Method for constructing BN heat conduction path metal-based liquid crystal epoxy copper-clad plate through silk-screen printing and application of metal-based liquid crystal epoxy copper-clad plate
The method of constructing patterned thermal conductivity paths and using liquid crystal epoxy resin binder through screen printing, the problem of complicated preparation of high-content BN composite materials and thermal resistance of thermal insulation layer is solved, and high thermal conductivity and good electrical breakdown strength are achieved. Metal-based liquid crystal epoxy copper clad plate meets the heat dissipation needs of electronic equipment.
Patent Information
- Application Number
- CN202411091351.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-22
AI Technical Summary
The method of constructing three-dimensional thermal conductivity paths in the prior art is complicated and difficult to achieve large-scale production. There is also a thermal resistance problem at the interface between the thermal insulation layer and the copper foil and the metal substrate.
A patterned thermal conductivity path is constructed on the surface of metal substrates and copper foil by screen printing, chemically modified hexagonal boron nitride as the thermal filler, and liquid crystal epoxy resin as the binder, through screen printing and hot pressing technology Metal-based liquid crystal epoxy copper clad plate with high thermal conductivity was prepared.
It achieves efficient thermal conductivity improvement, while maintaining good electrical breakdown strength and peel resistance, meeting the demand for heat dissipation of electronic equipment.
Smart Images

Figure CN119012528A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of heat dissipation of electronic circuit boards, and specifically relates to a method for constructing a metal-based liquid crystal epoxy copper-clad laminate with a BN thermal conductive path by screen printing and an application thereof. Background Art
[0002] Epoxy resin has excellent electrical insulation, mechanical strength and high temperature resistance, and is often used as the base of the thermal insulation layer of traditional copper clad laminates. The corresponding copper clad laminates are widely used in various electronic products. However, general epoxy resin-based copper clad laminates cannot meet the heat dissipation requirements of high frequency, miniaturization and integration in the electronics industry. For example, the thermal conductivity of FR-4 is only 0.2W·m -1 ·K -1 In order to improve the thermal conductivity of copper clad laminates, high thermal conductivity inorganic fillers can be added to the resin matrix on the one hand, and the intrinsic thermal conductivity of the resin matrix can be improved by introducing liquid crystal primitives on the other hand. Compared with ordinary epoxy resins, liquid crystal epoxy introduces microscopic orderly arranged structural units in the curing network, thereby improving the regularity of the molecular chain, suppressing uncoordinated molecular vibrations, and then reducing phonon scattering, and ultimately improving the overall thermal conductivity of the material.
[0003] Hexagonal boron nitride (h-BN) is a thermally conductive inorganic filler with high thermal conductivity, good thermal stability and chemical stability, and is often used to prepare the thermal insulation layer of copper-clad laminates. However, when the content of the thermally conductive filler is low, a continuous thermal conductive path cannot be formed due to the polymer barrier between the fillers, and the thermal conductivity of the polymer insulation layer cannot be effectively improved. Only when the addition amount of the thermally conductive filler reaches more than 50%, can a local continuous BN thermal conductive path be constructed in the epoxy resin matrix, thereby significantly improving the thermal conductivity of the composite material, but a high content of filler will greatly reduce the mechanical and bonding properties of the composite material. In order to solve this problem, a high-content BN composite material is often used to construct a three-dimensional structure of the thermal conductive path (such as the ice crystal template method), and then the epoxy resin is used to fix the thermal conductive path, but this preparation method is cumbersome and difficult to achieve large-scale production. In addition, the interface between the metal substrate and the polymer has an important influence on heat conduction and interface bonding. The better the epoxy resin interacts with the metal substrate, that is, the more perfect the thermal resistance layer is, the less conducive to heat conduction. On the contrary, if inorganic particles are in contact with the metal surface, it is beneficial to heat conduction but not conducive to interface bonding. Therefore, it is necessary to develop a new method for preparing thermally conductive copper-clad laminates to solve the above-mentioned difficulties in large-scale preparation of thermal conductive paths and the thermal resistance problem at the interface between the thermally conductive insulating layer and the copper foil and the metal substrate. Summary of the invention
[0004] In order to overcome the problems of the traditional method of constructing a three-dimensional heat conduction path with a high-content BN composite material, which is cumbersome, inefficient, and cannot be mass-produced, as well as the thermal resistance problem at the interface between the heat-conducting insulating layer and the copper foil and the metal substrate, the present invention provides a method for constructing a patterned heat conduction path inside an epoxy copper-clad laminate, using chemically modified micron hexagonal boron nitride as a patterned and matrix heat-conducting filler, and using liquid crystal epoxy resin as a binder. First, a patterned out-of-plane heat conduction path and an in-plane heat conduction matrix are prepared on the surface of a metal substrate and copper foil by a screen printing method, and then the metal substrate printed with a heat-conducting insulating layer and the printed surface of the copper foil are overlapped and hot-pressed to prepare a liquid crystal epoxy heat-conducting copper-clad laminate. The copper-clad laminate not only has a high thermal conductivity, but also has good electrical breakdown strength and anti-peeling performance.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] A first aspect of the present invention provides a method for constructing a metal-based liquid crystal epoxy copper-clad laminate with a BN thermal conductive path by screen printing, the method comprising the following steps:
[0007] S1. First, hexagonal boron nitride is modified with a surfactant, and then a liquid crystal epoxy monomer, a curing agent and a surface-modified boron nitride are dissolved in an organic solvent to prepare a high-boron nitride content coating liquid and a low-boron nitride content coating liquid, wherein the mass ratio of hexagonal boron nitride to the liquid crystal epoxy monomer is 3-4:2-1 in the high-boron nitride content coating liquid, and the mass ratio of hexagonal boron nitride to the liquid crystal epoxy monomer is 1-3:7-9 in the low-boron nitride content coating liquid;
[0008] S2, firstly, using a screen printing method to print a low-boron nitride content coating liquid on the surface of the copper foil and the aluminum plate to form a patterned thermal conductive matrix, and then using a screen printing method to fill the gaps of the patterned matrix on the surface of the substrate with a high-boron nitride content coating liquid to construct a patterned thermal conductive path, and then printing a patterned thermal conductive insulating layer on the surface of the copper foil and the aluminum plate;
[0009] S3. Overlap two copper foils and aluminum plates printed with patterned thermally conductive insulating layers and perform hot pressing to prepare a metal-based thermally conductive copper-clad laminate, wherein a coating liquid with a high boron nitride content constitutes an out-of-plane thermal conductive path and cooperates with a coating liquid with a low boron nitride content to construct an in-plane thermal conductive path.
[0010] Preferably, S2 is specifically as follows: placing a silk screen having a mask pattern above a copper foil or an aluminum plate, leaving gaps in the pattern, and then silk screen printing a coating liquid with a low boron nitride content on its surface. After drying, the mask is removed to form an in-plane thermal conductive substrate of the insulating layer. Another silk screen having a pattern matching that of the substrate is used to print a coating liquid with a high boron nitride content on the surface of the copper foil or aluminum plate to fill the gaps left by the previous printing. After drying, the mask is removed to form a patterned out-of-plane thermal conductive path.
[0011] On the one hand, the present invention adopts the method of screen printing to print a low-content BN / liquid crystal epoxy composite material thermal conductive matrix and a high-content BN / liquid crystal epoxy composite material patterned thermal conductive path on the surface of the metal substrate. The slurry in the screen printing process can achieve a certain degree of orientation through the mesh under pressure, which is conducive to the improvement of out-of-plane thermal conductivity. At the same time, the present invention first prints a patterned matrix, and then fills the gaps between the matrix patterns with a high-content BN / liquid crystal epoxy slurry, forcing the boron nitride filler to flow and orient along the out-of-plane direction, so that the out-of-plane orientation of the screen-printed insulating layer is 2-4 times higher than that of the ordinary blended sample. Because the boron nitride sheet belongs to anisotropic thermal conductive materials, the improvement of the out-of-plane orientation means that boron nitride can form a more effective out-of-plane thermal conductive path.
[0012] On the other hand, the present invention uses liquid crystal epoxy resin as an adhesive, first uses a relatively low content of modified hexagonal boron nitride as a filler, and uses a prefabricated mask screen to print a heat-conducting matrix on a metal surface, leaving a dot-shaped, linear or grid pattern gap. Then, a liquid crystal epoxy mixed solution with a high content of modified hexagonal boron nitride is printed on its surface to form a heat-conducting concentration point constructed by a high content of boron nitride, and the two cooperate to prepare a complete insulating layer. Finally, the two printed surfaces are superimposed and hot-pressed to obtain a metal-based liquid crystal epoxy thermally conductive copper-clad laminate. Among them, the ordered structure of the liquid crystal state ensures that the resin matrix has a high thermal conductivity, which is beneficial to reducing the interfacial thermal resistance between BN fillers, improving the thermal conductivity efficiency of the high-content BN / liquid crystal epoxy thermal conductive path, and synergizing with the low-content BN / liquid crystal epoxy thermal conductive matrix to form a thermally conductive network throughout the entire insulating layer, thereby significantly improving the thermal conductivity of the copper-clad laminate with a relatively low BN filling amount, and is beneficial to improving the peel strength and breakdown strength, showing the unique advantages of the patterned insulating layer. The study found that when the total BN content was 26.36wt%, the dot patterned insulation layer copper clad laminate exhibited excellent in-plane and out-of-plane thermal conductivity (20.48 and 11.48W / m·K), which is about 10 times the in-plane and out-of-plane thermal conductivity of the blend with similar BN content, and had higher peel strength (2.08N / mm) and breakdown strength (52.4kV / mm). When the BN content reached 48%, the in-plane and out-of-plane thermal conductivity of the grid pattern insulation layer copper clad laminate was better (36.13 and 25.78W / m·K), almost twice that of the dot pattern insulation layer copper clad laminate, but the peel strength and breakdown strength also decreased by about half. In general, the various properties of the patterned insulation layer copper clad laminate samples are higher than those of the blended composite insulation layer copper clad laminate samples with the same boron nitride content, and these performance indicators are also far higher than the thermal conductivity of other currently known boron nitride filler insulation layers.
