Lithium supplement modified battery cell diaphragm and preparation method thereof

By using porous organic framework materials and conductive networks on the lithium-ion battery separator, the problems of poor pore size distribution and electrolyte emollience of the lithium-ion battery separator are solved, and the initial coulombic efficiency and cycle life of the battery are significantly improved.

CN119009365AActive Publication Date: 2024-11-22GUOKE ENERGY TECH INNOVATION CENT (HEFEI) CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411204775.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-22
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

The pore size distribution and electrolyte wetting properties of existing lithium-ion battery separators lead to low initial Coulomb efficiency and short cycle life.

Method used

The preparation method of modified cell separator by applying lithium supplement solution to the surface of the cell matrix separator, including the use of 2,4,6-tris(4-aminophenyl)-1,3,5 -triazine, 2,5-dihydroxy-1,4-benzene dicarboxytaldehyde and other raw materials are prepared to prepare porous organic framework materials, and lithium sulfonate groups are grafted thereon to form a rich lithium source to improve lithium ion conductivity , acetylene black and carbon nanotubes are combined as conductive agents to form a conductive network.

Benefits of technology

Effectively adjust the pore size change and electrolyte wetting properties of the separator during charging and discharging, improve the number of lithium ion migration, extend the battery life, and improve the initial Coulomb efficiency and cycle stability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a lithium supplement modified battery cell diaphragm and a preparation method thereof, and relates to the technical field of battery materials. The invention discloses a preparation method of a lithium supplement agent modified battery cell diaphragm, which comprises the following steps: coating a lithium supplement agent solution on the surface of a battery cell matrix diaphragm, and drying to obtain the lithium supplement agent modified battery cell diaphragm, the lithium supplement agent solution is prepared by mixing a lithium supplement agent, a conductive agent, a binder and a solution; the lithium supplement agent layer is coated on the surface of the diaphragm, so that the initial coulombic efficiency and the cycling stability of the battery can be remarkably improved, the service life of the battery is prolonged, and the energy density of the battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery materials, and in particular to a lithium supplement modified battery core diaphragm and a preparation method thereof. Background Art

[0002] Existing lithium-ion batteries are widely used in portable electronic devices, electric vehicles, and energy storage devices, but due to their limited performance such as energy density and cycle life, it is difficult to meet the growing market demand. Polyolefin materials such as polyethylene (PE) and polypropylene (PP) are used as the main materials for lithium battery separators in the early stage of lithium battery research and development because of their excellent properties such as high strength and solution corrosion resistance and low price. However, traditional separators will have problems such as pore size changes and reduced electrolyte wettability during long-term use of the battery, which will affect the cycle life and safety of the battery. Therefore, it is urgent to develop an improved separator material to improve the overall performance of the battery. As one of the key components of the battery, the modified separator plays an important role in improving battery performance. The current separator modification methods mainly focus on the structural optimization of separator materials and surface coating technology.

[0003] The existing lithium-ion battery diaphragms are mainly made of polyethylene (PE) or polypropylene (PP) materials. Although these materials have good chemical stability and mechanical strength, their pore size distribution and electrolyte wettability are poor, which affects the overall performance of the battery. In addition, the prior art has not fully utilized lithium supplements to modify the diaphragms, resulting in limited initial coulombic efficiency and cycle performance of the battery. The present invention proposes a method for preparing a battery cell with a diaphragm modified with a lithium supplement, aiming to solve the problems of low initial coulombic efficiency and short cycle life. Summary of the invention

[0004] The purpose of the present invention is to provide a lithium supplement modified battery cell separator and a preparation method thereof, so as to solve the following technical problems: Existing separators are mainly made of polyethylene or polypropylene materials, which have poor pore size distribution and electrolyte wettability, resulting in low initial coulombic efficiency and short cycle life of the battery.

