Substrate with embedded fine circuit and forming method thereof
By preparing a metal layer with wool on the carrier and embedded in the insulating medium, the problems of low yield of fine line processing and difficult to control the line width in the prior art are solved, and efficient fine line embedded processing is achieved, which improves the Processing quality and stability.
Patent Information
- Application Number
- CN202410945366.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-22
AI Technical Summary
In the prior art, in fine line processing of 15 μm or below, the instrument and process requirements are high, the yield is low, the line drilling and corrosion are severe, and the width is difficult to control, especially during the flash corrosion process, the corrosion on the side of the line is difficult to predict.
The first metal layer with hair teeth is used to prepare fine lines on the carrier and embedded them in the insulating medium. Conductive through holes and blind holes are formed by mechanical drilling and electroplating to achieve embedded processing of the lines and avoid flash corrosion. The impact of the process on the corrosion of the side of the line.
The yield of fine line processing is significantly improved, the requirements for exposure and flash corrosion uniformity are reduced, the width of the copper line is controlled, and the impurity electromigration problem that may be introduced by the semi-addition method is avoided.
Smart Images

Figure CN119012545A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of packaging substrates, and in particular to a substrate with embedded fine circuits and a forming method thereof. Background Art
[0002] At present, there are three main common circuit manufacturing processes for organic substrates: subtractive method, semi-additive method SAP, and modified semi-additive method MSAP. Generally, the subtractive method can be used to make substrates with line width and line spacing greater than 50μm, and the modified semi-additive method can be used to make substrates with line width and line spacing greater than 25μm. Fine lines with line width and line spacing less than 25μm can only be made by semi-additive method or low-cost semi-additive method proposed in Chinese patent CN103491732B.
[0003] The semi-additive method uses the chemical properties of the ABF material itself developed by Japan's Ajinomoto Co., Ltd. to achieve the processing of fine lines below 25μm through chemical copper plating, graphic electroplating and flash etching processes. The semi-additive method is the most commonly used process for fine line processing in the substrate industry. However, the semi-additive method for fine line processing of 15μm and below has extremely high requirements for instruments and processes. During the flash etching process, the bottom of the fine line is easily corroded by the solution, resulting in line drilling or disconnection. Therefore, the instrument uniformity, process accuracy and stability of exposure, copper plating and flash etching are extremely high. The semi-additive method has a low yield for fine line processing below 15μm, severe line drilling, and it is difficult to control the line width due to the unpredictable corrosion of the line side during the flash etching process.
[0004] The low-cost semi-additive method proposed in Chinese patent CN103491732B breaks through the limitation that only ABF materials can be used for processing fine lines below 25μm, and realizes the processing of fine lines below 25μm on the inner layer of the substrate and the surface of the added insulating dielectric PP material (prepreg). However, the low-cost semi-additive method also has the problem of difficult control of line width. Summary of the invention
[0005] In order to solve at least part of the above problems in the prior art, the present invention provides a method for forming a substrate with embedded fine circuits, comprising:
[0006] Laminating an adhesive layer and a first metal layer with a protective metal layer on both the front and back sides of the carrier;
[0007] forming a fine circuit on the surface of the first metal layer located on the front side or the back side of the carrier to obtain a carrier with the fine circuit;
[0008] Taking a core board substrate, and laminating an insulating layer on the front and back of the core board substrate, and laminating a carrier with fine circuits on the surface of the insulating layer on both sides of the core board substrate, wherein the fine circuits are embedded in the insulating layer after laminating;
[0009] separating the protective metal layer from the first metal layer; and
[0010] The first metal layer is removed to obtain a substrate with fine circuits.
[0011] Furthermore, it also includes forming a through hole penetrating the substrate by mechanical drilling, arranging metal on the inner wall of the through hole, and filling the through hole with a dielectric material to obtain a conductive through hole, wherein the conductive through hole is electrically connected to the fine line.
[0012] Furthermore, it also includes:
[0013] Arranging a build-up circuit structure on opposite sides of a substrate having fine circuits, wherein the build-up circuit structure includes an insulating layer and fine circuits embedded in the insulating layer; and
[0014] A blind hole is formed in the build-up circuit structure, and metal is filled in the blind hole by electroplating to obtain a conductive blind hole, wherein the conductive blind hole is electrically connected to the conductive through hole and the fine circuit.
[0015] Furthermore, a first metal layer with a protective metal layer is laminated on one side surface of the carrier, and the first metal layer is located on the outside, and the protective metal layer is bonded to the adhesive layer.
[0016] Furthermore, the first metal layer is a metal layer with roughness.