[0013] In addition, the screen printing method is used to construct a boron nitride filled liquid crystal epoxy patterned composite thermal conductive insulation layer, which can enhance the orientation of BN and improve the thermal conductivity of the patterned part. The patterned thermal conductive path with high BN content has a high thermal conductivity efficiency and can be conducted through the area to the nearby matrix area with low filler content, thereby improving the overall in-plane and out-plane thermal conductivity of the insulation layer and achieving the effect of saving fillers. Moreover, liquid crystal epoxy has an ordered structure and fluidity at high temperatures, as well as the characteristics of oriented arrangement of the ordered structure under pressure, which is conducive to reducing the thermal resistance between fillers and ensuring the continuity of the thermal conductive path inside and outside the insulation layer.
[0014] Preferably, the liquid crystal epoxy monomer in S1 includes at least one of an aromatic imine type liquid crystal epoxy monomer, an aromatic ester type liquid crystal epoxy monomer, and a biphenyl type liquid crystal epoxy monomer.
[0015] The aromatic imine type liquid crystal epoxy monomer includes but is not limited to one or more of 4-[[4-(oxiranylmethoxy)phenyl]imino]methyl-benzoic acid 1,4-butanediyl ester, 4',4'-bis(4-hydroxybenzylidene)-diaminophenylene diglycidyl ether, p-terephthalylidene-bis-(4-aminophenol) diglycidyl ether, p-terephthalylidene-bis-(4-amino-3-methylphenol) diglycidyl ether, 4-(2-oxiranylmethoxy)-benzaldehyde 2-((4-(2-oxiranylmethoxy)phenyl)methylene)hydrazone, and 4-(2-oxiranylmethoxy)-N-((4-(2-oxiranylmethoxy)phenyl)methylene)aniline.
[0016] The chemical structure of the 4-[[4-(oxiranylmethoxy)phenyl]imino]methyl-benzoic acid 1,4-butanediyl ester is:
[0017]
[0018] The chemical structural formula of the 4',4'-bis(4-hydroxybenzylidene)-diaminophenylene diglycidyl ether is:
[0019]
[0020] The chemical structure of the p-terephthalylidene-bis-(4-aminophenol) diglycidyl ether is:
[0021]
[0022] The chemical structure of the p-terephthalylidene-bis-(4-amino-3-methylphenol) diglycidyl ether is:
[0023]
[0024] The chemical structure of the 4-(2-oxiranylmethoxy)-benzaldehyde 2-((4-(2-oxiranylmethoxy)phenyl)methylene)hydrazone is:
[0025]
[0026] The chemical structure of the 4-(2-oxiranylmethoxy)-N-((4-(2-oxiranylmethoxy)phenyl)methylene)aniline is:
[0027]
[0028] The aromatic ester liquid crystal epoxy monomers include but are not limited to 4-(oxiranylmethoxy)-benzoic acid 1,4-butanediylbis(oxy-4,1-phenylene) ester, 4-(9-oxiranylnonyloxy)benzoic acid 1,4-phenylene ester, 4-(10,11-epoxyundecenyloxy)phenyl-4-[(10,11-epoxyundecenyloxy)benzyloxy]benzoate, 1,1'-(1,4-phenylene)bis[4-(2-oxiranylmethoxy)benzoate]
[0029] The chemical structure of the 4-(oxiranylmethoxy)-benzoic acid 1,4-butanediylbis(oxy-4,1-phenylene)ester is:
[0030]
[0031] The chemical structure of the 4-(9-oxiranylnonyloxy)benzoic acid 1,4-phenyl ester is:
[0032]
[0033] The chemical structure of the 4-(10,11-epoxyundecenyloxy)phenyl-4-[(10,11-epoxyundecenyloxy)benzyloxy]benzoate is:
[0034]
[0035] The chemical structure of the 1,1'-(1,4-phenylene)bis[4-(2-oxiranylmethoxy)benzoate] is:
[0036]
[0037] The biphenyl type liquid crystal epoxy monomers include but are not limited to 2,2'-[1,2-ethanediylbis(oxy-2,1-ethanediyloxy[1,1'-biphenyl]-4',4-diyloxymethylene)]bis-oxirane, 4'-(2-oxirane methyloxy)-[1,1'-biphenyl]-4-carboxylic acid 4,4'-(1,4-butanediyl) ester, 4,4'-biphenyl bisphenol diglycidyl ether, 3,3'5,5'-tetramethylbiphenyl bisphenol diglycidyl ether
[0038] The chemical structure of the 2,2'-[1,2-ethanediylbis(oxy-2,1-ethanediyloxy[1,1'-biphenyl]-4',4-diyloxymethylene)]bis-ethylene oxide is:
[0039]
[0040] The chemical structure of the 4'-(2-oxiranylmethoxy)-[1,1'-biphenyl]-4-carboxylic acid 4,4'-(1,4-butanediyl) ester is:
[0041]
[0042] The chemical structure of the 4,4'-biphenyl bisphenol diglycidyl ether is:
[0043]
[0044] The chemical structure of the 3,3'5,5'-tetramethylbiphenyl bisphenol diglycidyl ether is:
[0045]
[0046] More preferably, the preparation method of the 4-[[4-(oxiranylmethoxy)phenyl]imino]methyl-benzoic acid 1,4-butanediyl ester liquid crystal epoxy monomer comprises the following steps:
[0047] (1) dibromobutane, 4-carboxybenzaldehyde and potassium carbonate are dissolved in N,N-dimethylformamide in a molar ratio of 1-2:1-3:5-7, heated to 70-90°C under the protection of inert gas for reaction for 4-6 hours, filtered to obtain a clear filtrate after reaction, the filtrate is concentrated and slowly dripped into ice water, stirred continuously, and the pH of the solution is adjusted to acidic, filtered to obtain a white solid, washed with water, and dried to obtain product A; (2) the white solid A of step (1) and p-aminophenol are dissolved in methanol in a molar ratio of 1-2:2-3, reacted at 80-100°C for 5-8 hours under the protection of inert gas, cooled to room temperature after reaction, filtered, washed and dried to obtain product B. (3) A large amount of epichlorohydrin and product B are mixed and heated to 90-110° C., and then benzyltrimethylammonium chloride is added in a molar ratio of product B: benzyltriethylammonium chloride = 1-1: 0.05-0.08. After the reaction system is refluxed at this temperature for 80-100 minutes, sodium hydroxide is added in batches within 1-3 hours in an amount twice the molar ratio of product B, and the water is removed. The reaction system is cooled and filtered, and the obtained solid is washed with ether. The solid is then dispersed in a 7-15% mass fraction sodium hydroxide aqueous solution, and an appropriate amount of xylene is added to improve the solubility. Thereafter, the solid is refluxed at 80-100° C. for 1-2 hours. After the reaction, the liquid crystal epoxy monomer of 4-[[4-(oxiranylmethoxy)phenyl]imino]methyl-benzoic acid 1,4-butanediyl ester is obtained by drying.
[0048] More preferably, the preparation method of the 1,1'-(1,4-phenylene)bis[4-(2-oxiranylmethoxy)benzoate] liquid crystal epoxy monomer comprises the following steps:
[0049] (1) Add p-hydroxybenzoic acid (0.3 mol) and methanol (200 ml) to a three-necked flask in sequence, place it in an oil bath and heat it to 80°C, dissolve potassium hydroxide (1 mol) in 65 ml of water and slowly drop it into the three-necked flask, stir for 30 min, then slowly drop allyl bromide (0.35 mol) into the three-necked flask, stir and reflux for 8 h. Cool to room temperature, filter to remove potassium bromide, and remove the solvent methanol by rotary evaporation. Add 1.25 L of deionized water and 300 ml of cyclohexane to the remaining solid in sequence, pour it into a separatory funnel and let it stand to separate, the lower layer is the aqueous phase. Heat the aqueous phase to 40°C and neutralize it with hydrochloric acid solution to neutrality. Filter and collect the white solid, wash it with water 3 times, and finally recrystallize it with ethanol, place it in a vacuum oven at 60°C and dry it for 24 h to obtain the pre-product 1. (2) Add pre-product 1 (0.1 mol), dimethylformamide (3 drops), and sulfoxide chloride (0.5 mol) to a three-necked flask in sequence, place in an oil bath and heat to 80°C, and stir to react for 4 hours. Remove excess sulfoxide chloride by vacuum filtration, cool to room temperature, add 60 ml of pyridine, and place in an ice bath. Dissolve hydroquinone (0.055 mol) in 40 ml of pyridine, slowly dropwise add to the three-necked flask, react in an ice bath for 4 hours, and react at room temperature for 20 hours. After the reaction is completed, add water to precipitate solids, wash the solids with 10% HCl aqueous solution, 10% sodium carbonate aqueous solution, and water in sequence, and finally recrystallize with ethyl acetate, place in a vacuum oven at 60°C and dry for 24 hours to obtain pre-product 2. (3) Add pre-product 2 (0.03 mol), m-chloroperbenzoic acid (0.3 mol), and dichloromethane (400 ml) to a three-necked flask in sequence, place in an oil bath and heat to 50°C, and stir to react for 48 hours. Cool to room temperature, add 0.3 mol sodium sulfite aqueous solution and 0.3 mol sodium bicarbonate aqueous solution in sequence, pour into a separatory funnel and let stand for stratification, the lower layer is the dichloromethane layer. The dichloromethane layer is rotary evaporated to remove dichloromethane, the solid is washed with water and methanol three times in sequence, and finally recrystallized with ethyl acetate, placed in a vacuum oven at 60°C and dried for 24 hours to obtain the final product 1,1'-(1,4-phenylene)bis[4-(2-oxiranylmethoxy)benzoate]
[0050] More preferably, the preparation method of the 4'-(2-oxiranylmethoxy)-[1,1'-biphenyl]-4-carboxylic acid 4,4'-(1,4-butanediyl) ester liquid crystal epoxy monomer comprises the following steps:
[0051] (1) dissolving 4'-hydroxybiphenyl-4-carboxylic acid in methanol, then dropping sulfuric acid, and then heating and refluxing for 5-7h. After the reaction, remove methanol, wash the obtained solid with water until it is neutral, and dry it to obtain product A; (2) mixing product A of step (1) with 1,4-butanediol and calcium acetate hydrate, heating to 170-190°C and refluxing for 1-3 hours, after the reaction is completed and cooled, methanol is added to collect the product, and the obtained solid is filtered and dried to obtain product B; (3) mixing a large amount of epichlorohydrin and product B, and heating to 90-110°C, and then mixing according to the molar ratio of product B: benzyltriethylammonium chloride = 1-2: 0.05-0.08 Benzyltrimethylammonium chloride is added in batches, and then the reaction system is refluxed at this temperature for 80-100 minutes. After the reaction, sodium hydroxide is added in batches within 1-3 hours. After removing the water, the obtained mixed solution is filtered to obtain a solid, and then the solid is washed with ether. The solid is then dispersed in a 7-15% mass fraction sodium hydroxide aqueous solution, and an appropriate amount of xylene is added to improve the solubility. Thereafter, the solid is refluxed at 80-100° C. for 1-2 hours to remove residual hydrogen chloride. After the reaction, the solid is filtered and washed with ethanol, and finally dried to obtain a 4'-(2-oxiranylmethoxy)-[1,1'-biphenyl]-4-carboxylic acid 4,4'-(1,4-butanediyl) ester liquid crystal epoxy monomer.
