Semi-solid-state battery electrode and preparation method and application thereof
By using lithium-ion batteries to add gel electrolytes in electrode sheets, the shortcomings in cycling stability and safety performance of semi-solid lithium-ion batteries are solved, and a longer service life and higher safety performance are achieved.
Patent Information
- Application Number
- CN202411163952.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-22
AI Technical Summary
The cycle stability and safety performance of existing semi-solid lithium-ion batteries are insufficient, especially during charging and discharging. The structural instability of the positive electrode and the volume expansion of the negative electrode lead to material cracks and powderization, which affects the service life and safety of the battery. .
Add gel electrolyte to the electrode sheet, and through a network structure composed of lithium salt, organic solvent, film forming additive, polymer and thermal initiator, it protects the active substances and alleviates the material cracks caused by volume expansion and shrinkage and Powdering problems and improve the mechanical and mechanical properties of the battery.
It significantly improves the circulation and safety performance of the battery, extends the service life of the battery, enhances the safe needle penetration rate, and reduces the attenuation of active substances and the leakage of the battery.
Smart Images

Figure BDA0005007283300000121 
Figure BDA0005007283300000131 
Figure BDA0005007283300000141
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of battery materials and relates to a semi-solid battery electrode and a preparation method and application thereof. Background Art
[0002] The strong side reactions between high-voltage positive electrodes and traditional electrolytes will cause huge electrode / electrolyte interface impedance, affecting the actual use of the battery. In order to improve the cycle stability of the battery, FEC is widely used as an additive for high-energy-density lithium batteries because it has the ability to decompose into a film on the electrode surface and inhibit interface side reactions. However, the structural instability of the high-nickel ternary positive electrode determines that during the charge and discharge process, the transition metal elements (nickel, cobalt, and manganese) in its structure will dissolve in the electrolyte, and transfer from the positive electrode to the negative electrode surface during the charge and discharge process, seriously damaging the solid electrolyte intermediate layer. The industrialization of silicon-based negative electrodes is accelerating due to their high gram capacity, but silicon-based negative electrode materials have a volume expansion problem during the charge and discharge process. Volume expansion can cause cracks in silicon-based negative electrode materials until they are pulverized, destroying the contact between the electrode material and the current collector, causing the active material to detach from the electrode sheet, and causing rapid decay of the battery capacity.
[0003] CN118040074A discloses a semi-solid lithium ion battery and a preparation method thereof, wherein the semi-solid lithium ion battery comprises a semi-solid electrode and a semi-solid electrolyte; the semi-solid electrode comprises a current collector and an electrode film loaded on the surface of the current collector, the electrode film comprises an active material, a conductive agent, an adhesive, an inorganic electrolyte and a liquid electrolyte; the semi-solid electrolyte is an electrolyte film prepared by comprising an inorganic electrolyte, a liquid electrolyte, a polymer electrolyte and an adhesive.
[0004] CN117790693A discloses an electrode and a preparation method thereof, a semi-solid battery and an electrical device. The electrode preparation method comprises: mixing an active material with a binder to obtain a first slurry; applying the first slurry on the surface of a current collector to form a porous active electrode; mixing a first polymer electrolyte, a first lithium salt, an organic solvent, a first inorganic solid electrolyte, an additive and a conductive agent to obtain a second slurry; and applying and pouring the second slurry into the porous active electrode to obtain a composite electrode.
[0005] Although the electrode prepared by the above scheme can improve the cycle performance of the battery, its safety performance is reduced due to its structural characteristics, and it is difficult to meet the requirements of safe acupuncture, which limits its application in practice. Summary of the invention
[0006] The purpose of the present invention is to provide a semi-solid battery electrode and a preparation method and application thereof. In the present invention, adding gel electrolyte to the electrode plate can improve the cycle performance and safety performance of the battery, and the safe needle puncture pass rate of the gelled battery is significantly improved.
[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a semi-solid battery electrode, comprising a current collector and an active material layer disposed on at least one side of the current collector, wherein the active material layer comprises an active material and a gel electrolyte, wherein the gel electrolyte has a network structure, and wherein the gel electrolyte comprises a lithium salt, an organic solvent, a film-forming additive, a high molecular polymer, and a thermal initiator.
