Metal halide perovskite solar cell and preparation method thereof
By using thiol acid as the intermediate layer in the preparation of perovskite film, the problems of poor repeatability and high defect density in the preparation of perovskite solar cells are solved, the stability of the film and the photoelectric conversion efficiency are improved, and the perovskite solar energy is promoted. Commercial application of batteries.
Patent Information
- Application Number
- CN202411245682.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-22
AI Technical Summary
In the existing perovskite solar cell preparation methods, the solution method has problems such as poor repeatability and high defect density, resulting in low perovskite film stability and photoelectric conversion efficiency.
During the preparation of perovskite film, thiol acid is added as the intermediate layer. The carboxylic groups of thiol acid inhibit the deprotonation of FA and form a strong coordination bond with Pb2+ in the lead iodide layer, reducing defect density and improving calcium The quality of titanium-ite film.
It improves the stability and photoelectric conversion efficiency of perovskite films, simplifies the process, enhances the repetition of preparation, and lays the foundation for the commercial application of perovskite solar cells.
Smart Images

Figure CN119012882A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solar cells, and in particular to a metal halide perovskite solar cell and a preparation method thereof. Background Art
[0002] In recent years, perovskite solar cells have developed rapidly as the third generation of solar cells. The photoelectric conversion efficiency of laboratory single-junction cells has exceeded 26%, which is comparable to that of crystalline silicon cells. Due to its low raw material cost, simple preparation process, and ability to be prepared on large areas and flexible substrates, it has great research value and commercial application potential.
[0003] At present, the preparation of perovskite solar cells mostly adopts the solution method. The most commonly used solution methods are the one-step method and the two-step method. The one-step method is to dissolve lead iodide and organic salts such as iodoformamide in an organic solvent according to a certain molar ratio, and then apply it on the hole transport layer or electron transport layer as a perovskite precursor solution, and directly form a perovskite light-absorbing layer after annealing; the two-step method is to first apply the lead iodide solution, form a lead iodide film after annealing, and then apply the organic salt solution on the lead iodide film, and form a perovskite film after annealing. Both have their advantages and disadvantages. The one-step method is simple to operate, but the repeatability is poor; the two-step method has high repeatability, but it is easy to have many under-coordinated Pb 2+ , which leads to an increase in defect density, affecting the transport and recombination of carriers. At the same time, the organic precursor solution also has a deprotonation problem. The stability of the prepared perovskite film decreases significantly over time.
[0004] Therefore, inventing an efficient and stable method for preparing perovskite thin films is of great significance for the two-step preparation of perovskite solar cells and subsequent industrial production. Summary of the invention
[0005] Based on the above content, the present invention provides a metal halide perovskite solar cell and a preparation method thereof. In the present invention, mercapto acid is added as an intermediate layer in the preparation process of the perovskite film, so that the carboxyl group in the mercapto acid can coordinate with I- in the organic precursor film to inhibit the deprotonation process of FA, and at the same time, the mercapto group in the mercapto acid can coordinate with the under-coordinated Pb in the lead iodide layer. 2+ Strong coordination bonds are formed, defect density is reduced, and the quality of perovskite films is improved, thereby preparing efficient and stable perovskite solar cells.
[0006] To achieve the above object, the present invention provides the following solutions:
[0007] One of the technical solutions of the present invention is a method for preparing a perovskite film, comprising the following steps:
[0008] coating a mercapto acid solution on the lead iodide film to prepare a mercapto acid intermediate layer;
[0009] coating an organic precursor solution on the mercapto acid intermediate layer, and then annealing to obtain the perovskite film;
[0010] The solute in the mercapto acid solution is one or more of 3-mercaptoisobutyric acid, 4-mercaptobutyric acid, and 4-mercapto-4-methylpentanoic acid, and the solvent is one of benzyl alcohol, ethanol, and isopropanol;
[0011] The solute in the organic precursor solution is one or more of iodoformamidine, iodomethylamine, chloromethylamine, and bromomethylamine, and the solvent is ethanol or isopropanol.