[0052] Preferably, the surfactant in S1 includes at least one of 3-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane and urea.
[0053] More preferably, the 3-aminopropyltriethoxysilane or γ-glycidyloxypropyltrimethoxysilane modified hexagonal boron nitride (BN) comprises the following steps:
[0054] (1) dissolving boron nitride powder in a sodium hydroxide aqueous solution, refluxing at 110-130°C for 20-30h, filtering after reaction, washing and drying to obtain BN powder with surface hydroxyl activated; (2) hydrolyzing ethanol and 3-aminopropyltriethoxysilane or γ-glycidyloxypropyltrimethoxysilane for 25-40min, adding toluene to a mixture of toluene and activated BN powder, refluxing at 100-120°C for 7-15h, filtering after reaction, washing and drying to obtain 3-aminopropyltriethoxysilane or γ-glycidyloxypropyltrimethoxysilane modified hexagonal boron nitride.
[0055] More preferably, the urea-modified hexagonal boron nitride is prepared by ball-milling boron nitride and urea at a weight ratio of 1:15-25 at a speed of 500-2000 rpm for 15-30h, dissolving the obtained powder in water, and removing urea by dialysis for 5-10 weeks, followed by filtration and drying to obtain urea-modified hexagonal boron nitride powder.
[0056] Preferably, the curing agent in S1 includes at least one of 1-benzyl-2-methylimidazole, 2-heptadecylimidazole, and 2,4-diamino-6-(2-undecylimidazole-1-ethyl)-S-triazine.
[0057] Preferably, the organic solvent in S1 can be any low-boiling point polar solvent, including at least one of acetone, ethanol, tetrahydrofuran, dichloromethane and dichloroethane.
[0058] Preferably, the gaps left in the mask pattern include dots, lines and grids. The mask pattern can be designed according to actual needs.
[0059] Preferably, the hot pressing in S3 is firstly maintained at 150-180°C for 2-3h, then heated to 170-200°C for 1-2h, then heated to 180-210°C for 0.5-1h, and finally cooled under pressure.
[0060] Preferably, in S2, the thickness of the patterned thermally conductive insulating layer is 50-150 μm.
[0061] The second aspect of the present invention provides a BN thermal conductive path metal-based liquid crystal epoxy copper clad laminate prepared by the method described in the first aspect.
[0062] The metal-based liquid crystal epoxy thermally conductive copper-clad laminate prepared by the method of the present invention not only has high thermal conductivity, but also has good electrical breakdown strength and anti-peeling performance, and can meet the growing demand for heat dissipation of electronic equipment.
[0063] Compared with the prior art, the present invention has the following beneficial effects:
[0064] The present invention discloses a method for constructing a metal-based liquid crystal epoxy copper-clad laminate with a BN thermal conductive path by screen printing. The present invention uses a surfactant to modify the surface of hexagonal boron nitride to obtain a boron nitride micron sheet, and then further combines it with a liquid crystal epoxy resin matrix, copper foil, and an aluminum plate to prepare a metal-based liquid crystal epoxy thermal conductive copper-clad laminate. Specifically, a low-content modified hexagonal boron nitride / liquid crystal epoxy mixed liquid is first printed on the surface of copper foil and aluminum plate to form a patterned thermal conductive matrix, and then a high-content modified hexagonal boron nitride / liquid crystal epoxy mixed liquid is used to fill the gaps of the patterned matrix on the surface of the substrate by a screen printing method to construct a patterned thermal conductive path (such as a dot matrix, a line, a grid, etc.), and then two copper foils and aluminum plates printed with a thermal conductive insulating layer are overlapped and hot pressed to prepare a metal-based thermal conductive copper-clad laminate, wherein the high-content modified hexagonal boron nitride / liquid crystal epoxy constitutes an out-of-plane thermal conductive path, and cooperates with the low-content boron nitride / liquid crystal epoxy matrix to form an in-plane thermal conductive path. During the screen printing process of the method, the slurry can achieve a certain degree of orientation through the mesh under pressure, which is beneficial to the improvement of out-of-plane thermal conductivity. Compared with ordinary epoxy resin, the ordered structure in liquid crystal epoxy can improve the thermal conductivity of the cured product. Therefore, the metal-based liquid crystal epoxy thermal conductive copper clad laminate prepared by the method of the present invention has excellent thermal conductivity, electrical breakdown strength and peel strength, and can well serve the growing demand for heat dissipation of electronic equipment. In general, the present invention has the following advantages:
[0065] (1) The present invention enhances the thermal conductivity of the patterned insulating layer through the structural order of the liquid crystal epoxy resin, and utilizes the good fluidity of the liquid crystal to fill the pores while maintaining the ordered structure, thereby reducing the interfacial thermal resistance between the fillers, which is conducive to promoting the synergistic effect between the patterned BN thermal conductive path and the matrix, thereby having better thermal conductivity than the ordinary BN high filler content mixed sample in terms of thermal conductivity. Therefore, by combining such an insulating layer with a metal substrate to make a copper clad laminate, its thermal conductivity can be greatly increased, and the electrical breakdown strength and peel strength will not be significantly reduced, thereby better meeting the needs of the electronic packaging field.
[0066] (2) A patterned insulating layer is printed on the metal surface through a screen printing process. This process requires applying pressure to make the BN slurry pass vertically through the mesh. After the solvent evaporates quickly, the vertical orientation of part of the BN filler is maintained, thereby greatly improving the out-of-plane thermal conductivity of the patterned thermal conductive path. BRIEF DESCRIPTION OF THE DRAWINGS
[0067] Figure 1The mask design diagram of different patterns in the process of constructing metal-based liquid crystal epoxy thermally conductive copper-clad laminates; the figure shows three dot, line, and grid pattern masks with different spacing (5, 10, 15mm) and pattern widths (0.3, 0.5, 1mm). The white hollow area indicates that the high-content filler fills the patterned out-of-plane thermal conductive path part, and the orange area indicates the low-content filler fills the in-plane thermal conductive substrate part.
[0068] Figure 2 Polarized observation photos of different patterned samples during the construction process of metal-based liquid crystal epoxy thermally conductive copper-clad laminates. DETAILED DESCRIPTION
[0069] The specific embodiments of the present invention are further described below. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0070] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are commercially available unless otherwise specified.
[0071] In the following examples or comparative examples, the out-of-plane and in-plane thermal diffusion coefficients α of the thermal conductive insulation layer of the liquid crystal epoxy resin and the metal-based liquid crystal epoxy thermal conductive copper-clad laminate are tested by a laser flash meter, and the specific heat capacity C is tested by a differential scanning calorimeter. p , use a density balance to test its density ρ, and then according to the formula k = C p ·ρ·α Calculate its in-plane and out-of-plane thermal conductivity.
[0072] In the following examples or comparative examples, the peel strength of the metal-based liquid crystal epoxy thermal conductive copper clad laminate was tested according to the national standard GB / T 2791-1995. A universal tensile testing machine was used to conduct the experiment. After the sample was cut into a size of 200 mm × 25 mm, the peel strength test was started, and the tensile speed was 50 mm·min -1 , the effective peeling length is at least 100 mm, and the peeling strength calculation formula is σ=F / B (F is the peeling force, B is the sample width, and σ is the peeling strength).
[0073] In the following embodiments or comparative examples, the breakdown strength of the metal-based liquid crystal epoxy thermal conductive copper-clad laminate is tested according to the national standard GB / T 4722-2017. The experiment is carried out using a breakdown tester, the sample is cut into a square with a side length of 100 mm, and the thickness is recorded, and then the breakdown strength test is carried out. The test voltage rise rate is 500 V / s, and the voltage value at the time of breakdown is observed. The breakdown strength calculation formula is U=V / t (U is the breakdown strength, V is the breakdown voltage, and t is the sample thickness).
[0074] Example 1: A method for constructing a BN thermal conductive path metal-based liquid crystal epoxy copper clad laminate by screen printing
[0075] The construction method comprises the following steps:
[0076] (1) Preparation of modified hexagonal boron nitride (BN) by 3-aminopropyltriethoxysilane
[0077] Weigh 40g of sodium hydroxide and 200mL of deionized water into a round-bottom flask, stir and dissolve, then add 20g of boron nitride powder, and then reflux at 120°C for 24h. After the reaction, filter, wash twice with water, and dry to obtain BN powder with surface hydroxyl activated.