[0009] The present invention adds a gel electrolyte to the active material layer of the semi-solid battery electrode. When the semi-solid battery electrode is a positive electrode, the positive electrode active material is surrounded by a gel polymer with a network structure, which optimizes the surface of the positive electrode active particles, protects the positive electrode active material, and delays the attenuation of the positive electrode active material. When the semi-solid battery electrode is a negative electrode, the negative electrode active material is surrounded by a gel polymer with a network structure, which optimizes the surface of the negative electrode active particles, plays a good buffering and protective role on the expansion and contraction of the negative electrode during the charge and discharge process, reduces the cracking and pulverization of the particles, and delays the attenuation of the negative electrode active material.
[0010] Preferably, the lithium salt comprises any one of lithium bisfluorophosphorylimide, lithium bistrifluorophosphorylimide, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorophosphate, lithium hexafluorophosphate or lithium tetrafluoroborate, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of lithium bisfluorophosphorylimide and lithium hexafluorophosphate, a combination of lithium dioxalatoborate and lithium hexafluorophosphate, or a combination of lithium difluorooxalatoborate and lithium dioxalatoborate, etc.
[0011] Preferably, the organic solvent includes any one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethyl acetate, ethyl propionate, 1,3-dioxolane, 4-methyl-1,3-dioxolane, 1,2-dimethoxyethane, acetone, acetonitrile, methyl acetate, ethyl acetate, methyl propionate, tetrahydrofuran or 2-methyltetrahydrofuran, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of propylene carbonate and dimethyl carbonate, a combination of ethyl propionate and 1,3-dioxolane, or a combination of methyl acetate and ethyl acetate, etc.
[0012] Preferably, the semi-solid battery electrode is a positive electrode, and the film-forming additive includes any one or a group of at least two of vinylene carbonate, fluoroethylene carbonate, vinyl sulfate, tris(trimethylsilyl)phosphate, lithium difluorophosphate or lithium difluorooxalatoborate.
[0013] Preferably, the semi-solid battery electrode is a negative electrode, and the film-forming additive includes any one of vinylene carbonate, vinyl carbonate, fluoroethylene carbonate or vinyl sulfite, or a combination of at least two of them. Typical but non-limiting combinations include a combination of vinylene carbonate and vinyl carbonate, a combination of fluoroethylene carbonate and vinyl sulfite, or a combination of vinyl carbonate and fluoroethylene carbonate, etc.
[0014] Preferably, the monomers of the high molecular weight polymer include acrylic ester compounds.
[0015] Preferably, the acrylate compound includes (ethoxy) bisphenol A diacrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, 1,6-hexanediol diacrylate, (ethoxy) 1,6-hexanediol diacrylate, 1,4-butanediol acrylate, neopentyl glycol diacrylate, (propoxy) neopentyl glycol diacrylate, polyethylene glycol diacrylate, pentaerythritol triacrylate, trimethylolpropane triacrylate, (ethoxy) trimethylolpropane triacrylate, (propoxy) trimethylolpropane Any one of triacrylate, di(trimethylolpropane) tetraacrylate, pentaerythritol tetraacrylate, (ethoxy)pentaerythritol tetraacrylate, dipentaerythritol tetraacrylate or (ethoxy)dipentaerythritol tetraacrylate, or a combination of at least two thereof; typical but non-limiting combinations include a combination of polyethylene glycol diacrylate and pentaerythritol triacrylate, a combination of pentaerythritol tetraacrylate and (ethoxy)pentaerythritol tetraacrylate, or a combination of dipentaerythritol tetraacrylate and (ethoxy)dipentaerythritol tetraacrylate, etc.
[0016] Preferably, the thermal initiator includes any one of azobisisobutyronitrile, dibenzoyl peroxide, di(4-tert-butylcyclohexyl)peroxydicarbonate, dodecanoyl peroxide or diisopropyl peroxydicarbonate, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of azobisisobutyronitrile and dibenzoyl peroxide, a combination of di(4-tert-butylcyclohexyl)peroxydicarbonate and dodecanoyl peroxide, or a combination of dodecanoyl peroxide and diisopropyl peroxydicarbonate, etc.
[0017] Preferably, the mass ratio of lithium salt, organic solvent, film-forming additive and thermal initiator in the gel electrolyte is (10-20):(70-90):(1-10):(0.01-0.5), for example: 10:85:4.6:0.4, 15:82:2.8:0.2, 20:76:3.9:0.1, 18:80:1.5:0.5 or 12:86:1.85:0.15, etc., not limited to the listed values, other values not listed within the numerical range are also applicable.