[0005] The purpose of the present invention can be achieved through the following technical solutions: A method for preparing a lithium supplement agent modified battery cell diaphragm comprises the following steps: applying a lithium supplement agent solution on the surface of a battery cell substrate diaphragm, and drying to obtain a lithium supplement agent modified battery cell diaphragm; The preparation method of the lithium supplement solution comprises the following steps: mixing a lithium supplement, a conductive agent, a binder and a solvent to obtain a lithium supplement solution; The preparation method of the lithium supplement comprises the following steps: S1: In a nitrogen atmosphere, 2,4,6-tris(4-aminophenyl)-1,3,5-triazine, 2,5-dihydroxy-1,4-benzenedicarboxylic acid aldehyde, o-dichlorobenzene and 1,4-dioxane are added to a reaction kettle, and acetic acid solution is added to disperse evenly, the temperature is controlled at 110-130° C., the reaction is kept warm for 48-72 hours, and then washed and dried to obtain component 1; S2: Add lithium tert-butoxide and N,N-dimethylformamide component one into a reaction kettle and disperse them evenly, add 1,3-propane sultone and disperse them evenly, mix component one and N,N-dimethylformamide component two and add them into the reaction kettle and disperse them evenly, control the temperature at 55-65°C, keep the reaction warm for 3-6 hours, wash with acetone, and dry to obtain a lithium supplement.

[0006] As a further embodiment of the present invention: the acetic acid solution in S1 is a 5-8 mol / L acetic acid aqueous solution; the addition ratio of 2,4,6-tris(4-aminophenyl)-1,3,5-triazine, 2,5-dihydroxy-1,4-benzenedicarboxylic acid aldehyde, o-dichlorobenzene, 1,4-dioxane, and acetic acid solution is 1 g: 0.45-1.2 g: 25-100 mL: 25-100 mL: 5-15 mL.

[0007] As a further scheme of the present invention: in S2, N,N-dimethylformamide component one and N,N-dimethylformamide component two are both N,N-dimethylformamide; the addition ratio of lithium tert-butoxide, N,N-dimethylformamide component one, 1,3-propane sultone, component one, and N,N-dimethylformamide component two is 0.05-0.1g:25-50mL:0.1-0.15g:1g:25-50mL.

[0008] As a further solution of the present invention: the coating amount of the lithium supplement solution on the surface of the battery substrate diaphragm is 0.5-2 mg / cm 2 .

[0009] As a further solution of the present invention: the specific step of drying is: drying the battery base diaphragm coated with the lithium supplement solution at 60-100° C. for 12-24 hours.

[0010] As a further solution of the present invention: the binder is polyvinylidene fluoride.

[0011] As a further solution of the present invention: the conductive agent is obtained by mixing acetylene black and carbon nanotubes in a mass ratio of 1:0.25-1.

[0012] As a further solution of the present invention, the mass ratio of lithium supplement agent: conductive agent: binder in the lithium supplement agent solution is 90-95:3-6:2-4.

[0013] As a further embodiment of the present invention: the solvent is any one of N-methylpyrrolidone and ethanol, and the solvent accounts for 2-10% of the total mass of the lithium supplement solution.

[0014] As a further solution of the present invention: the method of coating the lithium supplement agent on the surface of the battery core substrate diaphragm includes a scraper coating method, a transfer coating method, and an electrostatic spinning method.

[0015] As a further solution of the present invention: the battery base separator is made of polyolefin material; the polyolefin material includes polyethylene and polypropylene.

[0016] A lithium supplement modified battery cell diaphragm, prepared by any one of the above preparation methods.

[0017] Beneficial effects of the present invention: (1) The present application uses 2,4,6-tris(4-aminophenyl)-1,3,5-triazine and 2,5-dihydroxy-1,4-benzenedicarboxylic acid aldehyde as raw materials and acetic acid solution as a catalyst to prepare a porous organic framework material having a uniformly high specific surface area, porosity and stability, namely component one; component one can limit the diffusion of molecules with its large pore volume and small window size; the present application further uses component one and 1,3-propane sultone as raw materials, and under the action of a strong nucleophilic reagent, lithium tert-butoxide, the hydroxyl group of component one undergoes an electrophilic reaction, and the hydrogen atom in the hydroxyl group is replaced by a lithium ion. A porous polymer with lithium alcohol groups is generated, and the oxygen anions and lithium cations in the lithium alcohol groups attack the 1,3-propane sultone ring-opening addition between the cations and lithium ions of component one, respectively, and lithium sulfonate groups are grafted onto component one to obtain a lithium supplement. The grafted lithium sulfonate in the pores of the lithium supplement prepared in the present application and the abundant lithium salts in the pores provide abundant lithium sources and improve the lithium ion conductivity. The single-ion polymer electrolyte properties generated by the interaction between the lithium supplement and the anions make it easy for lithium ions to leave, which has a positive effect on increasing the lithium ion migration number and can effectively inhibit the growth of lithium dendrites.