[0078] 40 mL of toluene and 20 g of activated BN powder were added to the round-bottom flask, and 20 mL of anhydrous ethanol and 2 g of 3-aminopropyltriethoxysilane were added to the beaker. After hydrolysis for 30 min, the solution in the beaker was added to the round-bottom flask and refluxed at 110 ° C for 10 h. After the reaction, the mixture was filtered, washed with ethanol and vacuum dried to obtain 3-aminopropyltriethoxysilane-modified hexagonal boron nitride.
[0079] (2) Preparation of aromatic imine type liquid crystal epoxy monomer (4-[[4-(oxiranylmethoxy)phenyl]imino]methyl-benzoic acid 1,4-butanediyl ester)
[0080] Dibromobutane, p-carboxybenzaldehyde and potassium carbonate were added to a flask in a molar ratio of 1:2:6, and then N,N-dimethylformamide was added. After dissolving, it was heated to 80°C under N2 protection and reacted for about 5 hours. After the reaction, a clear filtrate was obtained by suction filtration. After the filtrate was concentrated by rotary evaporation at 90°C, it was slowly dripped into ice water, stirred continuously, and the pH of the solution was adjusted to acidic (pH=3-5) with hydrochloric acid, and then a white solid was obtained by filtration, which was then washed with deionized water and dried in a blast oven at 80°C to obtain product A.
[0081] The white solid A and p-aminophenol from the previous step were weighed in a molar ratio of 1:2, dissolved in methanol at a concentration of 0.14 g / mL, and reacted at 90°C for 5-8 hours under N2 protection. After the reaction, the mixture was cooled to room temperature, filtered, washed with methanol, and vacuum dried to obtain product B.
[0082] Epichlorohydrin and product B were mixed in a flask at a molar ratio of 50:1 and heated to 100°C. Benzyltrimethylammonium chloride was then added at a molar ratio of product B: benzyltriethylammonium chloride = 1:0.06. After the reaction system was refluxed for 90 minutes, sodium hydroxide was added in batches at a molar ratio of twice that of product B within 2 hours, and water was removed by azeotropic method. After the reaction system was cooled, it was filtered, the solid was washed with ether, and then the solid was dispersed in a 10% mass fraction of sodium hydroxide aqueous solution at a concentration of 0.16 g / mL, and 1 / 5 of the volume of the mixed solution was added with xylene to improve the solubility, and then refluxed at 90°C for 1 hour, filtered after the reaction and washed with anhydrous ethanol, and finally dried in vacuo at 50°C to obtain 4-[[4-(oxiranylmethoxy)phenyl]imino]methyl-benzoic acid 1,4-butanediyl ester.
[0083] (3) Preparation of patterned copper clad laminate by screen printing
[0084] 3-aminopropyltriethoxysilane modified hexagonal boron nitride and liquid crystal epoxy monomer were dissolved in acetone at 80% and 20% mass fractions respectively to form a mixed solution with a concentration of 0.1 g / mL, and then 5wt% monomer mass fraction of curing agent 1-benzyl-2-methylimidazole was added respectively, and after ultrasonic treatment for 10 minutes, a high boron nitride content coating solution and a low boron nitride content coating solution were prepared. Among them, 80% and 20% are the mass percentages of 3-aminopropyltriethoxysilane modified hexagonal boron nitride and liquid crystal epoxy monomer.
[0085] Use a dropper to transfer an appropriate amount of coating liquid to the engraved pattern ( Figure 1 The method is to print the patterned thermal conductive substrate on the surface of the copper foil and the aluminum plate with a coating liquid as ink and then use a scraper to transfer the preset pattern to the surface of the metal substrate (copper foil and aluminum plate). The pattern thickness is 80-100um. The first time is to print a patterned thermal conductive substrate on the surface of the copper foil and the aluminum plate with a coating liquid with a low boron nitride content. The second time is to fill the gaps of the first patterned substrate with a coating liquid with a high boron nitride content to construct a patterned thermal conductive path area (dot matrix). After printing the insulating layer (the content of BN in the insulating layer is 24.03wt%) on the surface of the copper foil and the surface of the aluminum plate according to the above method, the printed surface is overlapped and placed in a hot press for hot pressing and curing. The temperature is first raised to 180°C for 2h, then raised to 200°C for 1h, then raised to 210°C for 0.5h, and finally cooled under pressure to obtain a metal-based liquid crystal epoxy thermal conductive copper clad plate patterned sample. The high-content modified hexagonal boron nitride / liquid crystal epoxy constitutes an out-of-plane heat conduction path, and cooperates with the low-content boron nitride / liquid crystal epoxy matrix to form an in-plane heat conduction path.
[0086] Its in-plane and out-of-plane thermal conductivity, peel strength and breakdown strength are shown in Table 1.
[0087] Example 2: A method for constructing a BN thermal conductive path metal-based liquid crystal epoxy copper clad laminate by screen printing
[0088] The construction method comprises the following steps:
[0089] (1) Preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride
[0090] The preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride is consistent with that in Example 1.
[0091] (2) Preparation of aromatic imine type liquid crystal epoxy (4-[[4-(oxiranylmethoxy)phenyl]imino]methyl-benzoic acid 1,4-butanediyl ester)
[0092] The preparation of aromatic imine type liquid crystal epoxy is consistent with that in Example 1.
[0093] (3) Preparation of patterned copper clad laminate by screen printing
[0094] The difference from Example 1 is that 3-aminopropyltriethoxysilane-modified hexagonal boron nitride and liquid crystal epoxy monomer are prepared into high boron nitride content coating liquid and low boron nitride content coating liquid according to the mass fraction of 60% and 30% respectively. Figure 1 The content of BN in the insulating layer is 31.55wt%.
[0095] Its appearance is Figure 2 (b) shows that the in-plane thermal conductivity, peel strength and breakdown strength are shown in Table 1.
[0096] Example 3: A method for constructing a BN thermal conductive path metal-based liquid crystal epoxy copper clad laminate by screen printing
[0097] The construction method comprises the following steps:
[0098] (1) Preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride
[0099] The preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride is consistent with that in Example 1.
[0100] (2) Preparation of aromatic imine type liquid crystal epoxy (4-[[4-(oxiranylmethoxy)phenyl]imino]methyl-benzoic acid 1,4-butanediyl ester)
[0101] The preparation of aromatic imine type liquid crystal epoxy is consistent with that in Example 1.
[0102] (3) Preparation of patterned copper foil
[0103] The difference from Example 1 is that 3-aminopropyltriethoxysilane-modified hexagonal boron nitride and liquid crystal epoxy monomer are respectively prepared into a high boron nitride content coating liquid and a low boron nitride content coating liquid according to the mass fraction of 70% and 10%. At the same time, the pattern on the screen printing plate is Figure 1 The Dot-Silkprint-3 pattern in the figure. The content of BN in the insulating layer is 26.36wt%.
[0104] Its appearance is Figure 2 (a) shows the in-plane and out-plane thermal conductivity, peel strength and breakdown strength are shown in Table 1.
[0105] Example 4: A method for constructing a BN thermal conductive path metal-based liquid crystal epoxy copper clad laminate by screen printing
[0106] The construction method comprises the following steps:
[0107] (1) Preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride
[0108] The preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride is consistent with that in Example 1.
[0109] (2) Preparation of aromatic imine type liquid crystal epoxy (4-[[4-(oxiranylmethoxy)phenyl]imino]methyl-benzoic acid 1,4-butanediyl ester)
[0110] The preparation of aromatic imine type liquid crystal epoxy is consistent with that in Example 1.
[0111] (3) Preparation of patterned copper foil
[0112] The difference from Example 1 is that 3-aminopropyltriethoxysilane-modified hexagonal boron nitride and liquid crystal epoxy monomer are respectively prepared into a high boron nitride content coating liquid and a low boron nitride content coating liquid according to the mass fraction of 70% and 10%. At the same time, the pattern on the screen printing plate is Figure 1 The Line-Silkprint-1 pattern in the figure shows that the patterned thermal conductive path area is a line. The content of BN in the insulating layer is 22.72wt%.
[0113] Its appearance is Figure 2 (d) The in-plane and out-plane thermal conductivity, peel strength and breakdown strength are shown in Table 1.
[0114] Example 5: A method for constructing a BN thermal conductive path metal-based liquid crystal epoxy copper clad laminate by screen printing
[0115] The construction method comprises the following steps:
[0116] (1) Preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride
[0117] The preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride is consistent with that in Example 1.
[0118] (2) Preparation of aromatic imine type liquid crystal epoxy (4-[[4-(oxiranylmethoxy)phenyl]imino]methyl-benzoic acid 1,4-butanediyl ester)
[0119] The preparation of aromatic imine type liquid crystal epoxy is consistent with that in Example 1.
[0120] (3) Preparation of patterned copper foil
[0121] The difference from Example 1 is that 3-aminopropyltriethoxysilane-modified hexagonal boron nitride and liquid crystal epoxy monomer are prepared into high boron nitride content coating liquid and low boron nitride content coating liquid according to the mass fraction of 80% and 20% respectively. Figure 1 The Line-Silkprint-2 pattern in the embodiment shows that the patterned thermal conductive path area is a line. The content of BN in the insulating layer is 26.84wt%.
[0122] Its in-plane and out-of-plane thermal conductivity, peel strength and breakdown strength are shown in Table 1.
[0123] Example 6: A method for constructing a BN thermal conductive path metal-based liquid crystal epoxy copper clad laminate by screen printing
[0124] The construction method comprises the following steps:
[0125] (1) Preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride
[0126] The preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride is consistent with that in Example 1.
[0127] (2) Preparation of aromatic imine type liquid crystal epoxy (4-[[4-(oxiranylmethoxy)phenyl]imino]methyl-benzoic acid 1,4-butanediyl ester)
[0128] The preparation of aromatic imine type liquid crystal epoxy is consistent with that in Example 1.