[0017] Furthermore, when the carrier with fine circuits is pressed onto the surfaces of the insulating layers on both sides of the core substrate, the two carriers need to be aligned.
[0018] Furthermore, the carrier alignment method includes a mechanical alignment bolt method and an optical alignment method, wherein the mechanical alignment bolt method includes: using a laser drill to drill holes in the core substrate and the two carriers, and using the mechanical alignment bolt method for alignment;
[0019] Optical alignment methods include:
[0020] One of the two carriers is selected to use the circuit pattern as a positioning mark, and a second mechanical drilling is performed to form a first through hole for standby use. On the other carrier, a circuit pattern positioning mark is reserved when making the circuit pattern;
[0021] On the core substrate, a second through hole is drilled using a mechanical drill, the size of the second through hole is larger than the size of the first through hole, and the relative position of the second through hole on the substrate is consistent with the relative position of the first through hole on the substrate;
[0022] Using the through hole of one carrier and the alignment mark of another carrier as the optical alignment target for alignment; and
[0023] After the alignment is completed, the edges and corners of the substrate are locally heat treated for pre-fixation, or automated equipment is used for automatic alignment, grabbing and pressing.
[0024] The present invention also provides a method for forming a substrate with embedded fine circuits, comprising:
[0025] Providing a basic substrate structure, the basic substrate structure comprising a core substrate, a conductive through hole, a first interconnect structure and a build-up circuit located on both sides of the core substrate, wherein the conductive through hole penetrates the core substrate and is electrically connected to the first interconnect structure;
[0026] Providing a carrier, and laminating an adhesive layer and a first metal layer with a protective metal layer on both the front and back sides of the carrier;
[0027] forming a fine circuit on the surface of the first metal layer located on the front side or the back side of the carrier to obtain a carrier with the fine circuit;
[0028] Laminating insulating layers on the front and back sides of the basic substrate structure, and laminating carriers with fine circuits on the surfaces of the insulating layers on both sides of the basic substrate structure, wherein the fine circuits are embedded in the insulating layers after lamination;
[0029] separating the protective metal layer from the first metal layer; and
[0030] The first metal layer is removed to obtain a substrate with fine circuits.
[0031] Further, the basic substrate structure is formed by a subtractive method or a semi-additive method;
[0032] The first metal layer is a metal layer with rough edges.
[0033] Furthermore, it also includes: forming a blind hole in the insulating layer, and filling metal in the blind hole by electroplating to obtain a conductive blind hole, wherein the conductive blind hole is electrically connected to the conductive through hole and the fine line.
[0034] The present invention also provides a substrate with embedded fine circuits, comprising:
[0035] Core board substrate;
[0036] An inner circuit structure is arranged on the front and back sides of the core substrate, the inner circuit structure comprising an insulating layer and a fine circuit embedded in the insulating layer; and
[0037] A conductive through hole penetrates the core substrate and the inner layer circuit structure.
[0038] Furthermore, it also includes:
[0039] One or more build-up wiring structures are arranged on the surface of the inner wiring structure, wherein the build-up wiring structure includes an insulating layer and fine wiring embedded in the insulating layer; and
[0040] A conductive blind hole penetrates the build-up circuit structure and is electrically connected to the inner circuit structure.
[0041] The present invention has at least the following beneficial effects: (1) The method of the present invention utilizes the characteristics of the first metal layer with burrs to prepare fine circuits on the surface of the first metal layer, and then transfers the fine circuits to the core substrate laminated with an insulating medium. The fine circuits are embedded in the insulating material. During the flash etching process, the flash etching solution has no corrosive effect on the sides of the circuits, which significantly improves the yield of fine circuit processing, reduces the requirements for dry film exposure machines and the requirements for uniformity of flash etching production lines, and the copper circuits do not require circuit drilling, so the width of the copper circuits can be controlled. (2) The fine circuit processing process does not involve copper plating processes, and palladium will not be introduced during the processing process, which reduces the probability of electromigration during substrate aging and avoids the problem of impurity electromigration that may be introduced by the semi-additive process (SAP). (3) The method of the present invention can realize fine circuit processing with a line width and line spacing of less than 25μm / 25μm for the inner layer and the added layer of the substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] In order to further illustrate the above and other advantages and features of various embodiments of the present invention, a more specific description of various embodiments of the present invention will be presented with reference to the accompanying drawings. It will be understood that these drawings only depict typical embodiments of the present invention and are therefore not to be considered as limiting the scope thereof. In the accompanying drawings, for clarity, identical or corresponding parts will be represented by identical or similar reference numerals.
