Lithium ion battery electrolyte, lithium ion battery and electric equipment

By using tetra-(2-methyl-8-hydroxyquinoline) boron lithium and a specific structure additive S in the lithium-ion battery electrolyte, the lithium-ion battery is solved in the high-level interface mask. The gas production and charge transfer impedance problems under high voltage and high temperature conditions improve the cycling performance and first-time efficiency of the battery.

CN119009133AActive Publication Date: 2024-11-22GAC AION NEW ENERGY AUTOMOBILE CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411395422.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-08
Publication Date
2024-11-22
Estimated Expiration
2044-10-08

AI Technical Summary

Technical Problem

Existing lithium-ion batteries are prone to gas under high voltage and high temperature conditions, resulting in a decrease in circulation life, and the interface film formed by additives is relatively large, affecting the first-time efficiency of the battery.

Method used

Using tetra-(2-methyl-8-hydroxyquinoline) boron lithium and additive S with specific structures, the organic polymer-inorganic lithium salt composite interface mask is formed to alleviate the violent decomposition and gas production of electrolyte under high voltage and high temperature conditions. Problem: neutralize hydrofluoric acid, reduce charge transfer impedance, and improve the cycling performance and first-time efficiency of the battery.

Benefits of technology

Significantly improve the cycling performance and first-time efficiency of lithium-ion batteries under high voltage and high temperature conditions, reduce active lithium ion consumption, and improve the thermal stability and charge transfer efficiency of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005073636350000021
    Figure BDA0005073636350000021
  • Figure BDA0005073636350000061
    Figure BDA0005073636350000061
  • Figure BDA0005073636350000081
    Figure BDA0005073636350000081
Patent Text Reader

Abstract

The invention provides a lithium ion battery electrolyte, a lithium ion battery and electric equipment, and belongs to the technical field of lithium ion battery manufacturing. The lithium ion battery electrolyte comprises an organic solvent, a lithium salt and an additive, the additive comprises tetra (2-methyl-8-hydroxyquinoline) boron lithium and an additive S, the structural formula of the additive S is as shown in formula I, R1 and R2 in the formula I are respectively and independently selected from any one of hydrogen atoms, fluorine atoms, substituted or unsubstituted C1-C3 alkyl groups and substituted silyl groups, and R1 and R2 in the formula I are respectively and independently selected from any one of hydrogen atoms, fluorine atoms, substituted or unsubstituted C1-C3 alkyl groups and substituted silyl groups. The electrolyte can improve the problem of serious gas production when a corresponding lithium ion battery is applied under high-voltage and high-temperature conditions, so that the battery has relatively excellent cycle performance; and meanwhile, the charge transfer impedance of the corresponding battery at the interface can be reduced, and the active lithium ion consumption in the formation stage is reduced, so that the battery has relatively high first efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium-ion battery manufacturing, and in particular to a lithium-ion battery electrolyte, a lithium-ion battery and an electrical device. Background Art

[0002] In the prior art, lithium-ion batteries are used as power batteries in new energy vehicles because of their advantages such as green environmental protection, high energy density and long cycle life. Since new energy vehicles have high energy, long endurance and high and low temperature requirements, high-voltage ternary, lithium nickel manganese oxide and other high-energy cathode materials have become the development hotspots of new power batteries. However, when the existing commercial electrolyte is charged and discharged at high voltage (≥4.5V) and high temperature (≥45℃), the organic solvent in the electrolyte is easily oxidized and decomposed at the cathode interface and a large amount of gas is generated, resulting in the loss of active lithium ions at the cathode, which in turn leads to a sharp decrease in the battery cycle life. In order to suppress the gas production when the battery is used under high voltage and high temperature conditions, the current main method is to add additives such as 1,3-propene sultone (PST) and maleic anhydride to the electrolyte to improve the battery performance. However, these additives have poor effect on improving the high temperature performance of the battery at high voltages above 4.5V, so that the battery still has a more serious gas production problem when it is used under high voltage and high temperature conditions; in addition, the interface film formed by these additives also has a large impedance problem, which also affects the initial efficiency of the battery. Summary of the invention

[0003] The purpose of the present application is to provide a lithium-ion battery electrolyte, a lithium-ion battery and electrical equipment, which can improve the serious gas production problem of the corresponding lithium-ion battery when used under high voltage and high temperature conditions, so that the battery has a relatively excellent cycle performance; at the same time, it can also reduce the charge transfer impedance of the corresponding battery at the interface and reduce the consumption of active lithium ions in the formation stage, so that the battery has a higher initial efficiency.