[0018] Preferably, based on the mass of the gel electrolyte being 100%, the mass fraction of the high molecular weight polymer is 1 to 3%, for example, 1%, 1.5%, 2%, 2.5% or 3%, etc., not limited to the listed values, and other unlisted values within the numerical range are also applicable, preferably 1.5 to 2.5%.
[0019] Preferably, the mass ratio of the active material to the gel electrolyte is (90-95):(1-10), for example: 90:10, 91:9, 92:8, 94:6 or 95:5, etc., and is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0020] Preferably, the semi-solid battery electrode is a negative electrode, and the active material includes a carbon material, a silicon-carbon material or a silicon-oxygen material, preferably a combination of a carbon material and a silicon-oxygen material.
[0021] Preferably, the mass ratio of the silicon-carbon material to the silicon-oxygen material is (70-85):(15-30), for example: 70:30, 75:25, 80:20 or 85:15, etc., and is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0022] Preferably, the semi-solid battery electrode is a positive electrode, and the active material includes any one of a ternary nickel-cobalt-manganese positive electrode material, a lithium iron phosphate positive electrode material, a lithium manganese oxide positive electrode material, a lithium cobalt oxide positive electrode material or a nickel-manganese oxide lithium positive electrode material, or a combination of at least two thereof.
[0023] Preferably, the semi-solid battery electrode is a positive electrode, and the current collector comprises aluminum foil.
[0024] Preferably, the semi-solid battery electrode is a negative electrode, and the current collector comprises copper foil.
[0025] Preferably, the active material layer further includes a conductive agent and a binder.
[0026] Preferably, the conductive agent includes any one of conductive carbon black, carbon nanotubes, C65 or graphene, or a combination of at least two of them.
[0027] Preferably, the binder comprises polyvinylidene fluoride and / or styrene-butadiene rubber.
[0028] In a second aspect, the present invention provides a method for preparing the semi-solid battery electrode, the method comprising the following steps:
[0029] (1) mixing a lithium salt, a film-forming additive, a thermal initiator and an organic solution to obtain a mixed solution;
[0030] (2) mixing the mixed solution with the polymer monomer and stirring until the solution is clarified to obtain a gel electrolyte precursor solution;
[0031] (3) Mixing a gel electrolyte precursor solution and an active material to obtain an electrode slurry, coating the electrode slurry on a current collector surface, and pressing to obtain the semi-solid battery electrode.
[0032] During the preparation of the electrode of the present invention, the polymer monomers are cross-linked under the initiation of an initiator to form a high molecular polymer with a network structure, which is distributed between the particles of the battery pole piece, thereby alleviating the material cracking and pulverization problems caused by volume expansion and contraction between the particles, and also eliminating the battery leakage problem, thereby improving the mechanical and mechanical properties of the soft-pack battery.
[0033] Preferably, the molar concentration of the lithium salt in the mixed solution of step (1) is 1 to 1.2 mol / L, for example, 1 mol / L, 1.05 mol / L, 1.1 mol / L, 1.15 mol / L or 1.2 mol / L, etc., and is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0034] Preferably, the mass concentration of the film-forming additive in the mixed solution of step (1) is 1 to 10%, for example: 1%, 2%, 5%, 8% or 10%, etc., not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0035] Preferably, the mass concentration of the thermal initiator in the mixed solution of step (1) is 0.05-0.2%, for example: 0.05%, 0.08%, 0.1%, 0.15% or 0.2%, etc., not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0036] Preferably, a conductive agent and a binder are also added during the mixing process.
[0037] Preferably, the mass of the gel electrolyte precursor solution in step (3) is 2% to 10% of the total mass of the active material, conductive agent and binder, for example, 2%, 4%, 6%, 8% or 10%, etc., and is not limited to the listed values. Other values not listed within this numerical range are also applicable.
[0038] Preferably, the single-sided thickness of the coating in step (3) is 10 to 100 μm, for example, 10 μm, 20 μm, 50 μm, 80 μm or 100 μm, etc., and is not limited to the listed values. Other values not listed within the numerical range are also applicable.
[0039] Preferably, the pressing pressure in step (3) is 0.3-0.8 MPa, for example, 0.3 MPa, 0.4 MPa, 0.5 MPa, 0.6 MPa or 0.8 MPa, etc., and is not limited to the listed values. Other values not listed within the numerical range are also applicable.
[0040] Preferably, the pressing temperature in step (3) is 70-80°C, for example, 70°C, 72°C, 75°C, 78°C or 80°C, etc., and is not limited to the listed values. Other values not listed within the numerical range are also applicable.