[0043] Figures 1A to 1H A cross-sectional schematic diagram showing a process of manufacturing a substrate using a semi-additive method SAP based on ABF dielectric material;
[0044] Figures 2A to 2K A cross-sectional schematic diagram showing a process of manufacturing a substrate by a low-cost semi-additive method;
[0045] Figures 3A to 3I A cross-sectional schematic diagram showing a process of forming a substrate with embedded fine circuits according to an embodiment of the present invention;
[0046] Figure 4 A schematic cross-sectional view of a substrate with embedded fine circuits according to an embodiment of the present invention is shown; and
[0047] Figures 5A to 5H A cross-sectional schematic diagram shows a process of forming a substrate with embedded fine circuits according to another embodiment of the present invention. DETAILED DESCRIPTION
[0048] It should be noted that various components in the various drawings may be shown exaggeratedly for illustrative purposes and are not necessarily correct to scale.
[0049] In the present invention, each embodiment is only intended to illustrate the aspects of the present invention and should not be construed as limiting.
[0050] In the present invention, unless otherwise specified, the quantifiers "a", "an" and "an" do not exclude the presence of a plurality of elements.
[0051] It should also be pointed out that in the embodiments of the present invention, for the sake of clarity and simplicity, only a portion of the parts or components may be shown, but a person of ordinary skill in the art will understand that under the teachings of the present invention, required parts or components may be added as needed in specific scenarios.
[0052] It should also be pointed out that within the scope of the present invention, the terms "same", "equal", "equal to" and the like do not mean that the two values are absolutely equal, but allow a certain reasonable error, that is, the terms also cover "substantially the same", "substantially equal", and "substantially equal to".
[0053] It should also be pointed out that in the description of the present invention, the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than explicitly or implicitly indicating that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as explicitly or implicitly indicating relative importance.
[0054] In addition, the embodiments of the present invention describe the process steps in a specific order, but this is only for the convenience of distinguishing the steps, and does not limit the sequence of the steps. In different embodiments of the present invention, the sequence of the steps can be adjusted according to the adjustment of the process.
[0055] Figures 1A to 1H A cross-sectional schematic diagram shows a process of manufacturing a substrate using a semi-additive method (SAP) based on ABF dielectric material.
[0056] A semi-additive method based on ABF dielectric material includes the following steps:
[0057] Step 1, such as Figure 1AAs shown, an inner layer structure is provided, which includes a core board 101 , an inner layer metal 102 , and a through hole 103 , wherein the through hole 103 passes through the core board 101 , and the inner layer metal 102 is located on both sides of the core board 101 .
[0058] Step 2, such as Figure 1B As shown, ABF material 104 is pressed on both sides of the inner layer structure and pre-cured.
[0059] Step 3, such as Figure 1C As shown, a blind hole 105 is drilled in the ABF material 104 by laser to expose the inner metal 102 .
[0060] Step 4, such as Figure 1D As shown, a chemical copper plating process is performed on the surface of the ABF material 104 to form a chemical copper plating layer 106. The chemical copper plating process includes steps of fluffing, desmearing, neutralization, acid leaching, cleaning, micro-etching, pre-dipping, activation, reduction, and copper plating.
[0061] Step 5, such as Figure 1E As shown, a photoresist 107 is arranged on the surface of the chemical copper plating layer 106 and a circuit pattern 108 is formed by a photolithography process.
[0062] Step 6, such as Figure 1F As shown, metal is filled in the circuit pattern 108 through an electroplating process to form an electroplated metal pattern 109.
[0063] Step 7, such as Figure 1G As shown, the photoresist 107 is removed.
[0064] Step 8, such as Figure 1H As shown, the electroless copper layer 106 is removed by flash etching.
[0065] Repeat the above steps to achieve the processing of adding layers to the substrate.
[0066] The semi-additive method used for fine circuit processing of 15μm and below has extremely high requirements for instruments and processes. During the flash etching process, the bottom of the fine circuit is easily corroded by the solution, resulting in drilling or disconnection. Therefore, the uniformity of the instruments, process accuracy and stability of exposure, copper plating and flash etching are extremely high. The semi-additive method has low yield and severe drilling for fine circuit processing below 15μm. In addition, the corrosion of the side of the circuit during the flash etching process is difficult to predict, making it difficult to control the circuit width.
[0067] Figures 2A to 2K A cross-sectional schematic diagram showing a process of manufacturing a substrate using a low-cost semi-additive method.
[0068] A low-cost semi-additive method for making a substrate includes the following steps:
[0069] Step 1, such as Figure 2AAs shown, metallized vias 203 are made in the core board 201, and inner circuits 202 are made on the front and back sides of the core board 201. The inner circuits 202 of the package carrier are relatively wide and are usually completed by a subtractive method.