[0129] (3) Preparation of patterned copper foil
[0130] The difference from Example 1 is that 3-aminopropyltriethoxysilane-modified hexagonal boron nitride and liquid crystal epoxy monomer are prepared into high boron nitride content coating liquid and low boron nitride content coating liquid according to the mass fraction of 60% and 30% respectively. Figure 1 The Line-Silkprint-3 pattern in the embodiment shows that the patterned thermal conductive path area is a line. The content of BN in the insulating layer is 37.06wt%.
[0131] Its appearance is Figure 2 (c) shows that the in-plane and out-plane thermal conductivity, peel strength and breakdown strength are shown in Table 1.
[0132] Example 7: A method for constructing a BN thermal conductive path metal-based liquid crystal epoxy copper clad laminate by screen printing
[0133] The construction method comprises the following steps:
[0134] (1) Preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride
[0135] The preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride is consistent with that in Example 1.
[0136] (2) Preparation of aromatic imine type liquid crystal epoxy (4-[[4-(oxiranylmethoxy)phenyl]imino]methyl-benzoic acid 1,4-butanediyl ester)
[0137] The preparation of aromatic imine type liquid crystal epoxy is consistent with that in Example 1.
[0138] (3) Preparation of patterned copper foil
[0139] The difference from Example 1 is that 3-aminopropyltriethoxysilane-modified hexagonal boron nitride and liquid crystal epoxy monomer are prepared into high boron nitride content coating liquid and low boron nitride content coating liquid according to the mass fraction of 80% and 30% respectively. Figure 1 The Grid-Silkprint-1 pattern in the embodiment shows that the patterned thermal conductive path area is a grid. The content of BN in the insulating layer is 32.30wt%.
[0140] Its appearance is Figure 2 (e) shows that the in-plane and out-plane thermal conductivity, peel strength and breakdown strength are shown in Table 1.
[0141] Example 8: A method for constructing a BN thermal conductive path metal-based liquid crystal epoxy copper clad laminate by screen printing
[0142] The construction method comprises the following steps:
[0143] (1) Preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride
[0144] The preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride is consistent with that in Example 1.
[0145] (2) Preparation of aromatic imine type liquid crystal epoxy (4-[[4-(oxiranylmethoxy)phenyl]imino]methyl-benzoic acid 1,4-butanediyl ester)
[0146] The preparation of aromatic imine type liquid crystal epoxy is consistent with that in Example 1.
[0147] (3) Preparation of patterned copper foil
[0148] The difference from Example 1 is that 3-aminopropyltriethoxysilane-modified hexagonal boron nitride and liquid crystal epoxy monomer are prepared into high boron nitride content coating liquid and low boron nitride content coating liquid according to the mass fraction of 60% and 10% respectively. Figure 1 The Grid-Silkprint-2 pattern in the embodiment shows that the patterned thermal conductive path area is a grid. The content of BN in the insulating layer is 28.98wt%.
[0149] Its in-plane and out-of-plane thermal conductivity, peel strength and breakdown strength are shown in Table 1.
[0150] Example 9: A method for constructing a BN thermal conductive path metal-based liquid crystal epoxy copper clad laminate by screen printing
[0151] The construction method comprises the following steps:
[0152] (1) Preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride
[0153] The preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride is consistent with that in Example 1.
[0154] (2) Preparation of aromatic imine type liquid crystal epoxy (4-[[4-(oxiranylmethoxy)phenyl]imino]methyl-benzoic acid 1,4-butanediyl ester)
[0155] The preparation of aromatic imine type liquid crystal epoxy is consistent with that in Example 1.
[0156] (3) Preparation of patterned copper foil
[0157] The difference from Example 1 is that 3-aminopropyltriethoxysilane-modified hexagonal boron nitride and liquid crystal epoxy monomer are respectively prepared into a high boron nitride content coating liquid and a low boron nitride content coating liquid according to the mass fraction of 70% and 20%. Figure 1 The Grid-Silkprint-3 pattern in the embodiment shows that the patterned thermal conductive path area is a grid. The content of BN in the insulating layer is 48.24wt%.
[0158] Its appearance is Figure 2 (f) shows that the in-plane and out-plane thermal conductivity, peel strength and breakdown strength are shown in Table 1.
[0159] Example 10: A method for constructing a BN thermal conductive path metal-based liquid crystal epoxy copper clad laminate by screen printing
[0160] The construction method comprises the following steps:
[0161] (1) Preparation of hexagonal boron nitride modified with γ-glycidyloxypropyltrimethoxysilane
[0162] Weigh 40g of sodium hydroxide and 200mL of deionized water into a round-bottom flask, stir and dissolve, then add 20g of boron nitride powder, and then reflux at 120°C for 24h. After the reaction, filter, wash twice with water, and dry to obtain BN powder with surface hydroxyl activated.
[0163] 40 mL of toluene and 20 g of activated BN powder were added to a round-bottom flask, and 20 mL of anhydrous ethanol was added to a beaker. After adjusting to a weakly acidic environment (pH = 3-5) with acetic acid, 2 g of γ-glycidyloxypropyltrimethoxysilane was added for hydrolysis for 30 min, and then the solution in the beaker was added to the aforementioned round-bottom flask and refluxed at 110 ° C for 10 h. After the reaction, the mixture was filtered, washed with ethanol and vacuum dried to obtain γ-glycidyloxypropyltrimethoxysilane-modified hexagonal boron nitride.
[0164] (2) Preparation of aromatic imine type liquid crystal epoxy (4-[[4-(oxiranylmethoxy)phenyl]imino]methyl-benzoic acid 1,4-butanediyl ester)
[0165] The preparation of aromatic imine type liquid crystal epoxy is consistent with that in Example 1.
[0166] (3) Preparation of patterned copper foil
[0167] The difference from Example 1 is that the hexagonal boron nitride modified by γ-glycidyloxypropyltrimethoxysilane and the liquid crystal epoxy monomer are prepared into a high boron nitride content coating liquid and a low boron nitride content coating liquid according to the mass fraction of 70% and 20% respectively. Figure 1 The Grid-Silkprint-3 pattern in the embodiment shows that the patterned thermal conductive path area is a grid. The content of BN in the insulating layer is 47.52wt%.
[0168] Its in-plane and out-of-plane thermal conductivity, peel strength and breakdown strength are shown in Table 1.
[0169] Example 11: A method for constructing a BN thermal conductive path metal-based liquid crystal epoxy copper clad laminate by screen printing
[0170] The construction method comprises the following steps:
[0171] (1) Preparation of urea-modified hexagonal boron nitride
[0172] Boron nitride and urea were added to a ball mill at a weight ratio of 1:20, and then ball milled at a speed of 600 rpm for 20 hours. The obtained powder was dissolved in water at a concentration of 0.1 g / mL, and dialyzed for 1 week using a dialysis bag with a molecular weight cutoff of 3500 kDa to remove urea. After vacuum filtration and drying, urea-modified hexagonal boron nitride powder was obtained.
[0173] (2) Preparation of aromatic imine type liquid crystal epoxy (4-[[4-(oxiranylmethoxy)phenyl]imino]methyl-benzoic acid 1,4-butanediyl ester)
[0174] The preparation of aromatic imine type liquid crystal epoxy is consistent with that in Example 1.
[0175] (3) Preparation of patterned copper foil
[0176] The difference from Example 1 is that urea-modified hexagonal boron nitride and liquid crystal epoxy monomer are prepared into high boron nitride content coating liquid and low boron nitride content coating liquid according to the mass fraction of 70% and 20% respectively. Figure 1 The Grid-Silkprint-3 pattern in the embodiment shows that the patterned thermal conductive path area is a grid. The content of BN in the insulating layer is 45.78wt%.
[0177] Its in-plane and out-of-plane thermal conductivity, peel strength and breakdown strength are shown in Table 1.
[0178] Example 12: A method for constructing a BN thermal conductive path metal-based liquid crystal epoxy copper clad laminate by screen printing
[0179] The construction method comprises the following steps:
[0180] (1) Preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride
[0181] The preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride is consistent with that in Example 1.
[0182] (2) Preparation of aromatic ester liquid crystal epoxy monomer (1,1'-(1,4-phenylene)bis[4-(2-oxiranylmethoxy)benzoate])
[0183] Add p-hydroxybenzoic acid (0.3 mol) and methanol (200 ml) to a three-necked flask in turn, place it in an oil bath and heat it to 80°C, dissolve potassium hydroxide (1 mol) in 65 ml of water and slowly drop it into the three-necked flask, stir for 30 minutes, then slowly drop allyl bromide (0.35 mol) into the three-necked flask, stir and reflux for 8 hours. Cool to room temperature, filter to remove potassium bromide, and remove the solvent methanol by rotary evaporation. Add 1.25L of deionized water and 300ml of cyclohexane to the remaining solid in turn, pour it into a separatory funnel and let it stand for stratification, the lower layer is the aqueous phase. Heat the aqueous phase to 40°C and neutralize it with hydrochloric acid solution to neutrality. Filter and collect the white solid, wash it with water 3 times, and finally recrystallize it with ethanol, place it in a vacuum oven at 60°C and dry it for 24 hours to obtain the pre-product 1.
[0184] Add pre-product 1 (0.1 mol), dimethylformamide (3 drops), and sulfoxide chloride (0.5 mol) to a three-necked flask in sequence, place in an oil bath and heat to 80°C, and stir to react for 4 hours. Remove excess sulfoxide chloride by vacuum filtration, cool to room temperature, add 60 ml of pyridine, and place in an ice bath. Dissolve hydroquinone (0.055 mol) in 40 ml of pyridine, slowly dropwise add to the three-necked flask, react in an ice bath for 4 hours, and react at room temperature for 20 hours. After the reaction is completed, add water to precipitate solids, wash the solids with 10% HCl aqueous solution, 10% sodium carbonate aqueous solution, and water in sequence, and finally recrystallize with ethyl acetate, place in a 60°C vacuum oven and dry for 24 hours to obtain pre-product 2.