[0041] In a third aspect, the present invention provides a semi-solid-state battery, wherein the semi-solid-state battery comprises the semi-solid-state battery electrode as described in the first aspect.
[0042] Preferably, the semi-solid battery further comprises an electrolyte.
[0043] Preferably, the electrolyte comprises a wetting additive.
[0044] Preferably, the wetting additive includes any one of fluorobenzene, dimethyl carbonate or dimethylsiloxane, or a combination of at least two thereof.
[0045] Preferably, the mass concentration of the wetting additive in the electrolyte is 0.05-0.2%, for example: 0.05%, 0.08%, 0.1%, 0.15% or 0.2%, etc., not limited to the listed values, other unlisted values within the numerical range are also applicable.
[0046] Compared with the prior art, the present invention has the following beneficial effects:
[0047] (1) The present invention adds a suitable gel electrolyte to the active material layer of the electrode plate. The gel electrolyte can form a gel substance between the active materials in the electrode, which can not only protect the active materials, but also when the electrode is a negative electrode, the meshed gel electrolyte can also delay the volume expansion of the active particles caused by battery charging and discharging, reduce the cracking and pulverization of the particles, and extend the service life of the battery.
[0048] (2) The present invention adds a suitable gel electrolyte to the active material layer of the electrode plate to form a gel material between the active materials of the battery plate, which can improve the safety performance of the electrode and increase the puncture rate of the battery plate. DETAILED DESCRIPTION
[0049] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0050] The monomers of various acrylic polymers used in the embodiments and comparative examples of the present invention, such as diethylene glycol diacrylate and pentaerythritol tetraacrylate, are conventional chemical products and can be purchased through conventional commercial channels. Pentaerythritol tetrapropylene ethyl ester, pentaerythritol tetrapropylene propyl ester, pentaerythritol tetrapropylene butyl ester, pentaerythritol tetraacrylate siloxane, pentaerythritol tetraacrylate ethyl siloxane, pentaerythritol tetraacrylate propyl siloxane, etc. can be synthesized with pentaerythritol tetraacrylate as the base material.
[0051] Example 1
[0052] The present embodiment provides a semi-solid battery negative electrode, the semi-solid battery negative electrode comprising a copper foil and a negative electrode active material layer disposed on the surface of the copper foil, the negative electrode active material layer comprising a composite negative electrode material (silicon-containing graphite + silicon oxide, mass ratio of 85:15), a conductive agent C65, a binder PVDF (polyvinylidene fluoride) and a gel electrolyte, the gel electrolyte comprising a lithium salt (lithium hexafluorophosphate), an organic solvent (ethylene carbonate + ethylene sulfate, volume ratio of 3:7), a film-forming additive (vinyl carbonate + propylene sulfite + vinyl sulfate, mass ratio of 1:1:1.5), a polymer monomer (pentaerythritol tetraacrylate) and a thermal initiator (azobisisobutyronitrile), the semi-solid battery negative electrode is prepared by the following method:
[0053] (1) lithium hexafluorophosphate was mixed with ethylene carbonate and ethyl methyl carbonate in a volume ratio of 3:7 to obtain a lithium salt solution with a lithium salt concentration of 1.1 mol / L, and then 1%, 1%, and 1.5% of vinylene carbonate, propylene sulfite, and vinyl sulfate were added to the lithium salt solution, respectively, and 0.1% of azobisisobutyronitrile was stirred to obtain a mixed solution;
[0054] (2) adding 1.5% of pentaerythritol tetraacrylate monomer to the mixed solution, stirring thoroughly until the solution is clear, and obtaining a gel electrolyte precursor solution (the mass fraction of pentaerythritol tetraacrylate in the gel electrolyte in the solution is 1.5%);
[0055] (3) Silicon-containing graphite, C65, and PVDF are mixed in a mass ratio of 94:3:3, and a gel electrolyte precursor solution with a total mass of 5% of silicon graphite, C65, and PVDF is added to obtain a negative electrode slurry. The negative electrode slurry is coated on the surface of a copper foil with a single-sided coating thickness of 50 μm, and rolled at 80° C. and a pressure of 0.5 MPa to obtain the semi-solid battery negative electrode.