[0004] The embodiment of the present application is implemented as follows:

[0005] In a first aspect, an embodiment of the present application provides a lithium-ion battery electrolyte, including an organic solvent, a lithium salt and an additive, wherein the additive includes lithium tetrakis(2-methyl-8-hydroxyquinoline)borate and an additive S, and the structural formula of the additive S is as shown in Formula I:

[0006]

[0007] Among them, R 1 and R 2 Each of them is independently selected from any one of a hydrogen atom, a fluorine atom, a substituted or unsubstituted C1-C3 alkyl group and a substituted silyl group.

[0008] In the above technical solution, the lithium-ion battery electrolyte has the above-mentioned specific combination of additive components. On the one hand, the carboxylic anhydride in the above-mentioned specific structural additive S can form an interface film with good thermal stability on the surface of both the positive and negative electrodes, thereby effectively alleviating the problem of violent decomposition and gas production at the positive and negative electrode interfaces when the electrolyte is used under high voltage and high temperature conditions (helping to improve the battery's cycle performance); at the same time, the bipyridine ring in the structure has weak alkalinity and can neutralize the hydrofluoric acid produced by the decomposition of the electrolyte, thereby further alleviating the problem of poor battery performance caused by gas production (also helping to improve the battery's cycle performance), and the bipyridine ring can also complex some metal ions dissolved from the positive electrode (such as manganese ions), thereby improving the problem of battery capacity decay caused by the deposition of dissolved metal ions at the negative electrode. On the other hand, tetrakis(2-methyl-8-hydroxyquinoline)borate lithium can also decompose at the positive electrode to form an interface film rich in boron oxide and alkyl lithium, which can be synergistically decomposed with the additive S to form an organic polymer-inorganic lithium salt composite interface film on the positive electrode surface, thereby further improving the thermal stability of the interface film formed by the battery at the positive electrode interface; at the same time, the formed organic polymer-inorganic lithium salt composite interface film can also reduce the charge transfer impedance of the battery at the positive electrode interface, reduce the active lithium ion consumption in the formation stage, and thus improve the first efficiency of the battery. In the embodiment of the present application, by using two additives of specific structures for use in combination, the problem of severe gas production when the corresponding lithium-ion battery is used under high voltage and high temperature conditions can be improved, so that the battery has a relatively excellent cycle performance; at the same time, it can also make the battery have a higher first efficiency.

[0009] In some alternative embodiments, R 1 and R 2 Each of the groups is independently selected from any one of a hydrogen atom, a fluorine atom, a methyl group, an ethyl group, a propyl group, a trifluoromethyl group and trimethylsilane.

[0010] In the above technical solution, the structural selection of the additive S is further limited within a specific range, which helps to further improve the cycle performance and initial efficiency of the battery corresponding to the electrolyte when used at high voltage and high temperature.

[0011] In some optional embodiments, the mass percentage of the additive in the electrolyte is 0.2-3%.

[0012] In the above technical solution, the total amount of the additive is limited to a specific range, so that the battery corresponding to the electrolyte has relatively excellent cycle performance and initial efficiency when used at a high voltage.

[0013] In some optional embodiments, the electrolyte further includes an auxiliary additive, the auxiliary additive including at least one of vinyl sulfate, vinyl ethylene carbonate, 1,3-propane sultone, methylene disulfonate, 2-fluoropyridine, allyl isocyanate, triallyl isocyanurate, 2(5H)-furanone, tris(trimethylsilyl)phosphite and tripropylene phosphate.