[0185] Add pre-product 2 (0.03 mol), m-chloroperbenzoic acid (0.3 mol), and dichloromethane (400 ml) to a three-necked flask in sequence, place it in an oil bath and heat it to 50°C, and stir to react for 48 hours. Cool to room temperature, add 0.3 mol sodium sulfite aqueous solution and 0.3 mol sodium bicarbonate aqueous solution in sequence, pour into a separatory funnel and let stand to separate the layers. The lower layer is the dichloromethane layer. The dichloromethane layer is evaporated to remove dichloromethane, and the solid is washed three times with water and methanol in sequence, and finally recrystallized with ethyl acetate, placed in a vacuum oven at 60°C and dried for 24 hours to obtain the final product 1,1'-(1,4-phenylene)bis[4-(2-oxiranylmethoxy)benzoate] (3) Preparation of patterned copper foil
[0186] The difference from Example 1 is that 3-aminopropyltriethoxysilane-modified hexagonal boron nitride and liquid crystal epoxy monomer are respectively prepared into a high boron nitride content coating liquid and a low boron nitride content coating liquid according to the mass fraction of 70% and 20%. Figure 1 The Grid-Silkprint-3 pattern in the embodiment shows that the patterned thermal conductive path area is a grid. The content of BN in the insulating layer is 45.24wt%.
[0187] Its in-plane and out-of-plane thermal conductivity, peel strength and breakdown strength are shown in Table 1.
[0188] Example 13: A method for constructing a BN thermal conductive path metal-based liquid crystal epoxy copper clad laminate by screen printing
[0189] The construction method comprises the following steps:
[0190] (1) Preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride
[0191] The preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride is consistent with that in Example 1.
[0192] (2) Preparation of biphenyl type liquid crystal epoxy monomer (4'-(2-oxiranylmethoxy)-[1,1'-biphenyl]-4-carboxylic acid 4,4'-(1,4-butanediyl) ester)
[0193] 4'-Hydroxybiphenyl-4-carboxylic acid (5.0 g, 23.3 mmol) was dissolved in methanol (150 mL), and 95-98% concentrated sulfuric acid (5.0 mL) was added dropwise, and then the reaction mixture was heated to reflux at 50°C for 6 h. After the reaction, the methanol was distilled off under reduced pressure, and the obtained solid was washed with water until neutral, and dried to obtain product A;
[0194] The product A (0.1 mol) from the previous step was mixed with 1,4-butanediol (0.05 mol) and 0.2 g of calcium acetate hydrate in a flask, heated to 180°C and refluxed for two hours, then cooled to room temperature, and methanol was added to collect the product. The obtained solid was filtered and vacuum dried to obtain product B.
[0195] Epichlorohydrin (50 mol) and product B (1 mol) were mixed in a flask and heated to 100°C, and then benzyltrimethylammonium chloride was added in a molar ratio of product B: benzyltriethylammonium chloride = 1:0.06. Then the reaction system was refluxed at this temperature for 90 minutes, and 2 mol of sodium hydroxide was added in batches within 2 hours after the reaction, and the water was removed by azeotropic method. Subsequently, the obtained mixed solution was filtered to obtain a solid, and then the solid was washed with ether, and then the solid was dispersed in a 10% mass fraction of sodium hydroxide aqueous solution at a concentration of 0.16 g / mL, and 400 mL of xylene was added to improve the solubility, and then refluxed at 90°C for 1 hour to remove the residual hydrogen chloride, and after the reaction, the solid was filtered and washed with anhydrous ethanol, and finally vacuum dried at 50°C to obtain 4'-(2-oxiranylmethoxy)-[1,1'-biphenyl]-4-carboxylic acid 4,4'-(1,4-butanediyl) ester.
[0196] (3) Preparation of patterned copper foil
[0197] The difference from Example 1 is that 3-aminopropyltriethoxysilane-modified hexagonal boron nitride and liquid crystal epoxy monomer are respectively prepared into a high boron nitride content coating liquid and a low boron nitride content coating liquid according to the mass fraction of 70% and 20%. Figure 1 The Grid-Silkprint-3 pattern in the structure has a patterned thermal conductive path area of a grid. The content of BN in the insulating layer is 42.36wt%. In addition, the hot pressing curing is 150°C for 2 hours, then heated to 170°C for 1 hour, then heated to 180°C for 0.5 hours, and finally cooled under pressure.
[0198] Its in-plane and out-of-plane thermal conductivity, peel strength and breakdown strength are shown in Table 1.
[0199] Example 14: A method for constructing a BN thermal conductive path metal-based liquid crystal epoxy copper clad laminate by screen printing
[0200] The construction method comprises the following steps:
[0201] (1) Preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride
[0202] The preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride is consistent with that in Example 1.
[0203] (2) Preparation of aromatic imine type liquid crystal epoxy (4-[[4-(oxiranylmethoxy)phenyl]imino]methyl-benzoic acid 1,4-butanediyl ester)
[0204] The preparation of aromatic imine type liquid crystal epoxy is consistent with that in Example 1.
[0205] (3) Preparation of patterned copper foil
[0206] The difference from Example 1 is that 3-aminopropyltriethoxysilane modified hexagonal boron nitride and liquid crystal epoxy monomer are dissolved in an appropriate amount of acetone at a mass fraction of 70% and 20% respectively, and then 5wt% monomer mass fraction of curing agent 2-heptadecylimidazole is added, and after ultrasonic treatment for 10 minutes, a high boron nitride content coating liquid and a low boron nitride content coating liquid are prepared. At the same time, the pattern on the screen printing plate is Figure 1 The Grid-Silkprint-3 pattern in the embodiment shows that the patterned thermal conductive path area is a grid. The content of BN in the insulating layer is 46.84wt%.
[0207] Its in-plane and out-of-plane thermal conductivity, peel strength and breakdown strength are shown in Table 1.
[0208] Example 15: A method for constructing a BN thermal conductive path metal-based liquid crystal epoxy copper clad laminate by screen printing
[0209] The construction method comprises the following steps:
[0210] (1) Preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride
[0211] The preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride is consistent with that in Example 1.
[0212] (2) Preparation of aromatic imine type liquid crystal epoxy (4-[[4-(oxiranylmethoxy)phenyl]imino]methyl-benzoic acid 1,4-butanediyl ester)
[0213] The preparation of aromatic imine type liquid crystal epoxy is consistent with that in Example 1.
[0214] (3) Preparation of patterned copper foil
[0215] The difference from Example 1 is that 3-aminopropyltriethoxysilane modified hexagonal boron nitride and aromatic imine type liquid crystal epoxy monomer are dissolved in an appropriate amount of acetone at a mass fraction of 70% and 20% respectively, and then 5wt% monomer mass fraction of curing agent 2,4-diamino-6-(2-undecylimidazole-1-ethyl)-S-triazine is added, and after ultrasonic treatment for 10 minutes, a high boron nitride content coating liquid and a low boron nitride content coating liquid are prepared. At the same time, the pattern on the screen printing screen is Figure 1 The Grid-Silkprint-3 pattern in the embodiment shows that the patterned thermal conductive path area is a grid. The content of BN in the insulating layer is 48.88wt%.
[0216] Its in-plane and out-of-plane thermal conductivity, peel strength and breakdown strength are shown in Table 1.
[0217] Comparative Example 1: A method for constructing a BN thermal conductive path metal-based epoxy copper-clad laminate by screen printing
[0218] The construction method comprises the following steps:
[0219] (1) Preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride
[0220] The preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride is consistent with that in Example 1.
[0221] (2) Preparation of patterned copper foil
[0222] 3-Aminopropyltriethoxysilane modified hexagonal boron nitride and ordinary E51 epoxy monomer without liquid crystal structure were dissolved in an appropriate amount of acetone at a mass fraction of 70% and 10%, respectively, and then 5wt% of the monomer mass fraction of the curing agent 1-benzyl-2-methylimidazole was added respectively. After ultrasonication for 10 minutes, a high boron nitride content coating liquid and a low boron nitride content coating liquid were prepared.
[0223] Use a dropper to transfer an appropriate amount of coating liquid to the engraved pattern ( Figure 1 The first time, a patterned thermal conductive matrix is printed on the surface of the copper foil and the aluminum plate using a low boron nitride content coating liquid, and the second time, a high boron nitride content coating liquid is used to fill the gaps of the first patterned matrix to construct a patterned thermal conductive path area (dot matrix). After printing an insulating layer (thickness of 80-100um, BN content of 24.2wt%) on the surface of the copper foil and the surface of the aluminum plate, the printed surface is overlapped and placed in a hot press for hot pressing and curing. The temperature is first raised to 180°C for 2h, then raised to 200°C for 1h, and then raised to 210°C for 0.5h. Finally, the pressure is maintained and cooled to obtain a metal-based liquid crystal epoxy thermal conductive copper clad plate patterned sample. The high-content modified hexagonal boron nitride / liquid crystal epoxy constitutes an out-of-plane heat conduction path, and cooperates with the low-content boron nitride / liquid crystal epoxy matrix to form an in-plane heat conduction path.
[0224] Its in-plane and out-of-plane thermal conductivity, peel strength and breakdown strength are shown in Table 1.
[0225] Comparative Example 2: A method for constructing a BN thermal conductive path metal-based epoxy copper-clad laminate by screen printing
[0226] The construction method comprises the following steps:
[0227] (1) Preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride
[0228] The preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride is consistent with that in Example 1.
[0229] (2) Preparation of patterned copper foil
[0230] The difference from Comparative Example 1 is that the pattern on the screen printing screen is Figure 1 The Line-Silkprint-1 pattern in the embodiment has a patterned heat conduction path area of lines. The content of BN in the insulating layer is 28.15wt%.
[0231] Its in-plane and out-of-plane thermal conductivity, peel strength and breakdown strength are shown in Table 1.
[0232] Comparative Example 3: A method for constructing a BN thermal conductive path metal-based epoxy copper-clad laminate by screen printing
[0233] The construction method comprises the following steps:
[0234] (1) Preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride
[0235] The preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride is consistent with that in Example 1.