[0056] Example 2
[0057] The present embodiment provides a semi-solid-state battery positive electrode, the semi-solid-state battery positive electrode comprising a carbon-coated aluminum foil and a positive electrode active material layer disposed on the surface of the aluminum foil, the positive electrode active material layer comprising NCM811, a conductive agent C65, a binder PVDF (polyvinylidene fluoride) and a gel electrolyte, the gel electrolyte comprising a lithium salt (lithium hexafluorophosphate), an organic solvent (ethylene carbonate + ethyl methyl carbonate, with a volume ratio of 3:7), a film-forming additive (vinyl carbonate + propylene sulfite + vinyl sulfate, with a mass ratio of 1:1:1.5), a polymer monomer (pentaerythritol tetraacrylate) and a thermal initiator (azobisisobutyronitrile), and the semi-solid-state battery positive electrode is prepared by the following method:
[0058] (1) lithium hexafluorophosphate was mixed with ethylene carbonate and ethyl methyl carbonate in a volume ratio of 3:7 to obtain a lithium salt solution with a lithium salt concentration of 1.1 mol / L, and then 1%, 1%, and 1.5% of vinylene carbonate, propylene sulfite, and vinyl sulfate were added to the lithium salt solution, respectively, and 0.1% of azobisisobutyronitrile was stirred to obtain a mixed solution;
[0059] (2) adding 2.5% of pentaerythritol tetraacrylate monomer to the mixed solution, stirring thoroughly until the solution is clear, and obtaining a gel electrolyte precursor solution (the mass fraction of pentaerythritol tetraacrylate in the gel electrolyte in the solution is 2.5%);
[0060] (3) Silicon-containing graphite, C65, and PVDF are mixed in a mass ratio of 94:3:3, and a gel electrolyte precursor solution with a total mass of 5% of NCM811, C65, and PVDF is added to obtain a positive electrode slurry. The positive electrode slurry is coated on the surface of a carbon-coated aluminum foil with a single-sided coating thickness of 100 μm. The positive electrode is rolled at 80° C. and a pressure of 0.5 MPa to obtain the semi-solid battery positive electrode.
[0061] Example 3
[0062] The present embodiment provides a semi-solid battery negative electrode, the semi-solid battery negative electrode comprising a copper foil and a negative electrode active material layer disposed on the surface of the copper foil, the negative electrode active material layer comprising a composite negative electrode material (silicon-containing graphite + silicon oxide, mass ratio of 70:30), a conductive agent C65, a binder PVDF (polyvinylidene fluoride) and a gel electrolyte, the gel electrolyte comprising a lithium salt (lithium hexafluorophosphate), an organic solvent (ethylene carbonate + ethyl methyl carbonate, volume ratio of 3:7), a film-forming additive (vinyl carbonate + propylene sulfite + vinyl sulfate, mass ratio of 1:1:1.5), a polymer monomer (dipropylene glycol diacrylate) and a thermal initiator (azobisisobutyronitrile), the semi-solid battery negative electrode is prepared by the following method:
[0063] (1) lithium hexafluorophosphate was mixed with ethylene carbonate and ethyl methyl carbonate in a volume ratio of 3:7 to obtain a lithium salt solution with a lithium salt concentration of 1.1 mol / L, and then 1%, 1%, and 1.5% of vinylene carbonate, propylene sulfite, and vinyl sulfate were added to the lithium salt solution, respectively, and 0.1% of azobisisobutyronitrile was stirred to obtain a mixed solution;
[0064] (2) adding 2.5% of diethylene glycol diacrylate monomer to the mixed solution, stirring thoroughly until the solution is clear, and obtaining a gel electrolyte precursor solution (the mass fraction of diethylene glycol diacrylate in the gel electrolyte in the solution is 2.5%);
[0065] (3) Silicon-containing graphite, C65, and PVDF are mixed in a mass ratio of 94:3:3, and a gel electrolyte precursor solution with a total mass of 5% of silicon graphite, C65, and PVDF is added to obtain a negative electrode slurry. The negative electrode slurry is coated on the surface of a copper foil with a single-sided coating thickness of 50 μm, and rolled at 80° C. and a pressure of 0.5 MPa to obtain the semi-solid battery negative electrode.
