Deep nano nickel catalyst as well as preparation method and application thereof

By using pyrolysis treatment of nickel salts and solid organic matter in the preparation of nano nickel catalysts, deep nano nickel catalysts are formed, which solves the problems of complex process and low activity in the prior art, and achieves efficient catalytic activity improvement and cost reduction. In a variety of alkaline fuel cells and hydrogen energy applications.

CN119008987AInactive Publication Date: 2024-11-22SICHUAN UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411108653.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing nano nickel catalyst preparation process is complex and has low activity, making it difficult to replace the application of precious metal catalysts in alkaline media, especially in hydroxide reactions and hydrogen fuel cells.

Method used

The nickel salt and solid organic matter were stirred and dissolved in a solvent, and then evaporated in vacuum to pyrolytic treatment of the H2/Ar mixed gas to form a deep nano nickel catalyst with a nano nickel core and carbon shell structure, and passed through solid organic matter and low concentration hydrogen. The combined action of controlling nickel particle size and electronic structural modification.

Benefits of technology

A deep nano nickel catalyst with a particle size of 4 to 6 nanometers was prepared, which significantly improved the catalytic activity and was suitable for alkaline fuel cells, nickel hydrogen batteries and electrolytic water hydrogen production, reducing costs and improving catalytic efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008987A_ABST
    Figure CN119008987A_ABST
Patent Text Reader

Abstract

The invention discloses a deep nano nickel catalyst as well as a preparation method and application thereof, and belongs to the technical field of electrochemical catalysis. The preparation method comprises the following steps: dissolving nickel salt and a solid organic matter into a solvent according to a specific molar ratio, and evaporating the solvent to obtain a solid precursor; and performing pyrolysis reduction on the solid precursor in a low-concentration hydrogen atmosphere to obtain the deep nano nickel catalyst. The deep nano nickel catalyst comprises a nano nickel core and a carbon shell coating the surface of the nano nickel core, the particle size of the nano nickel core is 4-6 nm, and the thickness of the carbon shell is 1-2 nm. The deep nano nickel catalyst prepared by the method has relatively small size and high hydrogen oxidation and hydrogen reduction activity, and can be used in alkaline fuel cells, hydrogen-nickel batteries and water electrolysis devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrochemical catalysis, and specifically relates to a deep nano nickel catalyst and a preparation method and application thereof. Background Art

[0002] Compared with fossil fuels, sustainable hydrogen energy, with hydrogen fuel cells as the key application area, is more advanced, especially in terms of greenhouse gas emissions. Hydrogen exchange membrane fuel cells (HEMFCs) have attracted widespread attention in recent years due to the great achievements in efficient non-precious metal oxygen reduction reaction (ORR) electrocatalysts in alkaline media and alkaline membranes. However, at the anode end of HEMFCs, unlike in acidic media, the kinetics of hydrogen oxidation reaction (HOR) in alkaline media is worse, and more platinum-based catalysts need to be loaded to promote the reaction. In addition, for non-precious metal-based catalysts, their HOR activity is still 2 to 3 orders of magnitude lower than that of platinum-based catalysts. Therefore, it is a huge challenge to replace platinum-based catalysts with low-cost non-precious metal-based catalysts.

[0003] Nickel-hydrogen battery (nickel-hydrogen battery) is an alkaline storage battery with the advantage of ultra-long service life. It has broad application prospects in large-scale energy storage fields such as wind, solar, water and coal. The charging and discharging of the negative electrode of this battery is a conversion process of hydrogen evolution (HER) and HOR, which requires the use of catalysts. Like HEMFC, commercial nickel-hydrogen batteries still mainly use expensive platinum-based catalysts, so the development of cheap non-precious metal nickel-hydrogen battery negative electrode catalysts is of high value. At the same time, the development of this low-cost HER catalyst also has application prospects in the field of hydrogen production by electrolysis of water.