[0014] In the above technical solution, adding a specific type of auxiliary additive to the electrolyte can give the electrolyte more functions, thereby more comprehensively improving the comprehensive electrical performance of the corresponding battery (such as safety performance and cycle performance, etc.).

[0015] In some optional embodiments, the mass percentage of the auxiliary additive in the electrolyte is 0.5-5%.

[0016] In the above technical solution, the dosage of the auxiliary additive is limited to a specific range, so that the auxiliary additive has a suitable dosage, thereby being able to better improve the comprehensive electrical performance of the corresponding battery.

[0017] In some optional embodiments, the lithium salt includes at least one of lithium hexafluorophosphate, lithium difluorophosphate, lithium bis(fluorosulfonyl)imide, lithium difluorobis(oxalatophosphate), lithium tetrafluorooxalatophosphate, lithium difluorooxalatoborate, lithium bis(trifluoromethylsulfonyl)imide, and lithium bis(oxalatoborate).

[0018] Optionally, the mass percentage of lithium salt in the electrolyte is 10-20%.

[0019] Among the above technical solutions, the technical solution provided in the embodiment of the present application is applicable to a large number of lithium salt types and can provide a large number of feasible implementation plans, thereby facilitating the promotion and application of the technical solution provided in the present application.

[0020] Furthermore, limiting the amount of lithium salt to the above range can ensure that the lithium salt has a suitable amount, thereby better improving the comprehensive electrical performance of the corresponding battery.

[0021] In some optional embodiments, the organic solvent includes at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, dimethyl carbonate, fluoroethylene carbonate, 3,3,3-trifluoropropylene carbonate, methyl trifluoroethyl carbonate and 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether.

[0022] Among the above technical solutions, the technical solutions provided in the embodiments of the present application are applicable to a wide variety of organic solvents and can provide a wide variety of feasible implementation plans, thereby facilitating the promotion and application of the technical solutions provided in the present application.

[0023] In a second aspect, an embodiment of the present application provides a lithium-ion battery, comprising a housing, an electrode assembly, and the electrolyte provided in the embodiment of the first aspect. The electrode assembly is contained in the housing; and the electrolyte is contained in the housing.

[0024] In the above technical solution, the lithium-ion battery includes the electrolyte provided in the first aspect embodiment. With the unique advantages of the electrolyte, the lithium-ion battery has relatively excellent cycle performance and higher initial efficiency when used under high voltage and high temperature conditions.

[0025] In some optional embodiments, in the battery positive electrode of the electrode assembly, the positive electrode active material includes at least one of a transition metal phosphate and a transition metal oxide lithium salt.

[0026] Optionally, the positive electrode active material includes at least one of lithium iron manganese phosphate, lithium nickel cobalt manganese oxide, lithium nickel manganese oxide and lithium cobalt oxide.

[0027] Among the above technical solutions, the technical solution provided in the embodiment of the present application can be applied to the above-mentioned various positive electrode active material systems, providing more feasible implementation plans, thereby facilitating the promotion and application of the technical solution provided in the embodiment of the present application.

[0028] In addition, the use of the above-mentioned specific type of positive electrode active material has the advantage of being more resistant to high voltage and high temperature compared to the use of other types of positive electrode active materials.

[0029] In some optional embodiments, in the battery negative electrode of the electrode assembly, the negative electrode active material includes at least one of graphite, soft carbon, hard carbon, silicon, silicon oxides, and silicon-carbon composites.

[0030] Among the above technical solutions, the technical solution provided in the embodiment of the present application can be applied to the above-mentioned various negative electrode active material systems, providing more feasible implementation plans, thereby facilitating the promotion and application of the technical solution provided in the embodiment of the present application.

[0031] In a third aspect, an embodiment of the present application provides an electrical device, comprising a lithium-ion battery as provided in the embodiment of the second aspect. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0033] It should be noted that “and / or” in this application, such as “Feature 1 and / or Feature 2”, refers to the three situations of “Feature 1” alone, “Feature 2” alone, or “Feature 1” plus “Feature 2”.