[0066] Example 4
[0067] The only difference between this embodiment and embodiment 1 is that the mass fraction of pentaerythritol tetraacrylate in the gel electrolyte is 1%, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0068] Example 5
[0069] The difference between this embodiment and embodiment 1 is that the mass fraction of pentaerythritol tetraacrylate in the gel electrolyte is 3%, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0070] Example 6
[0071] The only difference between this embodiment and embodiment 2 is that the mass fraction of pentaerythritol tetraacrylate in the gel electrolyte is 1%, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0072] Example 7
[0073] The only difference between this embodiment and embodiment 2 is that the mass fraction of pentaerythritol tetraacrylate in the gel electrolyte is 3%, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0074] Application Example 1
[0075] In this application example, the negative electrode plate obtained in Example 1, the positive electrode plate obtained in Example 2 and the diaphragm are wound or laminated, the tabs are welded, and the battery is packaged to form a semi-solid gel battery cell. The immersion electrolyte 1mol / L LIPF6, EC / EMC=3:7, 1%, FB, is injected into the battery, and after being left at room temperature for 48 hours, it is formed at room temperature, the upper limit of the formation voltage is 3.8V, and the charging current is 0.1C and 0.2C; the formed battery is aged at high temperature, the aging temperature is 45°C, the time is 24h, and after aging, vacuum is evacuated, the vacuum degree is 88kPa, and the vacuum evacuation time is set to 5s, the film potential data is checked, the battery quality is checked, and the battery liquid absorption is estimated; the formed battery is divided into different capacities, and the currents of the different capacities are 0.2C and 0.5C respectively. After 2 weeks of cyclic charge and discharge, the battery process is completed, and other electrical performance tests can be performed.
[0076] Application Example 2
[0077] The only difference between this application example and application example 1 is that the negative electrode sheet prepared in embodiment 1 is replaced with the negative electrode sheet prepared in embodiment 3, and the other conditions and parameters are exactly the same as those in application example 1.
[0078] Application Example 3
[0079] The only difference between this application example and application example 1 is that the negative electrode sheet prepared in embodiment 1 is replaced with the negative electrode sheet prepared in embodiment 4, and the other conditions and parameters are exactly the same as those in application example 1.
[0080] Application Example 4
[0081] The only difference between this application example and application example 1 is that the negative electrode sheet prepared in embodiment 1 is replaced with the negative electrode sheet prepared in embodiment 5, and the other conditions and parameters are exactly the same as those in application example 1.
[0082] Application Example 5
[0083] The only difference between this application example and application example 1 is that the positive electrode sheet prepared in embodiment 2 is replaced with the positive electrode sheet prepared in embodiment 6, and the other conditions and parameters are exactly the same as those in application example 1.
[0084] Application Example 6
[0085] The only difference between this application example and application example 1 is that the positive electrode sheet prepared in embodiment 2 is replaced with the positive electrode sheet prepared in embodiment 7, and the other conditions and parameters are exactly the same as those in application example 1.
[0086] Application Example 7
[0087] The only difference between this application example and application example 1 is that fluorobenzene is not added to the electrolyte, and other conditions and parameters are exactly the same as those in application example 1.
[0088] Comparative application example 1
[0089] The only difference between this comparative application example and application example 1 is that no gel electrolyte is added to the positive and negative electrode plates, and the gel electrolyte is injected into the battery in the form of a solution, that is, the gel electrolyte solution is injected after the positive and negative electrodes and the separator are assembled into a battery. Other conditions and parameters are exactly the same as those in application example 1.
[0090] The differences in the components of the electrode and electrolyte are shown in Table 1 below:
[0091] Table 1
[0092]
[0093]
[0094] Performance Test:
[0095] (1) Initial internal resistance: Place the lithium-ion battery at 25°C, discharge it at a constant current of 0.5C to the lower limit voltage (3.0V), let it stand for 5 minutes, and directly test the battery ohmic impedance using an internal resistance tester. The AC signal frequency is set to 1KHz.
[0096] (2) First discharge capacity: Place the lithium-ion battery at 25°C, discharge it at a constant current of 0.5C to the lower limit voltage of the battery, and let it stand for 5 minutes; then charge it at a constant current of 0.5C to the upper limit voltage, and then charge it at a constant voltage of the upper limit voltage to a current of 0.05C, and let it stand for 5 minutes; then discharge it at a constant current of 0.5C to the lower limit voltage, and record the discharge capacity, which is the first discharge capacity.
[0097] (3) Cycle life at room temperature: Place the lithium-ion battery at 25°C, discharge at a constant current of 0.5C to the lower limit voltage (3.0V), and let it stand for 5 minutes; then charge at a constant current of 0.5C to the upper limit voltage (4.48V), then charge at a constant voltage of 4.48V to a current of 0.05C, and let it stand for 5 minutes; then discharge at a constant current of 0.5C to a voltage of 3.0V, and let it stand for 5 minutes. This is one charge and discharge cycle. Charge / discharge in this way until the ratio of the discharge capacity to the initial discharge capacity in a certain cycle is ≤80%. The number of cycles experienced is the cycle life.
