and the molar content ratio of carboxyl oxygen, hydroxyl oxygen and ether oxygen is 1.1:2.5:1.2.
[0134] Metal lithium was deposited on the NiO@nitrogen-oxygen co-doped carbon nanocage by constant direct current deposition, with the total amount of the NiO@nitrogen-oxygen co-doped carbon nanocage and metal lithium as the basis, and the content of the deposited metal lithium was 10wt%. The electrochemical performance test was carried out according to the method in Example 1. The results are shown in Table 1.
[0135] Comparative Example 1
[0136] The method of Example 1 is followed, except that the second pyrolysis of step (4) is not performed, and 10 wt% of metallic lithium is deposited on the nitrogen-oxygen co-doped carbon nanocage containing Ni(NO3)2 obtained in step (3) by constant direct current deposition.
[0137] The obtained nitrogen-oxygen co-doped carbon nanocage has a hollow cage structure with a diameter of 10nm and a cage wall thickness of 2nm. The specific surface area of the nitrogen-oxygen co-doped carbon nanocage is 380m 2 / g, the pore volume of the cage wall is 0.26cm 3 / g.
[0138] The material contains carbon, oxygen, nitrogen and nickel, wherein nickel exists in the form of ions. In the nitrogen-oxygen co-doped carbon nanocage, the molar content of nickel is 1.2%, the molar content of carbon is 84.1%, the molar content of oxygen is 11%, the molar content of nitrogen is 3.7%, the ratio of the molar content of oxygen to nickel is 9.17:1, and the ratio of the molar content of oxygen to nitrogen is 3.
[0139] Then, metallic lithium is deposited on the nitrogen-oxygen co-doped carbon nanocage by constant direct current deposition, with the total amount of the nitrogen-oxygen co-doped carbon nanocage and metallic lithium being taken as a reference, and the content of the deposited metallic lithium is 10 wt %.
[0140] The electrochemical performance test was carried out according to the method in Example 1. The results are shown in Table 1.
[0141] Comparative Example 2
[0142] (1) 14.67 g of basic nickel carbonate, 13.45 g of citric acid, and 100 mL of deionized water were mixed, stirred at 80° C. to obtain a homogeneous solution, and then heated and evaporated to obtain a solid precursor.
[0143] (2) placing the precursor obtained in step (1) in a porcelain boat, then placing the porcelain boat in the constant temperature zone of a tubular furnace, introducing nitrogen at a flow rate of 80 mL / min, and heating to 320°C at a rate of 10°C / min. After keeping the constant temperature for 2 hours, stopping heating, and cooling to room temperature under a nitrogen atmosphere to obtain a first pyrolysis product.
[0144] (3) The first pyrolysis product is added to an aqueous solution containing 1 M nitric acid, stirred at 90° C. for 4 h, and then filtered to collect the filtrate. The filter cake is then dried in a constant temperature oven at 120° C. for 6 h to obtain a carbon nanocage containing Ni(NO3)2.
[0145] (4) The carbon nanocage containing Ni(NO3)2 obtained in step (3) is placed in a porcelain boat, and then the porcelain boat is placed in the constant temperature zone of a tubular furnace, nitrogen is introduced at a flow rate of 80 mL / min, and the temperature is increased to 350°C at a rate of 10°C / min. After keeping the constant temperature for 2 hours, the heating is stopped and the mixture is cooled to room temperature in a nitrogen atmosphere to obtain NiO@carbon nanocage.
[0146] The NiO@ carbon nanocage has a hollow cage structure with a diameter of 13nm and a cage wall thickness of 2.6nm. The specific surface area of the NiO@ carbon nanocage is 521m 2 / g, and the pore volume of the cage wall is 0.72cm 3 / g.
[0147] In addition to carbon, the material also contains oxygen and nickel. In the NiO@nitrogen-oxygen co-doped carbon nanocage, the molar content of carbon is 77.84%, the molar content of nickel is 1%, the molar content of oxygen is 21.16%, and the ratio of the molar content of oxygen to nickel is 21.16:1.
[0148] XPS data analysis shows that the oxygen species in the NiO@carbon nanocage include hydroxyl oxygen, carboxyl oxygen and ether oxygen, and the ratio of the molar content of carboxyl oxygen, the molar content of hydroxyl oxygen and the molar content of ether oxygen is 1:2.3:1.1;
[0149] (5) depositing metallic lithium onto the NiO@carbon nanocage by constant direct current deposition, with the total amount of the NiO@carbon nanocage and metallic lithium being taken as a reference, and the content of the deposited metallic lithium being 10 wt %.