[0070] Step 2, such as Figure 2B As shown, a prepreg 204 and a copper foil 205 are laminated on the front and back sides of the core board 201, and the low-roughness structure on the surface of the copper foil is transferred to the prepreg.
[0071] Step 3, such as Figure 2C As shown, copper reduction: the copper foil 205 is thinned to 3um thickness. The purpose of this step is to reduce the etching amount of the copper electrode at the bottom of the blind hole during the surface copper removal process.
[0072] Step 4, such as Figure 2D As shown, laser drilling: a laser drilling machine is used to open a conducting blind hole 206 on the insulating prepreg 204. After subsequent metallization, the formed circuit is connected to the following circuit through the blind hole.
[0073] Step 5, such as Figure 2D As shown, after laser drilling, some resin will remain in the blind hole 206, and the slag will be removed by a desmearing process to improve the bonding strength of the chemically plated copper in the hole and the conductivity of the two-layer metal interconnection.
[0074] Step 6, such as Figure 2E As shown, the copper foil 205 is removed.
[0075] Step 7, such as Figure 2E As shown, plasma activation. The purpose of plasma activation is to treat the surface of the circuit board with plasma. On the one hand, it cleans the surface of the circuit board and removes the copper filling and the anti-oxidation stripping film on the surface of the prepreg. On the other hand, it activates the surface of the circuit board including the prepreg resin surface and the blind hole copper surface.
[0076] Step 8, such as Figure 2F As shown, chemical copper plating: chemical copper plating is performed on the prepreg 204 after the copper foil 205 is removed to form a chemical copper plating layer 207.
[0077] Step 9, such as Figure 2G As shown, photolithography: a photolithography layer 208 is formed on the surface of the chemical copper plating layer 207 and a portion of the photolithography layer 208 is removed through a photolithography process to form a circuit pattern 209, exposing the area that needs to be electroplated (exposing the blind holes and the chemical copper plating layer 207).
[0078] Step 10, such as Figure 2H As shown, electroplating: the photolithographic circuit board is placed in an electroplating tank, and copper is electroplated in the circuit pattern 209 and the blind hole 206 to obtain an electroplated copper layer 210.
[0079] Step 11, such as Fig.2I As shown, the photoresist layer 208 is removed.
[0080] Step 12, such as Figure 2J As shown, the chemically plated copper layer 207 is removed by flash etching.
[0081] Step 13, such as Figure 2K As shown, lower layer circuit processing: repeat steps 1-11 to form a more outer layer circuit.
[0082] The low-cost semi-additive method breaks through the limitation that only ABF materials can be used for fine circuit processing below 25μm, and realizes the processing of fine circuits below 25μm on the inner layer of the substrate and the surface of the added insulating medium PP material (prepreg). However, the low-cost semi-additive method also has the problem of difficult control of circuit width.
[0083] In view of the defects of the above existing methods, the present invention has developed a process method that can realize fine circuit substrates with line width and line spacing below 25μm with lower instrument and process requirements. Since the circuit has been buried in the ABF material during the flash etching process, the circuit processing yield is high, the circuit undercut is small, and the circuit width is controllable.
[0084] Figures 3A to 3I A cross-sectional schematic diagram shows a process of forming a substrate with embedded fine circuits according to an embodiment of the present invention.
[0085] A method for forming a substrate with embedded fine circuits comprises the following steps:
[0086] Step 1, such as Figure 3A As shown, the metal layers 402 on both sides of the core board 401 are removed to obtain a core board substrate as a carrier 403. The carrier can also be a plate-like structure such as a wafer, a glass material plate or a sapphire.
[0087] Step 2, such as Figure 3B As shown, an adhesive layer 404 and a first metal layer 406 with a protective metal layer 405 are pressed on both the front and back sides of the carrier 403. The first metal layer 406 is located on the outermost side, and the protective metal layer 405 is bonded to the adhesive layer 404. The adhesive layer 404 can be, for example, a temporary bonding adhesive, a prepreg, or other material with an adhesive function.
[0088] The first metal layer 406 is preferably a 3μm copper foil. Due to its thin thickness, the 3μm copper foil will be attached with an 18μm protective copper foil (protective metal layer). During lamination, the 3μm copper foil with the rough edges faces outwards, and the protective copper foil faces inwards to contact the temporary bonding adhesive.