[0098] (4) Safety puncture test pass rate: The safety puncture test is to place the battery in a 25°C environment, discharge it at 0.2C to the lower limit voltage, and let it stand for 10 minutes; then charge it at a constant current of 0.5C to the upper limit voltage (4.48V), and then charge it at a constant voltage of 4.48V to a current of 0.05C, and let it stand for 5 minutes; use a high-temperature resistant steel needle with a diameter of Ф (2.0±0.2) mm to penetrate it at a speed of (25mm±2.5mm / s) from a direction perpendicular to the battery plate, and the puncture position should be close to the geometric center of the punctured surface (the steel needle stays in the battery); observe for 30 minutes whether the battery catches fire or explodes. If the battery does not catch fire or explode, the test is passed. The ratio of the number of batteries that pass the test to the total number of tests in the same batch is defined as the pass rate. The test results are shown in Table 2:
[0099] Table 2
[0100]
[0101] As can be seen from Table 2, from Application Examples 1-2, the first discharge capacity of the battery made of the semi-solid battery electrode of the present invention can reach more than 1832 mAh, the initial internal resistance can reach less than 86 mΩ, the cycle life can reach more than 742 times, and the needle puncture pass rate can reach 100%.
[0102] By comparing Application Example 1 with Application Examples 3-4 and Application Example 1 with Application Examples 5-6, it can be concluded that the mass proportion of the polymer in the gel electrolyte of the semi-solid battery electrode plate of the present invention will affect its performance. When the mass proportion of the polymer in the gel electrolyte is controlled at 1.5-2.5%, the performance of the electrode plate obtained is better. If the mass proportion of the polymer in the gel electrolyte is too high, the cycle performance and rate charge and discharge performance of the battery will be significantly reduced. If the mass proportion of the polymer in the gel electrolyte is too low, the safety test performance of the battery will be affected.
[0103] From the comparison between Application Example 1 and Application Example 7, it can be seen that the wetting electrolyte also improves the performance of the gel semi-solid battery, and the wetting electrolyte has no effect on the safety performance of the battery.
[0104] By comparing Example 1 with Comparative Example 1, it can be seen that the use of gel electrolyte in the electrode plate of the present invention has an improvement effect on the cycle performance and safety performance of the battery. The safe needle puncture rate of the gelled battery is high, and the safe needle puncture rate of the ungelled or liquid battery is low.
[0105] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A semi-solid battery electrode, characterized in that: The semi-solid battery electrode includes a current collector and an active material layer arranged on at least one side of the current collector. The active material layer includes an active material and a gel electrolyte. The gel electrolyte has a network structure and includes a lithium salt, an organic solvent, a film-forming additive, a high molecular polymer and a thermal initiator.
2. The semi-solid battery electrode according to claim 1, characterized in that: The lithium salt includes any one of lithium bis(fluorophosphorylimide), lithium bis(trifluorophosphorylimide), lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorophosphate, lithium hexafluorophosphate or lithium tetrafluoroborate, or a combination of at least two thereof; Preferably, the organic solvent comprises any one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethyl acetate, ethyl propionate, 1,3-dioxolane, 4-methyl-1,3-dioxolane, 1,2-dimethoxyethane, acetone, acetonitrile, methyl acetate, ethyl acetate, methyl propionate, tetrahydrofuran or 2-methyltetrahydrofuran, or a combination of at least two thereof; Preferably, the semi-solid battery electrode is a positive electrode, and the film-forming additive includes any one or a combination of at least two of vinylene carbonate, fluoroethylene carbonate, vinyl sulfate, tris(trimethylsilyl)phosphate, lithium difluorophosphate or lithium difluorooxalatoborate; Preferably, the semi-solid battery electrode is a negative electrode, and the film-forming additive includes any one or a combination of at least two of vinylene carbonate, ethylene carbonate, fluoroethylene carbonate or 1,3-propane sultone; Preferably, the monomer of the high molecular polymer includes an acrylic acid ester compound; Preferably, the acrylate compound includes any one of (ethoxy) bisphenol A diacrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, 1,6-hexanediol diacrylate, (ethoxy) 1,6-hexanediol diacrylate, 1,4-butanediol acrylate, neopentyl glycol diacrylate, (propoxy) neopentyl glycol diacrylate, polyethylene glycol diacrylate, pentaerythritol triacrylate, trimethylolpropane triacrylate, (ethoxy) trimethylolpropane triacrylate, (propoxy) trimethylolpropane triacrylate, di(trimethylolpropane) tetraacrylate, pentaerythritol tetraacrylate, (ethoxy) pentaerythritol tetraacrylate, dipentaerythritol tetraacrylate or (ethoxy) dipentaerythritol tetraacrylate, or a combination of at least two thereof; Preferably, the thermal initiator includes any one of azobisisobutyronitrile, dibenzoyl peroxide, di(4-tert-butylcyclohexyl)peroxydicarbonate, dodecanoyl peroxide or diisopropyl peroxydicarbonate, or a combination of at least two thereof.