[0012] A second technical solution of the present invention is a perovskite film prepared according to the above-mentioned preparation method.
[0013] A third technical solution of the present invention is the use of the above-mentioned perovskite film in the preparation of perovskite solar cells.
[0014] A fourth technical solution of the present invention is a perovskite solar cell, comprising the above-mentioned perovskite film.
[0015] A fifth technical solution of the present invention is a method for preparing the above-mentioned perovskite solar cell. When the perovskite solar cell is a formal structure, the preparation method comprises the following steps:
[0016] preparing an electron transport layer on the surface of the substrate;
[0017] Preparing a perovskite light absorbing layer on the surface of the electron transport layer;
[0018] preparing a hole transport layer on the surface of the perovskite light absorbing layer;
[0019] Prepare an electrode on the surface of the hole transport layer to obtain the perovskite solar cell;
[0020] When the perovskite solar cell is an inverted structure, the preparation method comprises the following steps:
[0021] preparing a hole transport layer on the surface of the substrate;
[0022] Preparing a perovskite light absorbing layer on the surface of the hole transport layer;
[0023] preparing an electron transport layer on the surface of the perovskite light absorbing layer;
[0024] An electrode is prepared on the surface of the electron transport layer to obtain the perovskite solar cell.
[0025] The present invention discloses the following technical effects:
[0026] (1) The present invention provides a method for preparing a perovskite film. Mercapto acid can effectively inhibit the deprotonation process of FA in the organic precursor film, thereby improving the stability of the perovskite film. Mercapto acid can effectively solve the problem of partial Pb 2+ The uncoordinated state improves the crystallization quality of the perovskite film and thus improves the photoelectric conversion efficiency of the perovskite solar cell.
[0027] (2) The method of the present invention has a simple process and strong repeatability, and is applicable to both regular structure and inverted structure perovskite solar cells, laying a foundation for the commercial application of perovskite solar cells. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0029] Figure 1 This is a flow chart of the two-step method for preparing perovskite thin films in the present invention;
[0030] Figure 2 This is a structural diagram of the formal perovskite solar cell device prepared in Example 1;
[0031] Figure 3 This is a structural diagram of the inverted perovskite solar cell device prepared in Example 2;
[0032] Figure 4 This is a structural diagram of the flexible perovskite solar cell device prepared in Example 5;
[0033] Figure 5 This is a cross-sectional SEM image of the perovskite solar cell device prepared in Example 1;
[0034] Figure 6 This is a surface SEM image of the perovskite film prepared by the two-step method in Example 1;
[0035] Figure 7 The efficiency curves of the perovskite solar cells prepared in Example 1 and Comparative Example 1 are shown;
[0036] Figure 8 The maximum efficiency and storage time of the perovskite solar cells prepared in Example 3 and Comparative Example 1 are shown;
[0037] Fig. 9 This is an efficiency curve diagram of the perovskite solar cell prepared in Example 2;
[0038] Fig.10 This is an efficiency curve diagram of the perovskite solar cell prepared in Example 4;
[0039] Fig.11 This is the efficiency curve of the perovskite solar cell prepared in Example 5. DETAILED DESCRIPTION
[0040] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0041] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0042] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0043] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0044] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0045] A first aspect of the present invention provides a method for preparing a perovskite film, comprising the following steps:
[0046] coating a mercapto acid solution on the lead iodide film to prepare a mercapto acid intermediate layer;
[0047] coating an organic precursor solution on the mercapto acid intermediate layer, and then annealing to obtain the perovskite film;
[0048] The solute in the mercapto acid solution is one or more of 3-mercaptoisobutyric acid, 4-mercaptobutyric acid, and 4-mercapto-4-methylpentanoic acid, and the solvent is one of benzyl alcohol, ethanol, and isopropanol;
[0049] The solute in the organic precursor solution is one or more of iodoformamidine, iodomethylamine, chloromethylamine, and bromomethylamine, and the solvent is ethanol or isopropanol.