[0018] The lithium supplement agent prepared in the present application is added to the solution to prepare a coating on the surface of the diaphragm, which not only effectively regulates the problems of pore size change and reduced electrolyte wettability of the diaphragm during battery charging and discharging, but also effectively compensates for the initial irreversible lithium loss of the lithium-ion battery and improves the energy density of the battery; the lithium supplement agent can repair the SEI film during the battery cell cycle, and at the same time can significantly improve the initial coulomb efficiency and cycle stability of the battery, extend the battery life, and improve the battery energy density.

[0019] (2) In the present application, acetylene black and carbon nanotubes are used as a conductive agent. The carbon nanotubes achieve micron-scale connections, and the acetylene black fills nanoscale pores. The two work together to form a conductive network, thereby achieving the effect of reducing the internal resistance of the battery. DETAILED DESCRIPTION

[0020] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Example 1 The preparation method of a lithium supplement comprises the following steps: S1: In a nitrogen atmosphere, 1 g of 2,4,6-tris(4-aminophenyl)-1,3,5-triazine, 0.45 g of 2,5-dihydroxy-1,4-benzenedicarboxylic acid aldehyde, 50 mL of o-dichlorobenzene, and 50 mL of 1,4-dioxane were added to a reaction kettle, and 5 mL of a 5 mol / L aqueous acetic acid solution was added to disperse the mixture evenly. The temperature was controlled at 110°C, and the mixture was kept warm for 48 h. The mixture was washed and dried to obtain component 1. S2: Add 0.05 g lithium tert-butoxide and 25 mL N,N-dimethylformamide into a reactor and disperse them evenly, add 0.1 g 1,3-propane sultone and disperse them evenly, mix 1 g component 1 and 25 mL N,N-dimethylformamide and add them into the reactor and disperse them evenly, control the temperature at 55°C, keep the reaction warm for 3 hours, wash with acetone, and dry to obtain a lithium supplement.

[0022] Example 2 The preparation method of the lithium supplement comprises the following steps: S1: In a nitrogen atmosphere, 1 g of 2,4,6-tris(4-aminophenyl)-1,3,5-triazine, 0.8 g of 2,5-dihydroxy-1,4-benzenedicarboxylic acid aldehyde, 50 mL of o-dichlorobenzene, and 50 mL of 1,4-dioxane were added to a reaction kettle, and 10 mL of a 5 mol / L aqueous acetic acid solution was added to disperse the mixture evenly. The temperature was controlled at 120°C, and the mixture was kept warm for 48 h. The mixture was washed and dried to obtain component 1. S2: Add 0.08 g lithium tert-butoxide and 40 mL N,N-dimethylformamide into a reactor and disperse them evenly, add 0.12 g 1,3-propane sultone and disperse them evenly, blend 1 g component 1 and 40 mL N,N-dimethylformamide and add them into the reactor and disperse them evenly, control the temperature at 60°C, keep the reaction warm for 4.5 hours, wash with acetone, and dry to obtain a lithium supplement.

[0023] Example 3 The preparation method of the lithium supplement comprises the following steps: S1: In a nitrogen atmosphere, 1 g of 2,4,6-tris(4-aminophenyl)-1,3,5-triazine, 1.2 g of 2,5-dihydroxy-1,4-benzenedicarboxylic acid aldehyde, 50 mL of o-dichlorobenzene, and 50 mL of 1,4-dioxane were added to a reaction kettle, and 15 mL of a 5 mol / L aqueous acetic acid solution was added to disperse the mixture evenly. The temperature was controlled at 130°C, and the mixture was kept warm for 72 h. The mixture was washed and dried to obtain component 1. S2: Add 0.1 g lithium tert-butoxide and 50 mL N,N-dimethylformamide into a reactor and disperse them evenly, add 0.15 g 1,3-propane sultone and disperse them evenly, mix 1 g component 1 and 50 mL N,N-dimethylformamide and add them into the reactor and disperse them evenly, control the temperature at 65°C, keep the reaction warm for 6 hours, wash with acetone, and dry to obtain a lithium supplement.