[0089] The advantages of using 3μm copper foil are as follows: the bonding force between 3μm and 18μm copper foil is appropriate (it can withstand the process in chemical solution and can be separated smoothly from the middle); the 3μm copper foil surface has "tooth", and the dry film after exposure can stand up by using the bonding force provided by the tooth. Here, 3μm copper foil is used as an example for detailed introduction. The thickness is not limited to 3μm, as long as the first metal layer is a metal layer with tooth, and the thickness of the protective metal layer is not limited.
[0090] Step 3, such as Figure 3C As shown, a dry film is laminated on the surface of the first metal layer 406 on the front or back side of the carrier, and after exposure, development, electroplating, and film stripping, a fine circuit 407 is obtained on the surface of the first metal layer 406, thereby obtaining a carrier with a fine circuit.
[0091] The dry film lamination is to attach an anti-corrosion film, such as an anti-corrosion dry film, to the surface of the first metal layer 406;
[0092] Exposure is to transfer the circuit pattern on the mask to the resist film using ultraviolet rays emitted by the exposure machine;
[0093] The development is to use a developer to remove the resist film that has not undergone photopolymerization reaction, and the remaining resist film defines a circuit pattern on the surface of the first metal layer 406;
[0094] Electroplating is to fill metal in the circuit pattern through the electroplating process to obtain fine circuit 407;
[0095] Stripping is the process of removing the resist film using a chemical solution.
[0096] Step 4, such as Figure 3D As shown, a core board substrate 408 is taken, and an insulating layer 409 is laminated on the front and back sides of the core board substrate 408 , and a carrier 403 with fine circuits is laminated on the surface of the insulating layer 409 on both sides of the core board substrate 408 , wherein the fine circuit 407 is embedded in the insulating layer 409 after lamination.
[0097] In one embodiment of the present invention, the insulating layer 409 is preferably made of ABF material, and the PET film on the surface of the ABF material is removed after lamination.
[0098] In the step of laminating a carrier with fine lines, two carriers need to be aligned. The methods that can be adopted include but are not limited to the following two:
[0099] 1. Alignment bolts: Use a laser drill to drill holes in the core board substrate and the two carriers, and use mechanical alignment bolts for alignment.
[0100] 2. Optical alignment: Of the two carriers, select one with the circuit pattern as the alignment mark, and perform a second mechanical drill to form the first through hole for standby use (carrier 1). On the other carrier, reserve the circuit pattern alignment mark when making the circuit pattern (carrier 2). On the core board substrate where the pattern is finally left, use a mechanical drill to open a second through hole of a larger size. The size of the second through hole is larger than the size of the first through hole, and the relative position of the second through hole on the substrate is consistent with the relative position of the first through hole on the substrate. Use the through hole of carrier 1 and the alignment mark of carrier 2 as optical alignment targets for alignment. After the alignment is completed, perform local heat treatment on the edges and corners of the substrate for pre-fixation, or use automated equipment for automatic alignment grabbing and pressing.
[0101] Step 5, such as Figure 3E As shown, the protective metal layer 405 and the first metal layer 406 are separated, and the fine line 407 is transferred to the insulating layer 409 of the core substrate 408.
[0102] Step 6, such as Figure 3F As shown, the first metal layer 406 is removed by flash etching to obtain a substrate 410 with fine circuits. The fine circuits 407 are embedded in the insulating layer 409. During the flash etching, the fine circuits are already buried in the insulating medium, so the fine circuit processing yield is high, the circuit erosion is small, and the circuit width is controllable.
[0103] Step 7, such as Figure 3G As shown, a through hole penetrating the substrate 410 is formed by mechanical drilling, a metal is arranged on the inner wall of the through hole, and a dielectric material is filled in the through hole to obtain a conductive through hole 411. The dielectric material can be a resin. The conductive through hole 411 is electrically connected to the fine line 407.
[0104] Step 8, such as Figure 3H As shown, steps 1-6 are repeated to form a build-up circuit structure 412 on both sides of the substrate 410. The build-up circuit structure 412 includes an insulating layer and fine circuits embedded in the insulating layer.
[0105] Step 9, such as Fig. 3I As shown, a blind hole is formed in the build-up circuit structure 412 by laser drilling, and metal is filled in the blind hole by electroplating to obtain a conductive blind hole 413, and the conductive blind hole 413 is electrically connected to the conductive through hole 411 or the fine circuit 407, and the conductive blind hole 413 is electrically connected to the circuit structure in the build-up circuit structure 412 to achieve upper and lower layer connection.
[0106] Repeat steps 1-6 and laser drilling to make build-up circuits.
[0107] The present invention utilizes the above two characteristics of 3 μm copper foil, firstly processes fine circuits on a carrier core board laminated with 3 μm copper foil, and then "transfers" the fine circuits to a substrate laminated with a build-up insulating medium.