[0034] In addition, in the description of the present application, unless otherwise specified, the meaning of "multiple" in "one or more" refers to two or more; the range of "value a ~ value b" includes the two end values ​​"a" and "b", and the "unit" in "value a ~ value b + unit of measurement" represents the "unit of measurement" of both "value a" and "value b".

[0035] In the prior art, high-voltage resistant electrolyte additives usually use some organic substances, such as 1,3-propylene sultone or maleic anhydride, etc., but these additives are not effective in inhibiting gas production when used under high voltage and high temperature conditions, resulting in poor battery cycle performance. In addition, the interface film formed by these additives also has a large interface impedance, resulting in poor initial efficiency of the battery.

[0036] The inventors have found that by using a composite system of an additive S containing a bipyridine ring and a specific acid anhydride skeleton and lithium tetrakis(2-methyl-8-hydroxyquinoline)borate as an additive, the problem of severe gas production when the corresponding lithium-ion battery is used under high voltage and high temperature conditions can be improved, so that the battery has relatively excellent cycle performance; at the same time, it can also make the battery have a higher initial efficiency.

[0037] The following is a detailed description of a lithium-ion battery electrolyte, a lithium-ion battery, and an electrical device in an embodiment of the present application.

[0038] In a first aspect, an embodiment of the present application provides a lithium-ion battery electrolyte, including an organic solvent, a lithium salt and an additive, wherein the additive includes lithium tetrakis(2-methyl-8-hydroxyquinoline)borate and an additive S, and the structural formula of the additive S is as shown in Formula I:

[0039]

[0040] Among them, R 1 and R 2 Each of them is independently selected from any one of a hydrogen atom, a fluorine atom, a substituted or unsubstituted C1-C3 alkyl group and a substituted silyl group.

[0041] In the present application, the lithium-ion battery electrolyte has the above-mentioned specific combination of additive components. On the one hand, the carboxylic anhydride in the above-mentioned specific structural additive S can form an interface film with good thermal stability on the surface of both the positive and negative electrodes, thereby effectively alleviating the problem of violent decomposition and gas production at the positive and negative electrode interfaces when the electrolyte is used under high voltage and high temperature conditions (helping to improve the battery's cycle performance); at the same time, the bipyridine ring in the structure has weak alkalinity and can neutralize the hydrofluoric acid produced by the decomposition of the electrolyte, thereby further alleviating the problem of poor battery performance caused by gas production (also helping to improve the battery's cycle performance), and the bipyridine ring can also complex some metal ions dissolved from the positive electrode (such as manganese ions), thereby improving the problem of battery capacity decay caused by the deposition of dissolved metal ions at the negative electrode. On the other hand, tetrakis(2-methyl-8-hydroxyquinoline)borate lithium can also decompose at the positive electrode to form an interface film rich in boron oxide and alkyl lithium, which can be synergistically decomposed with the additive S to form an organic polymer-inorganic lithium salt composite interface film on the positive electrode surface, thereby further improving the thermal stability of the interface film formed by the battery at the positive electrode interface; at the same time, the formed organic polymer-inorganic lithium salt composite interface film can also reduce the charge transfer impedance of the battery at the positive electrode interface, reduce the active lithium ion consumption in the formation stage, and thus improve the first efficiency of the battery. In the embodiment of the present application, by using two additives of specific structures for use in combination, the problem of severe gas production when the corresponding lithium-ion battery is used under high voltage and high temperature conditions can be improved, so that the battery has a relatively excellent cycle performance; at the same time, it can also make the battery have a higher first efficiency.

[0042] It should be noted that since there are many components in the electrolyte and the physical and chemical properties of each component are different, it is necessary to focus on whether the components are compatible with each other in the process of selecting additives, that is, whether they will affect other components in the process of exerting their effects. This is one of the main reasons why there are many compounds with the same functional groups but few systems that can be used as composite additives. This is also a major difficulty in designing composite additive systems in this field.

[0043] As an example, R 1 and R 2 Each of the groups is independently selected from any one of a hydrogen atom, a fluorine atom, a methyl group, an ethyl group, a propyl group, a trifluoromethyl group and trimethylsilane.