[0236] (2) Preparation of patterned copper foil
[0237] The difference from Comparative Example 1 is that 3-aminopropyltriethoxysilane-modified hexagonal boron nitride and ordinary E51 epoxy monomer without liquid crystal structure are used to prepare boron nitride content coating liquid and low boron nitride content coating liquid according to the mass fraction of 70% and 20% respectively. At the same time, the pattern on the screen printing screen is Figure 1 The Grid-Silkprint-3 pattern in the embodiment shows that the patterned thermal conductive path area is a grid. The content of BN in the insulating layer is 43.22wt%.
[0238] Its in-plane and out-of-plane thermal conductivity, peel strength and breakdown strength are shown in Table 1.
[0239] Comparative Example 4: A method for constructing a BN thermal conductive path metal-based liquid crystal epoxy copper clad laminate
[0240] The construction method comprises the following steps:
[0241] (1) Preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride
[0242] The preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride is consistent with that in Example 1.
[0243] (2) Preparation of aromatic imine type liquid crystal epoxy (4-[[4-(oxiranylmethoxy)phenyl]imino]methyl-benzoic acid 1,4-butanediyl ester)
[0244] The preparation of aromatic imine type liquid crystal epoxy is consistent with that in Example 1.
[0245] (3) Preparation of Liquid Crystal Epoxy Composite Insulation Layer Copper Foil
[0246] 3-aminopropyltriethoxysilane modified hexagonal boron nitride was mixed with the monomer according to the mass fraction of 25% of liquid crystal epoxy monomer and dissolved in an appropriate amount of acetone, and then 5wt% of the monomer mass fraction of curing agent 1-benzyl-2-methylimidazole was added, and the mixture was ultrasonicated for 10 minutes to form a slurry, which was then scraped on the copper foil and aluminum plate to form an insulating layer with a thickness of 80-100um (the content of BN in the insulating layer was 23.27wt%), and the two substrate coating surfaces were overlapped and placed in a hot press for hot pressing curing, first at 180°C for 2h, then heated to 200°C for 1h, then heated to 210°C for 0.5h, and finally cooled under pressure to obtain a blend insulating layer sample, and its in-plane thermal conductivity, peel strength and breakdown strength are shown in Table 1.
[0247] Comparative Example 5: A method for constructing a BN thermal conductive path metal-based liquid crystal epoxy copper clad laminate
[0248] The construction method comprises the following steps:
[0249] (1) Preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride
[0250] The preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride is consistent with that in Example 1.
[0251] (2) Preparation of aromatic imine type liquid crystal epoxy (4-[[4-(oxiranylmethoxy)phenyl]imino]methyl-benzoic acid 1,4-butanediyl ester)
[0252] The preparation of aromatic imine type liquid crystal epoxy is consistent with that in Example 1.
[0253] (3) Preparation of Liquid Crystal Epoxy Composite Insulation Layer Copper Foil
[0254] 3-aminopropyltriethoxysilane modified hexagonal boron nitride was mixed with the monomer according to the mass fraction of 45% of liquid crystal epoxy monomer and dissolved in an appropriate amount of acetone, and then 5wt% of the monomer mass fraction of curing agent 1-benzyl-2-methylimidazole was added, and the mixture was ultrasonicated for 10 minutes to form a slurry, which was then scraped on the copper foil and aluminum plate to form an insulating layer with a thickness of 80-100um (the content of BN in the insulating layer was 45.88wt%), and the two substrate coating surfaces were overlapped and placed in a hot press for hot pressing curing, first at 180°C for 2h, then heated to 200°C for 1h, then heated to 210°C for 0.5h, and finally cooled under pressure to obtain a blend insulating layer sample, and its in-plane thermal conductivity, peel strength and breakdown strength are shown in Table 1.
[0255] Comparative Example 6: A method for constructing a BN thermal conductive path metal-based liquid crystal epoxy copper clad laminate by screen printing
[0256] The construction method comprises the following steps:
[0257] (1) Preparation of aromatic imine type liquid crystal epoxy (4-[[4-(oxiranylmethoxy)phenyl]imino]methyl-benzoic acid 1,4-butanediyl ester)
[0258] The preparation of aromatic imine type liquid crystal epoxy is consistent with that in Example 1.
[0259] (2) Preparation of patterned copper foil
[0260] Unmodified hexagonal boron nitride and liquid crystal epoxy monomer were dissolved in an appropriate amount of acetone at a mass fraction of 70% and 20%, respectively, and then 5wt% of the monomer mass fraction of the curing agent 1-benzyl-2-methylimidazole was added respectively. After ultrasonic treatment for 10 minutes, a high boron nitride content coating liquid and a low boron nitride content coating liquid were prepared.
[0261] Use a dropper to transfer an appropriate amount of coating liquid to the engraved pattern ( Figure 1The Grid-Silkprint-3 pattern in the figure is printed on a screen printing screen, and then the coating liquid is used as ink to transfer the preset pattern to the surface of the metal substrate (copper foil and aluminum plate) using a scraper. The transfer is done twice. The first time is to print a patterned thermal conductive matrix on the surface of the copper foil and the aluminum plate with a low boron nitride content coating liquid. The second time is to fill the gaps of the first patterned matrix with a high boron nitride content coating liquid to construct a patterned thermal conductive path area (grid). After printing an insulating layer with a thickness of 80-100um (the content of BN in the insulating layer is 46.2wt%) on the surface of the copper foil and the surface of the aluminum plate, the printed surfaces are overlapped and placed in a hot press for hot pressing and curing. The temperature is first raised to 180°C for 2h, then raised to 200°C for 1h, and then raised to 210°C for 0.5h. Finally, the pressure is maintained and cooled to obtain a metal-based liquid crystal epoxy thermal conductive copper clad plate patterned sample. The high-content hexagonal boron nitride / liquid crystal epoxy constitutes an out-of-plane heat conduction path, and cooperates with the low-content boron nitride / liquid crystal epoxy matrix to form an in-plane heat conduction path.
[0262] Its in-plane and out-of-plane thermal conductivity, peel strength and breakdown strength are shown in Table 1.
[0263] Comparative Example 7: A method for constructing a BN thermal conductive path metal-based liquid crystal epoxy copper clad laminate
[0264] (1) Preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride
[0265] The preparation of 3-aminopropyltriethoxysilane modified hexagonal boron nitride is consistent with that in Example 1.
[0266] (2) Preparation of blended series samples
[0267] 3-aminopropyltriethoxysilane modified hexagonal boron nitride was mixed with aromatic imine type liquid crystal epoxy monomer (4-[[4-(oxiranylmethoxy)phenyl]imino]methyl-benzoic acid 1,4-butanediyl ester) according to the mass fraction of liquid crystal epoxy monomer 0%, 10%, 20%, 30%, 40%, 50%, 60%, 70% respectively, and then dissolved in acetone to form a mixed solution of 0.1g / mL, and then 5%wt monomer mass fraction of curing agent 1-benzyl-2-methylimidazole was added. After ultrasonication for 10min, it was dropped into a mold with an outer diameter of 14cm, an inner diameter of 10cm, and a thickness of 0.5mm. After drying the solvent, it was placed in a hot press for hot pressing and curing, first at 180℃ for 2h, then heated to 200℃ for 1h, then heated to 210℃ for 0.5h, and finally cooled under pressure to obtain a series of blended samples. The thermal conductivity and tensile strength are shown in Table 2.
[0268] Table 1 Insulation layer test data of liquid crystal epoxy single-sided flexible thermal conductive copper clad laminates of Examples 1-15 and Comparative Examples 1-6
[0269]
[0270]
[0271] Note: BN mass content refers to the proportion of modified BN in the total amount of modified BN, liquid crystal epoxy monomer and curing agent.
[0272] From Table 1, the thermal conductivity data of each embodiment and comparative example are analyzed by range. Among the three pattern types (dot matrix, line, grid), the thermal conductivity of the grid pattern is the largest. The grid is the type with the largest patterned area. Since the boron nitride content of the patterned part is relatively high, there are more areas with high thermal conductivity, so the thermal conductivity effect is the best. Similarly, for the two factors of pattern width and pattern spacing, the larger the pattern width, the smaller the pattern spacing, that is, the larger the corresponding patterned area, the better the thermal conductivity effect. The thermal conductivity data of the embodiment are analyzed by variance. The influence of pattern spacing and matrix boron nitride content on the thermal conductivity of the out-of-plane and in-plane is not significant, so the influence of the change of pattern spacing and matrix boron nitride content on the thermal conductivity of the patterned sample can be ignored statistically, and other patterning factors, pattern type, pattern width, and pattern boron nitride content, are all factors that will have a significant effect on thermal conductivity. Therefore, combined with the results of range analysis and variance analysis, Example 3, Example 4, and Example 9 are selected as copper clad laminate formulas for comparison. It can be seen from Comparative Examples 1, 2, 3 and Examples 3, 4, and 9 that the thermal conductivity and breakdown strength of ordinary epoxy are significantly inferior to those of liquid crystal epoxy samples. Liquid crystal epoxy maintains an ordered structure during curing, which is not only conducive to the transmission of phonons and improves thermal conductivity, but also the regularity of the structure is conducive to resisting electrical breakdown, and is more advantageous in the application of copper clad laminates. Ordinary epoxy has more advantages in peel strength, because ordinary E51 epoxy resin is liquid at room temperature, has good fluidity, is more conducive to filling gaps, and reduces defects, but the peel strength of liquid crystal epoxy samples can also meet the use requirements. From the comparison of Example 9 and Example 10, it can be seen that the thermal conductivity and breakdown strength of the patterned sample of hexagonal boron nitride modified by γ-glycidyloxypropyltrimethoxysilane are slightly weaker than those of the sample of boron nitride modified by 3-aminopropyltriethoxysilane, but it is superior in peel strength because the chemical structures of the two are close, so the effect of modification is not much different. From the comparison between Example 9 and Example 11, it can be seen that the thermal conductivity of urea-modified boron nitride is better, because this modification is more destructive, has more grafted groups, and has a lower contact thermal resistance with the resin, but the peel strength and breakdown strength are not superior, because the structure of boron nitride is greatly damaged, and the urea-modified boron nitride has a greater tendency to aggregate than the other two modified boron nitrides, which will bring more defects. Based on the above experimental results, it can be seen that 3-aminopropyltriethoxysilane-modified boron nitride is a relatively more suitable filler choice among the three. From the comparison between Example 9 and Examples 12 and 13, it can be seen that the thermal conductivity, breakdown strength and peel strength of the patterned samples of aromatic ester type liquid crystal epoxy and biphenyl type liquid crystal epoxy are not as good as the patterned samples of aromatic imine type liquid crystal epoxy, indicating that the molecular structure of aromatic imine type liquid crystal epoxy is more conducive to forming a regular liquid crystal structure.From the comparison between Example 9 and Examples 14 and 15, it can be seen that different curing agents have similar curing mechanisms, so there is not much difference in peel strength, but in terms of thermal conductivity and breakdown strength, 2-heptadecylimidazole has more defects due to its faster curing speed, which is not as good as the other two curing agents. From the comparison between Comparative Examples 4 and 5 and Examples 3, 4, and 9, it can be seen that under the same filler content, the samples without screen printing patterning not only have lower thermal conductivity, but also have a breakdown strength value that is not as good as the corresponding embodiment. In terms of peel strength, except for Example 4, they are not as good as the samples after screen printing patterning. It can be seen that the sample structure after screen printing patterning is more regular. From the comparison between Comparative Example 6 and Example 9, it can be seen that the performance of the samples of unmodified boron nitride is slightly lower than that of the samples using modified boron nitride in all aspects. This is because the boron nitride has better compatibility with the resin after modification, which reduces the generation of defects.