[0108] Figure 4 A cross-sectional schematic diagram of a substrate with embedded fine circuits according to an embodiment of the present invention is shown.
[0109] like Figure 4 As shown, a substrate with embedded fine circuits includes: a core substrate 501, an inner layer circuit structure 502, a conductive through hole 503, a build-up layer circuit structure 504 and a conductive blind hole 505.
[0110] The inner circuit structure 502 is arranged on the front and back sides of the core substrate 501 , and the inner circuit structure 502 includes an insulating layer 5021 and a fine circuit 5022 embedded in the insulating layer 5021 .
[0111] The conductive via 503 penetrates the core substrate 501 and the inner layer circuit structure 502 .
[0112] One or more build-up circuit structures 504 are sequentially arranged on the surface of the inner circuit structure 502 , wherein the build-up circuit structure 504 includes an insulating layer 5041 and a fine circuit 5042 embedded in the insulating layer 5041 .
[0113] The conductive blind via 505 penetrates the build-up circuit structure 504 and is electrically connected to the inner circuit structure 502 .
[0114] Figures 5A to 5H A cross-sectional schematic diagram shows a process of forming a substrate with embedded fine circuits according to another embodiment of the present invention.
[0115] In order to adapt to the pin size and spacing of the chip during the micro-assembly process, the packaging substrate design has high requirements for the wiring density of the top layer. In actual design and production, in order to take into account the processing cost, the embedded fine line processing method of the present invention can be used in the circuit layer with ultra-fine line requirements, while the conventional circuit structure (non-embedded) and processing method (subtractive method, semi-additive method, etc.) are used in other layers. The specific steps are as follows:
[0116] Step 1, such as Figure 5A As shown, a basic substrate structure 300 is provided, wherein the basic substrate structure 300 includes a core substrate 301, a conductive through hole 302, a first interconnect structure 303 located on both sides of the core substrate 301, and a build-up circuit 304. The first interconnect structure 303 includes an insulating layer and a circuit located in the insulating layer. The conductive through hole 302 penetrates the core substrate 301 and is electrically connected to the first interconnect structure 303. The build-up circuit 304 is electrically connected to the first interconnect structure 303 through a conductive blind hole.
[0117] The basic substrate structure is manufactured by a subtractive method or a semi-additive method.
[0118] Step 2, such as Figure 5B As shown, the metal layers 602 on both sides of the core board 601 are removed to obtain a core board substrate as a carrier 603. The carrier can also be a plate-like structure such as a wafer, a glass material plate or a sapphire.
[0119] Step 3, such as Figure 5C As shown, an adhesive layer 604 and a first metal layer 606 with a protective metal layer 605 are pressed on both the front and back sides of the carrier 603. The first metal layer 606 is located on the outermost side, and the protective metal layer 605 is bonded to the adhesive layer 604. The adhesive layer 604 can be, for example, a temporary bonding adhesive, a prepreg, or other material with an adhesive function.
[0120] The first metal layer 606 is preferably a 3μm copper foil. Due to its thin thickness, the 3μm copper foil will be attached with an 18μm protective copper foil (protective metal layer). During lamination, the 3μm copper foil with the rough edges faces outwards, and the protective copper foil faces inwards to contact the temporary bonding adhesive.
[0121] The advantages of using 3μm copper foil are as follows: the bonding force between 3μm and 18μm copper foil is appropriate (it can withstand the process in chemical solution and can be separated smoothly from the middle); the 3μm copper foil surface has "tooth", and the dry film after exposure can stand up by using the bonding force provided by the tooth. Here, 3μm copper foil is used as an example for detailed introduction. The thickness is not limited to 3μm, as long as the first metal layer is a metal layer with tooth, and the thickness of the protective metal layer is not limited.
[0122] Step 4, such as Figure 5D As shown, a dry film is laminated on the surface of the first metal layer 606 on the front or back side of the carrier, and after exposure, development, electroplating, and film stripping, a fine circuit 607 is obtained on the surface of the first metal layer 606, thereby obtaining a carrier with a fine circuit.
[0123] The dry film lamination is to attach a resist film, such as a resist dry film, to the surface of the first metal layer 606;
[0124] Exposure is to transfer the circuit pattern on the mask to the resist film using ultraviolet rays emitted by the exposure machine;
[0125] Development is to use a developer to remove the resist film that has not undergone photopolymerization reaction, and the remaining resist film defines a circuit pattern on the surface of the first metal layer 606;
[0126] Electroplating is to fill metal in the circuit pattern through the electroplating process to obtain fine circuit 607;
[0127] Stripping is the process of removing the resist film using a chemical solution.