[0044] In this embodiment, the structural selection of the additive S is further limited within a specific range, which helps to further improve the cycle performance and initial efficiency of the battery corresponding to the electrolyte when used at high voltage and high temperature.

[0045] In order to better understand the technical solution, some specific compound structures of the additive S are used as examples below.

[0046]

[0047]

[0048]

[0049] It should be noted that the effect of additives is closely related to their dosage. Specifically, if the dosage is too small, the performance of the corresponding battery cannot be effectively improved; if the dosage is too high, the interface film formed will be too thick, which will also affect the performance of the corresponding battery. Based on this, considering the final performance of the corresponding battery, the dosage of the additive can be limited.

[0050] As an example, the mass percentage of the additive in the electrolyte is 0.2-3%, for example but not limited to any one of 0.2%, 0.5%, 1%, 1.5%, 2%, 2.5% and 3% by mass or a range between any two of them.

[0051] In this embodiment, the amount of the additive is limited to a specific range so that the battery corresponding to the electrolyte has relatively excellent cycle performance and initial efficiency when used at a high voltage.

[0052] As an example, the electrolyte also includes auxiliary additives, and the auxiliary additives include at least one of vinyl sulfate, vinyl ethylene carbonate, 1,3-propane sultone, methylene disulfonate, 2-fluoropyridine, allyl isocyanate, triallyl isocyanurate, 2(5H)-furanone, tris(trimethylsilyl)phosphite and tripropylene phosphate.

[0053] In this embodiment, adding a specific type of auxiliary additive to the electrolyte can give the electrolyte more functions, thereby more comprehensively improving the comprehensive electrical performance of the corresponding battery (such as safety performance and cycle performance, etc.).

[0054] As an example, the mass percentage of the auxiliary additive in the electrolyte is 0.5-5%, for example but not limited to any one of 0.5%, 1%, 2%, 3%, 4% and 5% or a range between any two of them.

[0055] In this embodiment, the amount of the auxiliary additive is limited to a specific range, so that the auxiliary additive has a suitable amount, thereby being able to better improve the comprehensive electrical performance of the corresponding battery.

[0056] As an example, the lithium salt includes at least one of lithium hexafluorophosphate, lithium difluorophosphate, lithium bis(fluorosulfonyl)imide, lithium difluorobis(oxalatophosphate), lithium tetrafluorooxalatophosphate, lithium difluorooxalatoborate, lithium bis(trifluoromethylsulfonyl)imide, and lithium bis(oxalatoborate).

[0057] In this embodiment, the technical solution provided in the embodiment of the present application is applicable to a large number of lithium salt types and can provide a large number of feasible implementation plans, thereby facilitating the promotion and application of the technical solution provided in the present application.

[0058] As an example, the mass percentage of lithium salt in the electrolyte is 10-20%, for example but not limited to any one of 10%, 12%, 14%, 16%, 18% and 20% or a range between any two of the mass percentages.

[0059] In this embodiment, the amount of lithium salt is further limited to the above range, so that the lithium salt has a suitable amount, thereby being able to better improve the comprehensive electrical performance of the corresponding battery.

[0060] As an example, the organic solvent includes at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, dimethyl carbonate, fluoroethylene carbonate, 3,3,3-trifluoropropylene carbonate, methyl trifluoroethyl carbonate, and 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether.

[0061] In this embodiment, the technical solution provided in the embodiment of the present application is applicable to a wide variety of organic solvents and can provide a wide variety of feasible implementation plans, thereby facilitating the promotion and application of the technical solution provided in the present application.

[0062] It should be noted that the components and amounts thereof in the electrolyte that are not particularly described or limited may be set according to conventional selections in the art.

[0063] In a second aspect, an embodiment of the present application provides a lithium-ion battery, comprising a housing, an electrode assembly, and the electrolyte provided in the embodiment of the first aspect. The electrode assembly is contained in the housing; and the electrolyte is contained in the housing.

[0064] In the present application, the lithium-ion battery includes the electrolyte provided in the first aspect embodiment. With the unique advantages of the electrolyte, the lithium-ion battery has relatively excellent cycle performance and higher initial efficiency when used under high voltage and high temperature conditions.