3. The semi-solid battery electrode according to claim 2, characterized in that: The mass ratio of lithium salt, organic solvent, film-forming additive and thermal initiator in the gel electrolyte is (10-20):(70-90):(1-10):(0.01-0.5); Preferably, based on 100% of the mass of the gel electrolyte, the mass fraction of the high molecular weight polymer is 1 to 3%, preferably 1.5 to 2.5%.
4. The semi-solid battery electrode according to any one of claims 1 to 3, characterized in that: The mass ratio of the active material to the gel electrolyte is (90-95):(1-10); Preferably, the semi-solid battery electrode is a negative electrode, and the active material comprises a carbon material, a silicon-carbon material or a silicon-oxygen material, preferably a combination of a carbon material and a silicon-oxygen material; Preferably, the mass ratio of the carbon material to the silicon-oxygen material is (70-85):(15-30); Preferably, the semi-solid battery electrode is a positive electrode, and the active material includes any one of a ternary nickel-cobalt-manganese positive electrode material, a lithium iron phosphate positive electrode material, a lithium manganese oxide positive electrode material, a lithium cobalt oxide positive electrode material or a nickel-manganese oxide lithium positive electrode material, or a combination of at least two thereof.
5. The semi-solid battery electrode according to any one of claims 1 to 4, characterized in that: The semi-solid battery electrode is a positive electrode, and the current collector comprises aluminum foil; Preferably, the semi-solid battery electrode is a negative electrode, and the current collector comprises copper foil; Preferably, the active material layer further comprises a conductive agent and a binder; Preferably, the conductive agent includes any one or a combination of at least two of conductive carbon black, carbon nanotubes, C65 or graphene; Preferably, the binder comprises polyvinylidene fluoride and / or styrene-butadiene rubber.
6. A method for preparing a semi-solid battery electrode according to any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: (1) mixing a lithium salt, a film-forming additive, a thermal initiator and an organic solution to obtain a mixed solution; (2) mixing the mixed solution with the polymer monomer and stirring until the solution is clarified to obtain a gel electrolyte precursor solution; (3) Mixing a gel electrolyte precursor solution and an active material to obtain an electrode slurry, coating the electrode slurry on a current collector surface, and pressing to obtain the semi-solid battery electrode.
7. The preparation method according to claim 6, characterized in that: The molar concentration of the lithium salt in the mixed solution of step (1) is 1 to 1.2 mol / L; Preferably, the concentration of the film-forming additive in the mixed solution of step (1) is 1 to 10% of the electrolyte content; Preferably, the concentration of the thermal initiator in the mixed solution in step (1) is 0.01 to 0.5% of the electrolyte content.
8. The preparation method according to claim 6 or 7, characterized in that: During the mixing process of step (3), a conductive agent and a binder are also added; Preferably, the mass of the gel electrolyte precursor solution is 2-10% of the total mass of the active material, the conductive agent and the binder.
9. The preparation method according to any one of claims 6 to 8, characterized in that: The single-side thickness of the coating in step (3) is 10 to 100 μm; Preferably, the pressing pressure in step (3) is 0.3-0.8 MPa; Preferably, the pressing temperature in step (3) is 70-80°C.
10. A semi-solid battery, characterized in that: The semi-solid-state battery comprises a semi-solid-state battery electrode as claimed in any one of claims 1 to 5; Preferably, the semi-solid battery further comprises an electrolyte; Preferably, the electrolyte includes a wetting additive; Preferably, the wetting additive comprises any one or a combination of at least two of fluorobenzene, dimethyl carbonate or dimethylsiloxane; Preferably, the mass concentration of the wetting additive in the electrolyte is 0.05-1%.
Citation Information
Cited By
Semi-solid-state battery positive electrode, preparation method thereof and semi-solid-state battery
CN121662735A
A semi-solid battery positive electrode and a preparation method thereof, and a semi-solid battery
CN121662735B