[0128] Step 5, such as Figure 5EAs shown, an insulating layer 608 is laminated on the front and back sides of the basic substrate structure 300 , and a carrier 603 with fine circuits 607 is laminated on the surface of the insulating layer 608 on both sides of the basic substrate structure 300 , wherein the fine circuits 607 are embedded in the insulating layer 608 after lamination.
[0129] In one embodiment of the present invention, the insulating layer 608 is preferably made of ABF material, and the PET film on the surface of the ABF material is removed after lamination. The insulating layer 608 can also be PP, polyimide PI, polyvinyl formal PVF and other common insulating media in the field of various packaging substrates.
[0130] Step 6, such as Fig. 5F As shown, the protective metal layer 605 and the first metal layer 606 are separated, and the fine lines 607 are transferred to the insulating layer 608 on both sides of the basic substrate structure 300 .
[0131] Step 7, such as Figure 5G As shown, the first metal layer 606 is removed by flash etching to obtain a substrate with fine lines 607. The fine lines 607 are embedded in the insulating layer 608. During the flash etching, the fine lines are already buried in the insulating medium, so the fine lines have a high processing yield, small line erosion, and controllable line width.
[0132] Step 8, such as Figure 5H As shown, a blind hole penetrating the insulating layer 608 is formed by laser drilling, and metal is arranged in the blind hole to obtain a conductive blind hole 609. The conductive blind hole 609 is electrically connected to the fine line 607 and the inner layer line 304.
[0133] Repeat steps 2-8 to form a build-up circuit structure on both sides of the substrate. The build-up circuit structure includes an insulating layer and a fine circuit embedded in the insulating layer.
[0134] The present invention designs a substrate structure in which fine circuits are embedded in dielectric materials, and develops a process method that can realize a fine circuit substrate with a line width and line spacing of less than 25μm with lower instrument and process requirements. Since the circuits are already buried in the ABF material during the flash etching process, the circuit processing yield is high, the circuit drilling is small, and the circuit width is controllable.
[0135] The ETS (Embedded Trace Substrate) substrate is a coreless packaging substrate with embedded copper wires. However, the present invention and the ETS substrate have the following essential differences in structure, use and substrate material:
[0136] From a structural point of view, the embedded fine circuit substrate of the present invention is a core substrate, while the ETS substrate is a coreless packaging substrate. The embedded fine circuit substrate of the present invention has no limit on the number of layers, but due to the need for thinness and the serious warping problem caused by the increase in the number of layers, the ETS substrate is usually 2-4 layers.
[0137] From the perspective of usage, the present invention is mainly used for processing ultra-fine circuits, reducing the processing cost of fine circuits with a line width and line spacing below 15μm, improving the yield, breaking through the processing limit of the conventional method (SAP) of the equipment, and improving the wiring density of the packaging substrate. Since the ETS substrate has no core board, the thickness of the core board is saved (the conventional thickness is 0.1-1.8mm), and it is mainly used to meet the ultra-thin requirements of the packaging structure.
[0138] From the material point of view, the insulating medium of the present invention can be ABF, PP, polyimide PI, polyvinyl formal PVF and other common insulating media in the field of various packaging substrates. However, since the ETS substrate does not have a core board, the glass fiber in the PP material is required to provide the necessary rigidity and mechanical strength, and only the PP material can be used as the insulating medium. At the same time, since the ETS substrate does not have a core board, even if PP is used as the insulating medium, there are still problems of poor mechanical strength and severe warping. In the present invention, the front and back refer to two opposite surfaces, and do not specifically refer to which side is the front and which side is the back.
[0139] Although some embodiments of the present invention have been described in this application document, it will be appreciated by those skilled in the art that these embodiments are merely shown as examples. Those skilled in the art may conceive of numerous variations, alternatives, and improvements under the teachings of the present invention without departing from the scope of the present invention. The appended claims are intended to define the scope of the present invention and to cover methods and structures within the scope of these claims themselves and their equivalents.
Claims
1. A method for forming a substrate with embedded fine circuits, characterized in that: include: Laminating an adhesive layer and a first metal layer with a protective metal layer on both the front and back sides of the carrier; forming a fine circuit on the surface of the first metal layer located on the front side or the back side of the carrier to obtain a carrier with the fine circuit; Taking a core board substrate, and laminating an insulating layer on the front and back of the core board substrate, and laminating a carrier with fine circuits on the surface of the insulating layer on both sides of the core board substrate, wherein the fine circuits are embedded in the insulating layer after laminating; separating the protective metal layer from the first metal layer; as well as The first metal layer is removed to obtain a substrate with fine circuits.