[0065] As an example, in the battery positive electrode of the electrode assembly, the positive electrode active material includes at least one of a transition metal phosphate and a transition metal oxide lithium salt.

[0066] In this embodiment, the technical solution provided in the embodiment of the present application can be applied to the above-mentioned various positive electrode active material systems, providing more feasible implementation plans, thereby facilitating the promotion and application of the technical solution provided in the embodiment of the present application.

[0067] As an example, the positive electrode active material includes at least one of lithium iron manganese phosphate, lithium nickel cobalt manganese oxide, lithium nickel manganese oxide, and lithium cobalt oxide.

[0068] In this embodiment, the use of the above-mentioned specific type of positive electrode active material has the advantage of being more resistant to high voltage and high temperature compared to the use of other types of positive electrode active materials.

[0069] As an example, in the battery negative electrode of the electrode assembly, the negative electrode active material includes at least one of graphite, soft carbon, hard carbon, silicon, silicon oxides and silicon-carbon composites.

[0070] In this embodiment, the technical solution provided in the embodiment of the present application can be applied to the above-mentioned various negative electrode active material systems, providing more feasible implementation schemes, thereby facilitating the promotion and application of the technical solution provided in the embodiment of the present application.

[0071] It should be noted that any structure not specifically described in the battery may be configured according to conventional selections in the art.

[0072] In a third aspect, an embodiment of the present application provides an electrical device, comprising a lithium-ion battery as provided in the embodiment of the second aspect.

[0073] It should be noted that there is no limitation on the types of electrical equipment, such as mobile phones, portable devices, laptops, electric vehicles, electric cars, ships, electric aircraft, spacecraft, electric toys, energy storage devices and electric tools.

[0074] The features and performance of the present application are further described in detail below in conjunction with the embodiments.

[0075] Example 1

[0076] The present invention provides a method for preparing an electrolyte, comprising the following steps:

[0077] Ethylene carbonate (EC), diethyl carbonate (DEC) and methyl trifluoroethyl carbonate (FEMC) were mixed in a mass ratio of 3:4:3 to obtain a mixed organic solvent; then, lithium hexafluorophosphate (LiPF 6 ), lithium tetrakis(2-methyl-8-hydroxyquinoline)borate and compound 1 and mix them evenly to obtain a lithium ion battery electrolyte; wherein, by mass percentage, the mixed organic solvent: lithium hexafluorophosphate: lithium tetrakis(2-methyl-8-hydroxyquinoline)borate: compound 1 = 89.8:10:0.1:0.1.

[0078] The preparation methods of the subsequent embodiments and comparative examples can all refer to Example 1. In order to better understand the differences between the embodiments and comparative examples, they are summarized in Table 1 below.

[0079] Table 1

[0080]

[0081]

[0082]

[0083] Here, “—” means that the component is not contained, and the amount of the organic solvent used is equal to 100 minus the remainder of the sum of the amounts of the remaining components.

[0084] Test Example 1

[0085] Electrical performance test

[0086] Test method:

[0087] The lithium ion battery electrolytes prepared in Examples 1 to 13 and Comparative Examples 1 to 4 were assembled into batteries and numbered accordingly. Then, the initial efficiency at 25°C, the capacity retention rate after 100 cycles at 25°C, the capacity retention rate after 100 cycles at 45°C, and the expansion rate after 15 days of storage at 45°C were tested and statistically reported in Table 2.

[0088] The battery is assembled as follows:

[0089] S1 is mixed with LiNi in a mass ratio of 96:2:2 0.5 Mn 1.5 O 4 (positive electrode active material), conductive carbon black (conductive agent) and polyvinylidene fluoride (binder) are dispersed in N-methyl-2-pyrrolidone to obtain positive electrode slurry; then, the positive electrode slurry is evenly coated on both sides of the aluminum foil; then, after drying, calendering and vacuum drying in sequence, an aluminum lead wire is welded with an ultrasonic welder to obtain a positive electrode sheet with a thickness of 125μm.