[0004] At present, Ni-based catalysts have been confirmed to be the most promising alkaline HER / HOR catalysts to replace precious metals. However, Ni itself has a strong adsorption effect on hydrogen radicals, which makes the desorption process of H* at its active site slow, so its catalytic activity is 2 to 3 orders of magnitude lower than that of precious metals. In order to improve the catalytic activity of Ni catalysts, it is necessary to rationally regulate the electronic structure of Ni. Modification with highly electronegative elements (B, C, N, O) is currently an effective method. On the other hand, the size of the nickel metal catalysts currently prepared is relatively large, generally above 20 nanometers. Some studies have pointed out that carbon coating of nickel particles can limit the growth of grains, reduce the particle size of nickel, and exert a higher catalytic effect. Although there are some technologies for preparing carbon-coated nickel catalysts in the literature, these methods mostly involve high-temperature hydrothermal and solvent thermal reactions, and the price of raw materials is relatively high, which cannot be prepared on a large scale. Summary of the invention

[0005] In view of the above-mentioned prior art, the present invention provides a deep nano nickel catalyst and a preparation method and application thereof, so as to solve the technical problems of the existing nano nickel catalyst preparation process being complicated and having low activity.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is to provide a method for preparing a deep nano nickel catalyst, comprising the following steps:

[0007] S1: adding nickel salt and solid organic matter into a solvent, stirring and dissolving, to obtain a mixed solution; then evaporating the solvent of the mixed solution under vacuum conditions to obtain a solid precursor; the solid organic matter is at least one of citric acid, glucose, urea and melamine;

[0008] S2: The solid precursor is ground through a 100-mesh sieve, and then pyrolyzed in a H2 / Ar mixed gas to obtain; the volume fraction of H2 in the H2 / Ar mixed gas does not exceed 8%; the pyrolysis process is to heat the solid precursor to 350-500°C and keep it warm for 0.5-2h.

[0009] Based on the above technical solution, the present invention can also be improved as follows.

[0010] Furthermore, the solvent is anhydrous ethanol; the ratio of the total mass of the nickel salt and the solid organic matter to the mass of the anhydrous ethanol is 1 to 3:1.

[0011] Furthermore, the molar ratio of nickel salt to solid organic matter is 1:0.2-2.

[0012] Furthermore, the nickel salt is at least one of nickel nitrate, nickel chloride, nickel sulfate and nickel acetate.

[0013] Furthermore, the nickel salt is nickel nitrate, and the solid organic matter is citric acid.

[0014] Furthermore, the stirring and dissolving temperature in S1 is 45-80° C., and the stirring and dissolving time is 20-120 min; the temperature for evaporating the solvent is 60-90° C., and the time is 2-10 h.

[0015] Furthermore, the volume fraction of H2 in the H2 / Ar mixed gas is 2 to 4%.

[0016] Furthermore, the heating rate of the solid precursor in S2 is 2-10°C / min; the final temperature of the heating is 450°C, and the holding time is 40min.

[0017] The invention also discloses a deep nano nickel catalyst prepared by the preparation method. The deep nano nickel catalyst comprises a nano nickel core and a carbon shell coated on the surface of the nano nickel core. The particle size of the nano nickel core is 4-6nm, and the thickness of the carbon shell is 1-2nm.

[0018] The invention also discloses the application of the deep nano nickel catalyst in preparing alkaline fuel cells, nickel hydrogen batteries or producing hydrogen by electrolyzing water.

[0019] The beneficial effects of the present invention are:

[0020] 1. The present invention uses dispersed solid organic matter as a carbon source to form a coating effect on nickel nanoparticles during pyrolysis reduction, inhibiting grain growth and modifying the electronic structure of surface nickel; low-concentration hydrogen can not only reduce nickel, but also prevent its further crystallization and growth. The solid organic matter and low-concentration hydrogen work together to achieve a deep nano nickel catalyst of 4 to 6 nanometers.