2. The method according to claim 1, characterized in that: The method also includes forming a through hole penetrating the substrate by mechanical drilling, arranging metal on the inner wall of the through hole, and filling the through hole with a dielectric material to obtain a conductive through hole, wherein the conductive through hole is electrically connected to the fine line.
3. The method according to claim 2, characterized in that Also includes: Arranging a build-up circuit structure on opposite sides of a substrate having fine circuits, wherein the build-up circuit structure includes an insulating layer and fine circuits embedded in the insulating layer; as well as A blind hole is formed in the build-up circuit structure, and metal is filled in the blind hole by electroplating to obtain a conductive blind hole, wherein the conductive blind hole is electrically connected to the conductive through hole and the fine circuit.
4. The method according to claim 1, characterized in that: The first metal layer with the protective metal layer is pressed on one side surface of the carrier, and the first metal layer is located on the outside, and the protective metal layer is bonded to the bonding layer.
5. The method according to any one of claims 1 to 4, characterized in that: The first metal layer is a metal layer with rough edges.
6. The method according to any one of claims 1 to 4, characterized in that: When the carrier with fine circuits is pressed onto the surfaces of the insulating layers on both sides of the core substrate, the two carriers need to be aligned.
7. The method according to claim 6, characterized in that The carrier alignment method includes a mechanical alignment bolt method and an optical alignment method, wherein the mechanical alignment bolt method includes: using a laser drill to drill holes on the core substrate and the two carriers, and using the mechanical alignment bolt method for alignment; Optical alignment methods include: One of the two carriers is selected to use the circuit pattern as a positioning mark, and a second mechanical drilling is performed to form a first through hole for standby use. On the other carrier, a circuit pattern positioning mark is reserved when making the circuit pattern; On the core substrate, a second through hole is drilled using a mechanical drill, the size of the second through hole is larger than the size of the first through hole, and the relative position of the second through hole on the substrate is consistent with the relative position of the first through hole on the substrate; Using the through hole of one carrier and the alignment mark of another carrier as the optical alignment target for alignment; and After the alignment is completed, the edges and corners of the substrate are locally heat treated for pre-fixation, or automated equipment is used for automatic alignment, grabbing and pressing.
8. A method for forming a substrate with embedded fine circuits, characterized in that: include: Providing a basic substrate structure, the basic substrate structure comprising a core substrate, a conductive through hole, a first interconnect structure and a build-up circuit located on both sides of the core substrate, wherein the conductive through hole penetrates the core substrate and is electrically connected to the first interconnect structure; Providing a carrier, and laminating an adhesive layer and a first metal layer with a protective metal layer on both the front and back sides of the carrier; forming a fine circuit on the surface of the first metal layer located on the front side or the back side of the carrier to obtain a carrier with the fine circuit; Laminating insulating layers on the front and back sides of the basic substrate structure, and laminating carriers with fine circuits on the surfaces of the insulating layers on both sides of the basic substrate structure, wherein the fine circuits are embedded in the insulating layers after lamination; separating the protective metal layer from the first metal layer; as well as The first metal layer is removed to obtain a substrate with fine circuits.
9. The method according to claim 8, characterized in that The basic substrate structure is formed by a subtractive process or a semi-additive process; The first metal layer is a metal layer with rough edges.
10. The method according to claim 8, characterized in that Also includes: A blind hole is formed in the insulating layer, and metal is filled in the blind hole by electroplating to obtain a conductive blind hole, wherein the conductive blind hole is electrically connected to the conductive through hole and the fine line.
11. A substrate with embedded fine circuits, characterized in that: include: Core board substrate; An inner circuit structure is arranged on the front and back sides of the core substrate, and the inner circuit structure includes an insulating layer and a fine circuit embedded in the insulating layer; as well as A conductive through hole penetrates the core substrate and the inner layer circuit structure.
12. The substrate according to claim 11, characterized in that Also includes: One or more build-up circuit structures are arranged on the surface of the inner circuit structure, wherein the build-up circuit structure includes an insulating layer and fine circuits embedded in the insulating layer; as well as A conductive blind hole penetrates the build-up circuit structure and is electrically connected to the inner circuit structure.
Citation Information
Cited By
Manufacturing method of double-sided wire-embedded printed circuit board
CN120935937A
A manufacturing method of a double-sided buried wire printed circuit board
CN120935937B
Manufacturing method based on ETS process lead etching-back and packaging substrate
CN121843537A
A manufacturing method based on ETS process lead etching back and packaging substrate
CN121843537B
Housing, electronic device, and method for manufacturing housing
WO2026113575A1