[0273] Table 2 Tensile strength and thermal conductivity results of samples containing 3-aminopropyltriethoxysilane-modified boron nitride / liquid crystal epoxy series in comparative example 7
[0274]
[0275] In order to further explore the influence trend of boron nitride filler on the performance of copper clad laminate, a series of samples with different boron nitride contents were prepared in Comparative Example 7 using 3-aminopropyltriethoxysilane-modified boron nitride and aromatic imide-type liquid crystal epoxy monomers. It can be seen from Table 2 that once the boron nitride filler is added, the tensile strength drops sharply. After exceeding 40%, the mechanical properties of the composite material have become very fragile, so the content of the matrix filler is preferably controlled below 30%. From the improvement of thermal conductivity, it can be seen that when the filler content is above 50%, as the filler content increases, the increase in thermal conductivity is much greater than the filler content below 50%. Therefore, in order to obtain better thermal conductivity, the filler content of the patterned part is preferably controlled above 60%.
[0276] In summary, the present invention uses modified BN and liquid crystal epoxy adhesive to prepare a patterned heat-conducting unit with a high boron nitride filling content and an insulating layer of a heat-conducting matrix with a low filling content on a metal substrate and copper foil, and then the metal substrate, the heat-conducting insulating layer and the copper foil are composited to form a heat-conducting copper-clad laminate, and the heat-conducting units are connected to each other to form a heat-conducting path running through the metal substrate and the copper foil, and then the patterned heat-conducting path and the low-content micron BN filler / liquid crystal epoxy are matched with each other, and the ordered structure in the liquid crystal epoxy body and the synergistic effect between the filled BN heat-conducting path are used to construct an efficient heat-conducting network running through the entire heat-conducting insulating layer and connecting the metal base and the copper foil. Since the liquid crystal epoxy resin has a certain ordered structure, it can solve the contradiction between the adhesion and thermal conductivity between the inorganic particles and the metal substrate. Therefore, the metal-based liquid crystal epoxy heat-conducting copper-clad laminate prepared by the method of the present invention has excellent thermal conductivity, electrical breakdown strength and peel strength, and can well serve the growing demand for heat dissipation of electronic equipment.
[0277] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the protection scope of the present invention.
Claims
1. A method for constructing a BN thermal conductive path metal-based liquid crystal epoxy copper clad laminate by screen printing, It is characterized in that The following steps are involved: S1. First, hexagonal boron nitride is modified with a surfactant, and then a liquid crystal epoxy monomer, a curing agent and a surface-modified boron nitride are dissolved in an organic solvent to prepare a high-boron nitride content coating liquid and a low-boron nitride content coating liquid, wherein the mass ratio of hexagonal boron nitride to the liquid crystal epoxy monomer is 3-4:2-1 in the high-boron nitride content coating liquid, and the mass ratio of hexagonal boron nitride to the liquid crystal epoxy monomer is 1-3:7-9 in the low-boron nitride content coating liquid; S2, firstly, using a screen printing method to print a low-boron nitride content coating liquid on the surface of the copper foil and the aluminum plate to form a patterned thermal conductive matrix, and then using a screen printing method to fill the gaps of the patterned matrix on the surface of the substrate with a high-boron nitride content coating liquid to construct a patterned thermal conductive path, and then printing a patterned thermal conductive insulating layer on the surface of the copper foil and the aluminum plate; S3. Overlap two copper foils and aluminum plates printed with patterned thermally conductive insulating layers and perform hot pressing to prepare a metal-based thermally conductive copper-clad laminate, wherein a coating liquid with a high boron nitride content constitutes an out-of-plane thermal conductive path and cooperates with a coating liquid with a low boron nitride content to construct an in-plane thermal conductive path.
2. A method for constructing a BN thermal conductive path metal-based liquid crystal epoxy copper clad laminate by screen printing according to claim 1, It is characterized in that S2 is specifically as follows: placing a silk screen with a mask pattern on top of a copper foil or an aluminum plate, leaving gaps in the pattern, and then screen printing a coating liquid with a low boron nitride content on its surface. After drying, the mask is removed to form an in-plane thermal conductive substrate of the insulating layer. Another silk screen matching the substrate pattern is used to print a coating liquid with a high boron nitride content on the surface of the copper foil or aluminum plate to fill the gaps left by the previous printing. After drying, the mask is removed to form a patterned out-of-plane thermal conductive path.
3. A method for constructing a BN thermal conductive path metal-based liquid crystal epoxy copper clad laminate by screen printing according to claim 1, It is characterized in that S1 The liquid crystal epoxy monomer includes at least one of an aromatic imine liquid crystal epoxy monomer, an aromatic ester liquid crystal epoxy monomer, and a biphenyl liquid crystal epoxy monomer; the aromatic imine liquid crystal epoxy monomer includes 4-[[4-(oxiranylmethoxy)phenyl]imino]methyl-benzoic acid 1,4-butanediyl ester, 4',4'-bis(4-hydroxybenzylidene)-diaminophenylene diglycidyl ether, terephthalylidene-bis-(4-aminophenol) diglycidyl ether Glycerol ether, terephthalylidene-bis-(4-amino-3-methylphenol) diglycidyl ether, 4-(2-oxiranylmethoxy)-benzaldehyde 2-((4-(2-oxiranylmethoxy)phenyl)methylene)hydrazone, 4-(2-oxiranylmethoxy)-N-((4-(2-oxiranylmethoxy)phenyl)methylene)aniline; the aromatic ester type liquid crystal epoxy monomer includes 4-(oxiranylmethoxy)- Benzoic acid 1,4-butanediylbis(oxy-4,1-phenylene) ester, 4-(9-oxiranylnonyloxy)benzoic acid 1,4-phenylene ester, 4-(10,11-epoxyundecenyloxy)phenyl-4-[(10,11-epoxyundecenyloxy)benzyloxy]benzoate, 1,1'-(1,4-phenylene)bis[4-(2-oxiranylmethoxy)benzoate] one or more; the biphenyl type liquid crystal ring The oxygen monomer includes one or more of 2,2'[1,2-ethanediylbis(oxy-2,1-ethanediyloxy[1,1'-biphenyl]-4',4-diyloxymethylene)]bis-oxirane, 4'-(2-oxiranemethyloxy)-[1,1'-biphenyl]-4-carboxylic acid 4,4'-(1,4-butanediyl) ester, 4,4'-biphenyl bisphenol diglycidyl ether, and 3,3'5,5'-tetramethylbiphenyl bisphenol diglycidyl ether.
4. A method for constructing a BN thermal conductive path metal-based liquid crystal epoxy copper clad laminate by screen printing according to claim 1, It is characterized in that S1 The surfactant includes at least one of 3-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane and urea.
5. A method for constructing a BN thermal conductive path metal-based liquid crystal epoxy copper clad laminate by screen printing according to claim 1, It is characterized in that S1 The curing agent includes at least one of 1-benzyl-2-methylimidazole, 2-heptadecylimidazole, and 2,4-diamino-6-(2-undecylimidazole-1-ethyl)-S-triazine.
6. A method for constructing a BN thermal conductive path metal-based liquid crystal epoxy copper clad laminate by screen printing according to claim 1, It is characterized in that S1 The organic solvent includes at least one of acetone, ethanol, tetrahydrofuran, dichloromethane and dichloroethane.
7. A method for constructing a BN thermal conductive path metal-based liquid crystal epoxy copper clad laminate by screen printing according to claim 2, It is characterized in that The gaps left in the pattern include dots, lines and grids.
8. A method for constructing a BN thermal conductive path metal-based liquid crystal epoxy copper clad laminate by screen printing according to claim 1, It is characterized in that The hot pressing in S3 is firstly maintained at 150-180°C for 2-3h, then heated to 170-200°C for 1-2h, then heated to 180-210°C for 0.5-1h, and finally cooled under pressure.
9. A method for constructing a BN thermal conductive path metal-based liquid crystal epoxy copper clad laminate by screen printing according to claim 1, It is characterized in that In S2, the thickness of the patterned thermally conductive insulating layer is 50-150 μm.
10. A BN thermal conductive path metal-based liquid crystal epoxy copper clad laminate prepared by the method according to any one of claims 1 to 9.