[0090] S2 is prepared by mixing graphite (negative electrode active material), conductive carbon black (conductive agent), styrene-butadiene rubber and carboxymethyl cellulose (binder) in a mass ratio of 95:1.5:1.5:2 and dispersing the mixture in deionized water to obtain a negative electrode slurry. The negative electrode slurry is then coated on both sides of a copper foil. The mixture is then dried, rolled and vacuum dried in sequence, and a nickel lead wire is welded on the mixture with an ultrasonic welder to obtain a negative electrode sheet having a thickness of 125 μm.

[0091] S3: The prepared positive electrode sheet, negative electrode sheet and ion separator (PP / PE / PP three-layer composite separator) are wound to obtain a bare battery cell. Then, the bare battery cell and the shell, as well as the high-voltage electrolyte group prepared in Examples 1 to 13 and Comparative Examples 1 to 4 are injected into the dried battery. After packaging, standing, formation, shaping and capacity testing, the battery is assembled.

[0092] The test of the electrical parameters of the battery and the corresponding calculation formula are as follows:

[0093] (1) First efficiency test of the battery:

[0094] The battery that has not been charged and activated after filling is placed at 25℃, and the battery is charged and discharged once using a 0.1C current in the charge and discharge voltage range of 3.5~4.85V, and its charge and discharge capacity is recorded.

[0095] (2) Battery capacity retention test after 100 cycles at 25°C:

[0096] The battery was placed at 25°C, and the battery was charged and discharged in a voltage range of 3.5 to 4.85V using a current of 0.5C, and the discharge retention capacity at the 100th cycle was recorded.

[0097] (3) Battery capacity retention test after 100 cycles at 45°C:

[0098] The battery was placed at 45°C, and the battery was charged and discharged in a voltage range of 3.5 to 4.85V using a current of 0.5C, and the discharge retention capacity at the 100th cycle was recorded.

[0099] (4) Battery expansion rate test at 45°C for 15 days:

[0100] The battery was charged and discharged three times at room temperature (25°C) with a current of 0.33C in the charge and discharge voltage range of 3.5-4.85V, then fully charged with 0.33C, and the thickness of the battery was tested at room temperature (25°C) before high-temperature storage. The battery was then placed at high temperature (45°C) for 15 days, then taken out and placed at room temperature (25°C) for 2h, and the thickness of the battery after high-temperature storage was tested.

[0101] The calculation formula is as follows:

[0102] First efficiency (%) = (first discharge capacity / first charge capacity) × 100%.

[0103] 100-cycle capacity retention rate (%) = (100th discharge retention capacity / 1st cycle discharge capacity) × 100%.

[0104] Expansion rate after storage at 45°C for 15 days (%) = (battery thickness after high-temperature storage - battery thickness before high-temperature storage) / battery thickness before high-temperature storage × 100%.

[0105] Table 2

[0106]

[0107] Referring to Table 2, it can be seen from the test results of Examples 1 to 13 and Comparative Example 1 that the composite additive provided in the embodiments of the present application, compared with the conventional types of additives, the corresponding battery of the former can have better initial efficiency and cycle performance when used under high voltage and high temperature conditions.

[0108] It can be seen from the test results of Example 5 and Example 6 that when the upper limit of the total amount of additives is within a specific range, compared to when it is not within the specific range, the battery corresponding to the former can have both better initial efficiency and cycle performance when used under high voltage and high temperature conditions.

[0109] It can be seen from the test results of Example 7 and Examples 12 to 13 that, on the basis of the electrolyte containing the composite additive provided in the embodiments of the present application, further adding the auxiliary additive provided in the embodiments of the present application can enable the corresponding battery to have better initial efficiency and cycle performance when used under high voltage and high temperature conditions.

[0110] It can be seen from the test results of Example 4 and Comparative Examples 2 to 3 that when the composite additives provided in the embodiments of the present application are used, compared with using only one of them, the battery corresponding to the former can have both better initial efficiency and cycle performance when used under high voltage and high temperature conditions.