[0150] The electrochemical performance test was carried out according to the method in Example 1. The results are shown in Table 1.
[0151] Comparative Example 3
[0152] (1) 14.67 g of basic nickel carbonate, 20.46 g of ethylenediaminetetraacetic acid (EDTA), and 100 mL of deionized water were mixed, stirred at 80° C. to obtain a homogeneous solution, and then heated and evaporated to obtain a solid precursor.
[0153] (2) placing the precursor obtained in step (1) in a porcelain boat, then placing the porcelain boat in the constant temperature zone of a tubular furnace, introducing nitrogen at a flow rate of 80 mL / min, and heating to 350°C at a rate of 10°C / min. After keeping the constant temperature for 2 hours, heating is stopped, and the product is cooled to room temperature under a nitrogen atmosphere to obtain a carbon-coated nickel product, in which the nickel exists in the form of a single nickel substance.
[0154] (3) depositing metallic lithium onto the carbon-coated nickel by constant direct current deposition, with the total amount of the carbon-coated nickel and metallic lithium being taken as a reference and the content of the deposited metallic lithium being 10 wt %.
[0155] The electrochemical performance test was carried out according to the method in Example 1. The results are shown in Table 1.
[0156] Table 1
[0157] Cycle time (h) Coulomb efficiency after 50 cycles (%) Example 1 1000 99.8% Example 2 950 99.7% Example 3 937 99.5% Example 4 850 98.5% Example 5 824 98.3% Comparative Example 1 500 95.2% Comparative Example 2 700 93.5% Comparative Example 3 476 92.1%
[0158] It can be seen from the results in Table 1 that the metal lithium negative electrode formed by the composite of NiO@nitrogen and oxygen co-doped carbon nanocage prepared in the embodiment of the present invention and metal lithium has a longer cycle life and higher coulombic efficiency.
[0159] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A negative electrode active material, characterized in that: The negative electrode active material includes NiO@nitrogen-oxygen co-doped carbon nanocage, and metal lithium filled in the cage cavity of the NiO@nitrogen-oxygen co-doped carbon nanocage; The X-ray photoelectron spectroscopy shows that the molar content of nickel in the NiO@nitrogen-oxygen co-doped carbon nano cage is not less than 0.5%, and the molar content ratio of oxygen to nickel is 0.5-20:
1.
2. The negative electrode active material according to claim 1, wherein The NiO in the NiO@nitrogen-oxygen co-doped carbon nanocage is located on the inner surface of the nitrogen-oxygen co-doped carbon nanocage.
3. The negative electrode active material according to claim 1 or 2, wherein The molar content of carbon in the NiO@nitrogen-oxygen co-doped carbon nanocage measured by X-ray photoelectron spectroscopy is 50-88.5%, preferably 60-88%; the molar content of nickel is 0.5-10%, preferably 1-5%; the molar content of oxygen is 1-31%, preferably 5-15%; the molar content of nitrogen is 1-10%, preferably 3-10%; And / or, the molar ratio of oxygen to nitrogen in the NiO@nitrogen-oxygen co-doped carbon nanocage is 2-10:1, preferably 2.5-6:1, as measured by X-ray photoelectron spectroscopy; And / or, the molar ratio of oxygen to nickel in the NiO@nitrogen-oxygen co-doped carbon nanocage is 5-10:1 as measured by X-ray photoelectron spectroscopy.
4. The negative electrode active material according to any one of claims 1 to 3, wherein X-ray photoelectron spectroscopy revealed that the oxygen species in the NiO@nitrogen-oxygen co-doped carbon nanocage included carboxyl oxygen, hydroxyl oxygen and ether oxygen. Preferably, the molar ratio of carboxyl oxygen, hydroxyl oxygen and ether oxygen is 1-2:1-5:1-2, preferably 1-1.5:1-1.8:
1.
5. The negative electrode active material according to any one of claims 1 to 4, wherein: The diameter of the NiO@nitrogen and oxygen co-doped carbon nanocage is 2-50 nm, preferably 10-50 nm, and more preferably 10-30 nm; And / or, the specific surface area of the NiO@nitrogen-oxygen co-doped carbon nanocage is 50-1000m 2 / g, preferably 200-800m 2 / g, more preferably 300-600m 2 / g; And / or, the thickness of the cage wall of the NiO@nitrogen-oxygen co-doped carbon nanocage is 1-50 nm, preferably 1-30 nm, more preferably 1-20 nm; And / or, the pore volume of the cage wall of the NiO@nitrogen and oxygen co-doped carbon nanocage is 0.1-1cm 3 / g, preferably 0.1-0.5cm 3 / g.