[0021] 2. The deep nano nickel catalyst of the present invention can be used as a catalyst for the anode hydrogen oxidation reaction in alkaline fuel cells, a cathode catalyst for hydrogen nickel batteries, and a catalyst for electrolytic hydrogen decomposition reaction, which has a positive role in promoting the development and utilization of hydrogen energy. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 TEM images of deep nano nickel catalysts obtained in Example 1 and Comparative Example 1;

[0023] Figure 2 1 is the XRD phase diagram of the deep nano nickel catalyst in Example 1 and Comparative Example 1;

[0024] Figure 3 The LSV curves of the hydrogen oxidation of the deep nano nickel catalysts in Examples 1 to 5 and Comparative Example 1;

[0025] Figure 4 1 is the LSV curve of hydrogen evolution of the deep nano nickel catalyst in Examples 1 to 5 and Comparative Example 1. DETAILED DESCRIPTION

[0026] The specific implementation modes of the present invention are described in detail below with reference to the embodiments.

[0027] Example 1

[0028] A deep nano nickel catalyst is prepared by the following steps:

[0029] S1: Add 5 mmol nickel nitrate hexahydrate and 4 mmol citric acid to 0.8 g anhydrous ethanol, stir and dissolve in a water bath at 80°C for 20 min to obtain a mixed solution; then place the mixed solution in a vacuum oven, dry it at 80°C for 4 h under vacuum conditions, evaporate the solvent of the mixed solution to dryness, and obtain a solid precursor;

[0030] S2: Grind the solid precursor through a 100-mesh sieve, and then load the powder into a tubular furnace for pyrolysis reduction. The pyrolysis reduction atmosphere is a H2 / Ar mixed gas, and the volume fraction of H2 in the mixed gas is 2%. The pyrolysis reduction process is: heat up to 450°C at a heating rate of 10°C / min, keep warm for 40 minutes, and cool to room temperature with the furnace to obtain a deep nano nickel catalyst.

[0031] Example 2

[0032] A deep nano nickel catalyst is prepared by the following steps:

[0033] S1: Add 5mmol nickel sulfate and 2.5mmol glucose to 1g anhydrous ethanol, stir and dissolve in a water bath at 60°C for 40min to obtain a mixed solution; then place the mixed solution in a vacuum oven, dry it at 70°C for 8h under vacuum conditions, evaporate the solvent of the mixed solution to dryness, and obtain a solid precursor;

[0034] S2: Grind the solid precursor through a 100-mesh sieve, and then load the powder into a tubular furnace for pyrolysis reduction. The pyrolysis reduction atmosphere is Ar gas. The pyrolysis reduction process is: heat up to 390°C at a heating rate of 5°C / min, keep warm for 1 minute, and cool to room temperature with the furnace to obtain a deep nano nickel catalyst.

[0035] Example 3

[0036] A deep nano nickel catalyst is prepared by the following steps:

[0037] S1: Add 5 mmol nickel acetate and 5 mmol urea to 0.4 g anhydrous ethanol, stir and dissolve in a water bath at 50°C for 120 min to obtain a mixed solution; then place the mixed solution in a vacuum oven, dry it at 60°C for 10 h under vacuum conditions, evaporate the solvent of the mixed solution to dryness, and obtain a solid precursor;

[0038] S2: Grind the solid precursor through a 100-mesh sieve, and then load the powder into a tubular furnace for pyrolysis reduction. The pyrolysis reduction atmosphere is a H2 / Ar mixed gas, and the volume fraction of H2 in the mixed gas is 5%. The pyrolysis reduction process is: heat up to 500°C at a heating rate of 10°C / min, keep warm for 30 minutes, and cool to room temperature with the furnace to obtain a deep nano nickel catalyst.

[0039] Example 4

[0040] A deep nano nickel catalyst is prepared by the following steps:

[0041] S1: Add 5mmol nickel nitrate hexahydrate and 2.5mmol glucose to 1g anhydrous ethanol, stir and dissolve in a water bath at 80°C for 20min to obtain a mixed solution; then place the mixed solution in a vacuum oven, dry it at 90°C for 2h under vacuum conditions, evaporate the solvent of the mixed solution to dryness, and obtain a solid precursor;

[0042] S2: Grind the solid precursor through a 100-mesh sieve, and then load the powder into a tubular furnace for pyrolysis reduction. The pyrolysis reduction atmosphere is a H2 / Ar mixed gas, and the volume fraction of H2 in the mixed gas is 2%. The pyrolysis reduction process is: heat up to 450°C at a heating rate of 10°C / min, keep warm for 1h, and cool to room temperature with the furnace to obtain a deep nano nickel catalyst.