[0050] In some embodiments of the present invention, the concentration of the mercapto acid solution is 0.5 to 2 mg / mL.
[0051] The concentration of the organic precursor solution is 0.3 mmol / mL to 0.6 mmol / mL.
[0052] Too high or too low a concentration of the organic precursor solution will result in poor quality perovskite films, thereby affecting device efficiency. Therefore, the present invention preferably limits the concentration of the organic precursor solution to 0.3 mmol / mL to 0.6 mmol / mL.
[0053] The annealing temperature is 120-180° C. and the annealing time is 10-30 minutes.
[0054] In some embodiments of the present invention, the lead iodide thin film is prepared by coating a lead iodide precursor solution on a substrate and annealing at 50 to 100° C. for 30 seconds to 3 minutes;
[0055] The solute in the lead iodide precursor solution is lead iodide, and the solvent is at least one of N,N-dimethylformamide, N-methylpyrrolidone, dimethyl sulfoxide, etc.;
[0056] The concentration of the lead iodide precursor solution is 1.0 mmol / mL to 2.0 mmol / mL.
[0057] The thickness of the lead iodide film is 300-450nm.
[0058] The thickness of the mercapto acid intermediate layer is 20 to 60 nm.
[0059] The thickness of the perovskite film is 500-800nm.
[0060] The reasons why the present invention limits the thickness of the lead iodide film, the mercapto acid intermediate layer, and the perovskite film to the above parameter range are as follows: the lead iodide film also determines the thickness of the perovskite film to a certain extent. If the lead iodide film is too thin, part of the organic precursor solution will not react completely after spin coating. If the lead iodide film is too thick, the lead iodide content in the perovskite film formed by the final annealing will be too high. Both situations will affect the efficiency of the final device. The perovskite film needs to be maintained at an appropriate thickness so that it can have better light absorption ability as a light-absorbing layer, thereby improving the final efficiency of the device. The mercapto acid intermediate layer plays a role of passivation and anchoring as an intermediate layer. If it is too thin, its effect will be negligible. If it is too thick, physical barriers will exist in the perovskite film. After the lead iodide layer and the organic precursor solution are reacted and annealed, a more suitable perovskite structure cannot be formed.
[0061] A second aspect of the present invention provides a perovskite film prepared according to the above preparation method.
[0062] A third aspect of the present invention provides an application of the above-mentioned perovskite film in the preparation of a perovskite solar cell.
[0063] A fourth aspect of the present invention provides a perovskite solar cell, comprising the above-mentioned perovskite film.
[0064] In some embodiments of the present invention, the perovskite solar cell is a regular structure or an inverted structure;
[0065] When the perovskite solar cell is a formal structure, it includes a substrate, an electron transport layer, a perovskite light absorption layer, a hole transport layer and an electrode arranged in sequence from bottom to top;
[0066] When the perovskite solar cell is an inverted structure, it includes a substrate, a hole transport layer, a perovskite light absorption layer, an electron transport layer and an electrode arranged in sequence from bottom to top;
[0067] The perovskite light absorbing layer is the above-mentioned perovskite film.
[0068] When the perovskite solar cell is of an inverted structure, a buffer layer is further provided between the electron transport layer and the electrode.
[0069] In some embodiments of the present invention, the substrate is a rigid conductive substrate or a flexible conductive substrate;
[0070] The rigid conductive substrate is a flat glass on which a conductive film is coated, and the conductive film includes FTO or ITO;
[0071] The flexible conductive substrate is one of PEN, PVA and PT;
[0072] The electron transport layer is tin oxide, titanium oxide, PCBM, BCP, C60 One of;
[0073] The hole transport layer is one of Spiro-OMeTAD, PEDOT:PSS, nickel oxide, and molybdenum oxide;
[0074] The electrode is one of gold, silver, copper and carbon.
[0075] The thickness of the electron transport layer is 30-80 nm.
[0076] The thickness of the hole transport layer is 20-90 nm.
[0077] The electrode is in the form of a thin film; the thickness of the electrode is 70-120 nm.