6. The negative electrode active material according to any one of claims 1 to 5, wherein: Based on the total amount of the NiO@nitrogen and oxygen co-doped carbon nanocages and metallic lithium, the content of metallic lithium is 2-90wt%, preferably 2-50wt%.
7. A method for preparing a negative electrode active material, characterized in that: The method includes: (1) providing a homogeneous solution containing a Ni salt, ethylenediaminetetraacetic acid and a solvent, and then removing the solvent from the homogeneous solution to obtain a precursor; the mass ratio of the Ni salt to the ethylenediaminetetraacetic acid is 1:0.1-100; (2) subjecting the precursor to a first pyrolysis under an inert atmosphere and / or a reducing atmosphere to obtain a first pyrolysis product; (3) contacting the first pyrolysis product with an oxygen-containing acid and then drying it; (4) Under an inert atmosphere, subjecting the product obtained in step (3) to a second pyrolysis to obtain NiO@nitrogen-oxygen co-doped carbon nanocages; the temperature of the second pyrolysis is 250-400° C.; (5) depositing metallic lithium onto the NiO@nitrogen-oxygen co-doped carbon nanocage by electrodeposition.
8. The preparation method according to claim 7, wherein: In the step (3), the product obtained by contacting the pyrolysis product with the oxygen-containing acid is directly dried after optional solid-liquid separation, without the need for a washing step.
9. The preparation method according to claim 7 or 8, wherein: In step (1), the mass ratio of the Ni salt to EDTA is 1:0.5-50, preferably 1:0.5-5; And / or, the solvent is ethanol and / or water.
10. The preparation method according to any one of claims 7 to 9, wherein: In step (2), the first pyrolysis conditions include: a heating rate of 0.5-30°C / min, preferably 1-10°C / min; a temperature not higher than 450°C, preferably 350-450°C, more preferably 350-400°C; and a constant temperature time of 20-600min, preferably 60-480min.
11. The preparation method according to any one of claims 7 to 10, wherein: The oxygen-containing acid is provided by an aqueous solution of nitric acid; and / or, the concentration of the aqueous solution of nitric acid is 0.5-2 mol / L, preferably 0.5-1 mol / L; And / or, in step (3), the contact temperature is 20-110°C, preferably 60-90°C; the contact time is 0.1-48h, preferably 4-12h.
12. The preparation method according to any one of claims 7 to 11, wherein: In step (4), the second pyrolysis conditions include: a heating rate of 0.5-15°C / min, preferably 1-10°C / min; a temperature of 250-350°C, preferably 300-350°C; and a constant temperature time of 20-600min, preferably 60-480min.
13. The preparation method according to any one of claims 7 to 12, wherein: In step (5), based on the total amount of the NiO@nitrogen-oxygen co-doped carbon nanocage and metallic lithium, the content of the deposited metallic lithium is 2-90wt%, preferably 2-50wt%; Preferably, the electrodeposition is selected from constant direct current electrodeposition and / or pulse electrodeposition.
14. A metal lithium negative electrode, comprising a current collector and an active layer composited on the current collector, wherein the active layer comprises an active material, a binder and an optional conductive agent; It is characterized in that The active material includes the negative electrode active material according to any one of claims 1 to 6 or the negative electrode active material prepared by the preparation method according to any one of claims 7 to 13.
15. The metal lithium negative electrode according to claim 14, based on the total mass of the active layer, the content of the active material is 50-95wt%, preferably 70-95wt%; the content of the binder is 1-50wt%, preferably 2-20wt%; the content of the conductive agent is 0-10wt%, preferably 5-10wt%.
16. A metal lithium battery, characterized in that: The metal lithium battery comprises the metal lithium negative electrode according to claim 14 or 15; Preferably, the metal lithium battery is any one of a lithium sulfur battery, a lithium oxygen battery, a lithium iodine battery, a lithium selenium battery, a lithium tellurium battery, a lithium oxygen battery and a lithium carbon dioxide battery.
Citation Information
Patent Citations
Nitrogen-oxygen co-doped carbon-coated metal lithium anode active material, anode, lithium metal battery and preparation and application thereof
CN111755668A
Metal oxide composite material and preparation method and application thereof
CN113540456A
Negative electrode material, negative electrode sheet, electrochemical device, and electronic device
CN114270574A
Nitrogen-doped nano carbon material and preparation method thereof, metal lithium negative electrode and preparation method thereof, and metal lithium battery
CN116031405A