[0111] It can be seen from the test results of Example 3 and Comparative Example 4 that when the composite additive provided in the embodiment of the present application is used, compared with replacing additive S with other conventional additives, the battery corresponding to the former can have both better initial efficiency and cycle performance when used under high voltage and high temperature conditions.

[0112] The embodiments described above are part of the embodiments of the present application, rather than all of the embodiments. The detailed description of the embodiments of the present application is not intended to limit the scope of the present application for protection, but merely represents the selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application.

Claims

1. A lithium ion battery electrolyte, characterized in that: The method comprises an organic solvent, a lithium salt and an additive, wherein the additive comprises lithium tetrakis(2-methyl-8-hydroxyquinoline)borate and an additive S, and the structural formula of the additive S is as shown in Formula I: Wherein, R1 and R2 are independently selected from any one of a hydrogen atom, a fluorine atom, a substituted or unsubstituted C1-C3 alkyl group and a substituted silyl group.

2. The lithium ion battery electrolyte according to claim 1, characterized in that: The R1 and R2 are independently selected from any one of a hydrogen atom, a fluorine atom, a methyl group, an ethyl group, a propyl group, a trifluoromethyl group and trimethylsilane.

3. The lithium ion battery electrolyte according to claim 1, characterized in that The mass percentage of the additive in the electrolyte is 0.2-3%.

4. The lithium ion battery electrolyte according to any one of claims 1 to 3, characterized in that The electrolyte further includes an auxiliary additive, which includes at least one of vinyl sulfate, vinyl ethylene carbonate, 1,3-propane sultone, methylene disulfonate, 2-fluoropyridine, allyl isocyanate, triallyl isocyanurate, 2(5H)-furanone, tris(trimethylsilyl)phosphite and tripropylene phosphate.

5. The lithium ion battery electrolyte according to claim 4, characterized in that: The mass percentage of the auxiliary additive in the electrolyte is 0.5-5%.

6. The lithium ion battery electrolyte according to any one of claims 1 to 3, characterized in that The lithium salt comprises at least one of lithium hexafluorophosphate, lithium difluorophosphate, lithium bis(fluorosulfonyl)imide, lithium difluorobis(oxalate)phosphate, lithium tetrafluorooxalatephosphate, lithium difluorooxalatoborate, lithium bis(trifluoromethylsulfonyl)imide and lithium bis(oxalate)borate; Optionally, the mass percentage of the lithium salt in the electrolyte is 10-20%.

7. The lithium ion battery electrolyte according to any one of claims 1 to 3, characterized in that The organic solvent includes at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, dimethyl carbonate, fluoroethylene carbonate, 3,3,3-trifluoropropylene carbonate, methyl trifluoroethyl carbonate and 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether.

8. A lithium ion battery, characterized in that: include: case; an electrode assembly, the electrode assembly being accommodated in the housing; as well as The electrolyte according to any one of claims 1 to 7, wherein the electrolyte is contained in the casing.

9. The lithium-ion battery according to claim 8, characterized in that: In the battery positive electrode of the electrode assembly, the positive electrode active material includes at least one of a transition metal phosphate and a transition metal oxide lithium salt; Optionally, the positive electrode active material includes at least one of lithium iron manganese phosphate, lithium nickel cobalt manganese oxide, lithium nickel manganese oxide and lithium cobalt oxide.

10. The lithium ion battery according to claim 8, characterized in that In the battery negative electrode of the electrode assembly, the negative electrode active material includes at least one of graphite, soft carbon, hard carbon, silicon, silicon oxide and silicon-carbon composite.

11. An electrical device, characterized in that: The invention comprises a lithium ion battery as claimed in any one of claims 8 to 10.

Citation Information

Patent Citations

  • Apparatus for producing solid-state secondary battery and method for producing solid-state secondary battery

    CN113728481A

  • Aromatic phosphine copper complex as well as synthesis method and application thereof

    CN115433213A

  • Electrolyte and lithium ion battery

    CN118572191A

  • Organic electro-luminescence device

    CN1735299A

  • Boron-containing chemicals as cathode additives, si anode additives, electrolyte additives or separator modifiers for li-ion batteries