[0024] Example 4 A method for preparing a lithium supplement agent modified battery cell separator comprises the following steps: A1: 84.6 g of the lithium supplement agent prepared in Example 1, 1.8 g of acetylene black, 1.08 g of carbon nanotubes, 2.52 g of polyvinylidene fluoride, and 10 g of N-methylpyrrolidone were mixed to obtain a lithium supplement agent solution; A2: Use the doctor blade coating method to apply the lithium supplement solution on the surface of Celgard2400 porous polypropylene separator, with a coating amount of 1 mg / cm 2 , and dried at 80°C for 15h to obtain a lithium supplement agent modified battery cell separator.

[0025] Example 5 A method for preparing a lithium supplement modified battery cell separator comprises the following steps: A1: 84.6 g of the lithium supplement agent prepared in Example 2, 1.8 g of acetylene black, 1.08 g of carbon nanotubes, 2.52 g of polyvinylidene fluoride, and 10 g of N-methylpyrrolidone were mixed to obtain a lithium supplement agent solution; A2: Use the doctor blade coating method to apply the lithium supplement solution on the surface of Celgard2400 porous polypropylene separator, with a coating amount of 1 mg / cm 2 , and dried at 80°C for 15h to obtain a lithium supplement agent modified battery cell separator.

[0026] Example 6 A method for preparing a lithium supplement modified battery cell separator comprises the following steps: A1: 84.6 g of the lithium supplement agent prepared in Example 3, 1.8 g of acetylene black, 1.08 g of carbon nanotubes, 2.52 g of polyvinylidene fluoride, and 10 g of N-methylpyrrolidone were mixed to obtain a lithium supplement agent solution; A2: Use the doctor blade coating method to apply the lithium supplement solution on the surface of Celgard2400 porous polypropylene separator, with a coating amount of 1 mg / cm 2 , and dried at 80°C for 15h to obtain a lithium supplement agent modified battery cell separator.

[0027] Example 7 A method for preparing a lithium ion battery comprises the following steps: B1: Preparation of pole piece: The positive electrode active material is LiFePO4, the conductive agent is acetylene black, and the binder is polytetrafluoroethylene (PTFE). The active material, acetylene black, and PTFE with a mass ratio of 75:20:5 are fully ground, mixed evenly, and anhydrous ethanol is added as a dispersant, pressed into a positive electrode sheet with a thickness of 100um, and then punched into a disc with a diameter of 8mm at 10MPa, and dried in a constant temperature drying oven at 100℃ for 24h. The aluminum sheet is used as the positive electrode current collector to obtain the positive electrode sheet; B2: electrolyte preparation: 1M LiPF6 / EC+DMC; B3: Battery assembly: The battery was assembled in a glove box filled with argon (water content <1 ppm). The metal lithium sheet was used as the auxiliary electrode and the reference electrode (copper sheet current collector). The diaphragm was the lithium supplement modified battery diaphragm prepared in Example 4. After assembly in the mold, the mold was sealed and allowed to stand at room temperature for 10 h. The battery was obtained.

[0028] Embodiment 8 The preparation method of lithium ion battery comprises the following steps: B1: Preparation of pole piece: The positive electrode active material is LiFePO4, the conductive agent is acetylene black, and the binder is polytetrafluoroethylene (PTFE). The active material, acetylene black, and PTFE with a mass ratio of 75:20:5 are fully ground, mixed evenly, and anhydrous ethanol is added as a dispersant, pressed into a positive electrode sheet with a thickness of 100um, and then punched into a disc with a diameter of 8mm at 10MPa, and dried in a constant temperature drying oven at 100℃ for 24h. The aluminum sheet is used as the positive electrode current collector to obtain the positive electrode sheet; B2: electrolyte preparation: 1M LiPF6 / EC+DMC; B3: Battery assembly: This was carried out in a glove box filled with argon (water content <1ppm), with the metal lithium sheet used as the auxiliary electrode and reference electrode (copper sheet current collector), and the diaphragm used the lithium supplement modified battery diaphragm prepared in Example 5. After assembly in the mold, the mold was sealed and allowed to stand at room temperature for 10 hours to obtain a battery.