[0043] Example 5

[0044] A deep nano nickel catalyst is prepared by the following steps:

[0045] S1: Add 5mmol nickel nitrate hexahydrate and 2.5mmol citric acid to 1g anhydrous ethanol, stir and dissolve in a water bath at 80°C for 20min to obtain a mixed solution; then place the mixed solution in a vacuum oven, dry it at 80°C for 4h under vacuum conditions, evaporate the solvent of the mixed solution to dryness, and obtain a solid precursor;

[0046] S2: Grind the solid precursor through a 100-mesh sieve, and then load the powder into a tubular furnace for pyrolysis reduction. The pyrolysis reduction atmosphere is a H2 / Ar mixed gas, and the volume fraction of H2 in the mixed gas is 5%. The pyrolysis reduction process is: heat up to 360°C at a heating rate of 2°C / min, keep warm for 2h, and cool to room temperature with the furnace to obtain a deep nano nickel catalyst.

[0047] Comparative Example 1

[0048] A deep nano nickel catalyst is prepared by the following steps:

[0049] S1: Add 5 mmol nickel nitrate hexahydrate and 4 mmol citric acid to 0.8 g anhydrous ethanol, stir and dissolve in a water bath at 80°C for 20 min to obtain a mixed solution; then place the mixed solution in a vacuum oven, dry it at 80°C for 4 h under vacuum conditions, evaporate the solvent of the mixed solution to dryness, and obtain a solid precursor;

[0050] S2: Grind the solid precursor through a 100-mesh sieve, and then load the powder into a tubular furnace for pyrolysis reduction. The pyrolysis reduction atmosphere is a H2 / Ar mixed gas, and the volume fraction of H2 in the mixed gas is 10%. The pyrolysis reduction process is: heat up to 450°C at a heating rate of 10°C / min, keep warm for 40 minutes, and cool to room temperature with the furnace to obtain a deep nano nickel catalyst.

[0051] Experimental example

[0052] 1. Morphology and structure analysis

[0053] The morphology and structure of the deep nano nickel catalysts prepared in Examples 1 to 5 are similar. Taking the deep nano nickel catalyst in Example 1 as an example, the morphology and structure of the deep nano nickel catalyst prepared by the method in the example of the present invention are described.

[0054] The deep nano nickel catalysts in Example 1 and Comparative Example 1 were analyzed by TEM and XRD. Figure 1 and Figure 2 As shown; among them, Figure 1 (a) is a TEM image of the deep nano nickel catalyst obtained in Example 1, Figure 1 (b) is a TEM image of the deep nano nickel catalyst obtained in Comparative Example 1; Figure 2 The XRD phase diagram of the deep nano nickel catalyst in Example 1 and Comparative Example 1. It can be seen from the figure that the deep nano nickel catalyst is composed of a nano nickel core and a carbon shell coated on the surface of the nano nickel core, and the particle size of the nano nickel core of the deep nano nickel catalyst obtained in Example 1 is 4-6nm, and the thickness of the carbon shell is 1-2nm, and the particle size of the nano nickel core of the deep nano nickel catalyst obtained in Comparative Example 1 is 10-20nm, and the thickness of the carbon shell is 3-5nm, that is, the size of the deep nano nickel catalyst in Comparative Example 1 is much larger than that of the deep nano nickel catalyst in Example 1. Figure 2 It can be seen that this is because the crystallinity of Comparative Example 1 is significantly enhanced and the particles grow significantly, resulting in their larger size.