[0029] Embodiment 9 The preparation method of lithium ion battery comprises the following steps: B1: Preparation of pole piece: The positive electrode active material is LiFePO4, the conductive agent is acetylene black, and the binder is polytetrafluoroethylene (PTFE). The active material, acetylene black, and PTFE with a mass ratio of 75:20:5 are fully ground, mixed evenly, and anhydrous ethanol is added as a dispersant, pressed into a positive electrode sheet with a thickness of 100um, and then punched into a disc with a diameter of 8mm at 10MPa, and dried in a constant temperature drying oven at 100℃ for 24h. The aluminum sheet is used as the positive electrode current collector to obtain the positive electrode sheet; B2: electrolyte preparation: 1M LiPF6 / EC+DMC; B3: Battery assembly: The battery was assembled in a glove box filled with argon (water content <1 ppm). The metal lithium sheet was used as the auxiliary electrode and the reference electrode (copper sheet current collector). The diaphragm was the lithium supplement modified battery diaphragm prepared in Example 6. After the assembly was completed in the mold, the mold was sealed and allowed to stand at room temperature for 10 hours. The battery was obtained.

[0030] Comparative Example 1 A method for preparing a lithium ion battery comprises the following steps: B1: Preparation of pole piece: The positive electrode active material is LiFePO4, the conductive agent is acetylene black, and the binder is polytetrafluoroethylene (PTFE). The active material, acetylene black, and PTFE with a mass ratio of 75:20:5 are fully ground, mixed evenly, and anhydrous ethanol is added as a dispersant, pressed into a positive electrode sheet with a thickness of 100um, and then punched into a disc with a diameter of 8mm at 10MPa, and dried in a constant temperature drying oven at 100℃ for 24h. The aluminum sheet is used as the positive electrode current collector to obtain the positive electrode sheet; B2: electrolyte preparation: 1M LiPF6 / EC+DMC; B3: Battery assembly: carried out in a glove box filled with argon (moisture <1ppm), with metal lithium sheets as auxiliary electrodes and reference electrodes (copper sheet current collector), and Celgard2400 porous polypropylene membrane as the diaphragm. After assembly in the mold, seal it and let it stand at room temperature for 10 hours; obtain the battery sample.

[0031] Comparative Example 2 The preparation method of the lithium supplement comprises the following steps: S1: In a nitrogen atmosphere, 1 g of 2,4,6-tris(4-aminophenyl)-1,3,5-triazine, 0.45 g of 2,5-dihydroxy-1,4-benzenedicarboxylic acid aldehyde, 50 mL of o-dichlorobenzene, and 50 mL of 1,4-dioxane were added to a reaction kettle, and 5 mL of a 5 mol / L aqueous acetic acid solution was added to disperse the mixture evenly. The temperature was controlled at 110°C, and the mixture was kept warm for 48 h. The mixture was washed and dried to obtain component 1. S2: 0.1 g of lithium methanesulfonate and 1 g of component 1 are mixed to obtain a lithium supplement.

[0032] Comparative Example 3 Compared with Example 5, Comparative Example 3 is only that the lithium supplement agent prepared in Example 2 added in Example 5 is replaced by the lithium supplement agent prepared in Comparative Example 2 in an equal amount, and the other components and preparation method are completely the same as those in Example 5.

[0033] Comparative Example 4 Compared with Example 8, Comparative Example 4 only replaces the lithium supplement agent modified battery cell separator prepared in Example 5 used in Example 8 with the lithium supplement agent modified battery cell separator prepared in Comparative Example 3, and the other components and preparation methods are completely consistent with Example 8.

[0034] Comparative Example 5 Compared with Example 5, Comparative Example 5 is only that the lithium supplement prepared in Example 2 added in Example 5 is replaced by lithium methanesulfonate in equal amount, and the other components and preparation method are completely the same as those in Example 5.

[0035] Comparative Example 6 Compared with Example 8, Comparative Example 6 only replaces the lithium supplement agent modified battery cell separator prepared in Example 5 used in Example 8 with the lithium supplement agent modified battery cell separator prepared in Comparative Example 5, and the other components and preparation methods are completely consistent with Example 8.

[0036] Performance Testing (1) Electrochemical performance ① Electrochemical stability window: Linear sweep voltammetry was used to test the electrochemical stability window of the material using a CHI electrochemical workstation; a stainless steel sheet was used as the working electrode, and a lithium sheet was used as the auxiliary electrode to assemble a semi-blocked cell (stainless steel sheet / diaphragm (immersed in electrolyte) / stainless steel sheet), and the working parameters were: scan rate of 0.002 V / s, sampling interval of 0.001 V; the test results are shown in Table 1; ② Ionic conductivity: The electrochemical impedance spectroscopy method was used to test the M2273 electrochemical workstation. First, a semi-blocked cell (stainless steel sheet / diaphragm (immersed in electrolyte) / stainless steel sheet) was assembled. The working parameters were: ambient temperature 20°C, sinusoidal amplitude 5mV, scanning frequency 0.1-10 4 Hz, and the impedance spectrum is obtained. The intersection point of the straight line and the real axis in the impedance spectrum is recorded as the bulk resistance Rb, and the ionic conductivity σ is calculated according to the following formula; σ=d / (Rb·S) Where, σ-ionic conductivity, s / cm; d-film thickness, cm; Rb-film bulk resistance, Ω; S-film area, cm 2 ; The calculation results are shown in Table 1; ③ Lithium ion migration number: The AC impedance method and steady-state current were used to test using an M2273 electrochemical workstation. First, a semi-blocked battery (stainless steel sheet / diaphragm (immersed in electrolyte) / stainless steel sheet) was assembled. The working parameters were: polarization potential 10mV, test time 3000s. From the obtained polarization current curve, the initial current I0 and the polarization steady-state current value I s ; respectively in 0.1-10 4 In the Hz frequency range, the AC impedance test is performed on the material before and after polarization to obtain the AC impedance curve, and the initial resistance R0 and the polarization steady-state resistance R ss ; and calculate the lithium ion migration number t according to the following formula Li+ : t Li+ =[I s (V-I0R0)] / [I0(VI s Rss )] Where, t Li+ -Lithium ion migration number; I0-initial state current, A; I s - steady-state current, A; V-polarization voltage, V; R0-initial state resistance, Ω; R ss Steady-state resistance, Ω; the test results are shown in Table 1; Table 1: Electrochemical impedance spectroscopy data statistics

[0037] It can be seen from Table 1 that the diaphragm prepared in the present application has a higher liquid absorption rate and porosity than the existing Celgard2400 porous polypropylene diaphragm, which increases its conductivity; the lithium ion migration number of the diaphragm prepared in the present application is close to 1, which is better than the traditional Celgard2400 porous polypropylene diaphragm.

[0038] (2) Charge and discharge test: At room temperature, the battery was cycled using the LAND CT-2001A battery test system; the charge and discharge voltage range was 2.8-4.2V (vs Li / Li+), and the current density was 1.4mA / cm 2 ; The battery capacity retention rate was tested by charging and discharging at a charge and discharge rate of 0.5C for 500 cycles; the test results are shown in Table 2; Table 2: Statistical table of performance test data of Examples 7-9 and Comparative Examples 1, 4 and 6

[0039] As can be seen from Table 2, the present application coats a lithium replenisher containing lithium elements on the surface of the diaphragm, which effectively compensates for the initial irreversible lithium loss of the lithium-ion battery, improves the energy density of the battery, and significantly improves the battery energy density and cycle stability of the battery, thereby extending the battery life.

[0040] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.