[0055] 2. Catalytic activity analysis

[0056] The catalytic activity of the deep nano nickel catalyst in Examples 1 to 5 and Comparative Example 1 was analyzed, including hydrogen oxidation electrochemical test and electrolytic hydrogen decomposition test. The electrolyte used in the hydrogen oxidation electrochemical test was a 0.1 mol / L KOH solution; the solution used in the electrolytic hydrogen decomposition test was a 1 mol / L KOH solution, the diameter of the glassy carbon electrode used was 5 mm, and the catalyst loading on the glassy carbon electrode was 0.5 mg / cm 2 , the rotating disk electrode speed is 2500 rpm.

[0057] Hydrogen hydroxide electrochemical test results are as follows Figure 3 As shown in the figure, it can be seen that the deep nano nickel catalyst prepared according to the preparation method of the present invention (Examples 1 to 5) shows better hydrogen oxidation catalytic activity than the deep nano nickel catalyst in Comparative Example 1.

[0058] The test results of electrolysis hydrogen are as follows Figure 4 As shown in the figure, it can be seen that the deep nano nickel catalyst prepared according to the preparation method (Examples 1 to 5) of the present invention shows better hydrogen evolution catalytic activity than the deep nano nickel catalyst in Comparative Example 1.

[0059] Although the specific implementation of the present invention is described in detail in conjunction with the embodiments, it should not be understood as limiting the scope of protection of this patent. Within the scope described in the claims, various modifications and variations that can be made by those skilled in the art without creative work still fall within the scope of protection of this patent.

Claims

1. A method for preparing a deep nano nickel catalyst, It is characterized in that The following steps are involved: S1: adding nickel salt and solid organic matter into a solvent, stirring and dissolving, to obtain a mixed solution; then evaporating the solvent of the mixed solution under vacuum conditions to obtain a solid precursor; the solid organic matter is at least one of citric acid, glucose, urea and melamine; S2: Grind the solid precursor through a 100-mesh sieve and then 2 / Ar mixed gas is pyrolyzed to obtain the H 2 H / Ar mixed gas 2 The volume fraction does not exceed 8%; the pyrolysis process is to heat the solid precursor to 350-500°C and keep it warm for 0.5-2h.

2. The preparation method according to claim 1, Features: The solvent is anhydrous ethanol; the ratio of the total mass of the nickel salt and the solid organic matter to the mass of the anhydrous ethanol is 1 to 3:

1.

3. The preparation method according to claim 1 or 2, Features: The molar ratio of the nickel salt to the solid organic matter is 1:0.2-2.

4. The preparation method according to claim 3, Features: The nickel salt is at least one of nickel nitrate, nickel chloride, nickel sulfate and nickel acetate.

5. The preparation method according to claim 4, Features: The nickel salt is nickel nitrate, and the solid organic matter is citric acid.

6. The preparation method according to claim 1, Features: The stirring and dissolving temperature in S1 is 45-80°C, and the stirring and dissolving time is 20-120 minutes; the temperature for evaporating the solvent is 60-90°C, and the time is 2-10 hours.

7. The preparation method according to claim 1, Features: The H 2 H / Ar mixed gas 2 The volume fraction is 2 to 4%.

8. The preparation method according to claim 1, Features: The heating rate of the solid precursor in S2 is 2 to 10 °C / min; The final temperature of the heating is 450°C and the holding time is 40 minutes.

9. A deep nano nickel catalyst, Features: The deep nano nickel catalyst is prepared by the preparation method according to any one of claims 1 to 8; the deep nano nickel catalyst comprises a nano nickel core and a carbon shell coated on the surface of the nano nickel core, the particle size of the nano nickel core is 4 to 6 nm, and the thickness of the carbon shell is 1 to 2 nm.

10. Use of the deep nano nickel catalyst according to claim 9 in the preparation of alkaline fuel cells, nickel hydrogen batteries or hydrogen production by water electrolysis.

Citation Information

Patent Citations

  • Carbon-coated nickel composite material and preparation method thereof

    CN109304475A

  • Nitrogen-doped induced carbon-coated bicrystal Ni catalyst as well as preparation method and application thereof

    CN116742024A

  • Preparation method and application of amorphous carbon coated nano nickel-based hydroxide catalyst

    CN116864699A