Claims

1. A method for preparing a lithium supplement modified battery cell diaphragm, characterized in that: The method comprises the following steps: applying a lithium supplement agent solution on the surface of a battery cell substrate diaphragm and drying the solution to obtain a lithium supplement agent modified battery cell diaphragm; The preparation method of the lithium supplement solution comprises the following steps: mixing a lithium supplement, a conductive agent, a binder and a solvent to obtain a lithium supplement solution; The preparation method of the lithium supplement comprises the following steps: S1: In a nitrogen atmosphere, 2,4,6-tris(4-aminophenyl)-1,3,5-triazine, 2,5-dihydroxy-1,4-benzenedicarboxylic acid aldehyde, o-dichlorobenzene and 1,4-dioxane are added to a reaction kettle, and acetic acid solution is added to disperse evenly, the temperature is controlled at 110-130° C., the reaction is kept warm for 48-72 hours, and then washed and dried to obtain component 1; S2: Add lithium tert-butoxide and N,N-dimethylformamide component one into a reaction kettle and disperse them evenly, add 1,3-propane sultone and disperse them evenly, mix component one and N,N-dimethylformamide component two and add them into the reaction kettle and disperse them evenly, control the temperature at 55-65°C, keep the reaction warm for 3-6 hours, wash with acetone, and dry to obtain a lithium supplement.

2. The method for preparing a lithium supplement modified battery cell diaphragm according to claim 1, characterized in that: The acetic acid solution in S1 is a 5-8 mol / L acetic acid aqueous solution; the addition ratio of 2,4,6-tris(4-aminophenyl)-1,3,5-triazine, 2,5-dihydroxy-1,4-benzenedicarboxylic acid aldehyde, o-dichlorobenzene, 1,4-dioxane, and acetic acid solution is 1 g: 0.45-1.2 g: 25-100 mL: 25-100 mL: 5-15 mL.

3. The method for preparing a lithium supplement modified battery cell diaphragm according to claim 1, characterized in that: In S2, N,N-dimethylformamide component one and N,N-dimethylformamide component two are both N,N-dimethylformamide; the addition ratio of lithium tert-butoxide, N,N-dimethylformamide component one, 1,3-propane sultone, component one, and N,N-dimethylformamide component two is 0.05-0.1g:25-50mL:0.1-0.15g:1g:25-50mL.

4. The method for preparing a lithium supplement modified battery cell diaphragm according to claim 1, characterized in that: The coating amount of lithium supplement solution on the surface of the battery substrate diaphragm is 0.5-2mg / cm 2 .

5. The method for preparing a lithium supplement modified battery cell diaphragm according to claim 1, characterized in that: The specific steps of drying are: drying the battery base diaphragm coated with the lithium supplement solution at 60-100° C. for 12-24 hours.

6. The method for preparing a lithium supplement modified battery cell diaphragm according to claim 1, characterized in that: The binder is polyvinylidene fluoride.

7. The method for preparing a lithium supplement modified battery cell diaphragm according to claim 1, characterized in that: The conductive agent is obtained by mixing acetylene black and carbon nanotubes in a mass ratio of 1:0.25-1.

8. The method for preparing a lithium supplement modified battery cell diaphragm according to claim 1, characterized in that: The mass ratio of lithium supplement agent: conductive agent: binder in the lithium supplement agent solution is 90-95:3-6:2-4.

9. The method for preparing a lithium supplement modified battery cell diaphragm according to claim 1, characterized in that: The solvent is any one of N-methylpyrrolidone and ethanol, and the solvent accounts for 2-10% of the total mass of the lithium supplement solution.

10. A lithium supplement modified battery cell diaphragm, characterized in that: Prepared by the preparation method described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method for supplementing lithium to lithium ion battery pole piece

    CN106410120A

  • Nondestructive lithium-supplementing composite diaphragm as well as preparation method and application thereof

    CN114552125A

  • Method for supplementing lithium for diaphragm and stabilizing lithiation layer

    CN116826303A

  • Preparation method of lithium supplement battery, lithium supplement battery and electronic equipment

    CN117117332A

  • Lithium-ion battery based on in-situ negative-electrode lithium supplementation, and preparation method therefor

    WO2024109853A1