[0078] The reasons why the present invention limits the thickness of the electron transport layer, the hole transport layer, and the electrode to the above parameter range are as follows: if the thickness of the electron transport layer is too thick, it will cause recombination of carriers, increase the defects in the layer, affect charge extraction and transport, and thus affect the efficiency of the device; if the thickness of the electron transport layer is too thin, it will affect the electron transport capacity; the same is true for the hole transport layer; the resistance of the electrode decreases with increasing thickness, and the electrode structure affects the performance of the battery by affecting the series resistance of the battery. When the electrode thickness is within the above parameter range, the battery performance is optimal.
[0079] A fifth aspect of the present invention provides a method for preparing the above-mentioned perovskite solar cell. When the perovskite solar cell is a formal structure, the preparation method comprises the following steps:
[0080] preparing an electron transport layer on the surface of the substrate;
[0081] Preparing a perovskite light absorbing layer on the surface of the electron transport layer;
[0082] preparing a hole transport layer on the surface of the perovskite light absorbing layer;
[0083] Prepare an electrode on the surface of the hole transport layer to obtain the perovskite solar cell;
[0084] When the perovskite solar cell is an inverted structure, the preparation method comprises the following steps:
[0085] preparing a hole transport layer on the surface of the substrate;
[0086] Preparing a perovskite light absorbing layer on the surface of the hole transport layer;
[0087] preparing an electron transport layer on the surface of the perovskite light absorbing layer;
[0088] An electrode is prepared on the surface of the electron transport layer to obtain the perovskite solar cell.
[0089] In some embodiments of the present invention, the preparation method of the electron transport layer is any one of spin coating, chemical bath, and scraping; the preparation method of the air transport layer is any one of spin coating, chemical bath, scraping, and sputtering; the preparation method of the electrode is any one of evaporation, sputtering, and scraping.
[0090] The above steps are all carried out under nitrogen, argon or dry air atmosphere with humidity below 40%.
[0091] The English names of the compounds involved in the present invention have the following meanings:
[0092] DMF: N,N-dimethylformamide
[0093] DMSO: dimethyl sulfoxide
[0094] IPA: Isopropyl alcohol
[0095] Spiro-OMeTAD: 2,2',7,7'-Tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene
[0096] TBP: 4-tert-butylpyridine
[0097] PCBM: Phenyl-C61-butyric acid methyl ester
[0098] BCP: Bathcopper
[0099] NMP: N-methylpyrrolidone
[0100] The technical solutions described in the present invention, unless otherwise specified, are all conventional solutions in the art, and the reagents or raw materials used, unless otherwise specified, are purchased from commercial channels or have been disclosed.
[0101] The TBP solution (4-tert-butylpyridine solution) used in the examples of the present invention was directly purchased and had a purity of 96%.
[0102] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0103] Example 1
[0104] Step 1: Prepare a SnO2 electron transport layer on a FTO conductive substrate by chemical bath deposition, and anneal it in air at 170°C for 25 minutes to obtain an electron transport layer with a thickness of 60 nm.
[0105] Step 2: Dissolve 642.4 mg of lead iodide in 1 mL of a mixed solvent of DMF and DMSO (solvent volume ratio DMF:DMSO=9:1) to prepare a lead iodide precursor solution, which is then spin-coated on the electron transport layer and annealed in nitrogen at 60°C for 2 min to prepare a lead iodide film with a thickness of 320 nm.
[0106] Step 3: Dissolve 0.5 mg, 1 mg, and 2 mg of 3-mercaptoisobutyric acid in 1 mL of IPA solvent to prepare mercapto acid solutions with concentrations of 0.5 mg / mL, 1 mg / mL, and 2 mg / mL, respectively. Then, spin-coat the mercapto acid solutions of different concentrations on the lead iodide film to prepare a mercapto acid intermediate layer with a thickness of 20 nm.
[0107] Step 4: Dissolve 80 mg of iodoformamide and 17 mg of chloromethylamine in 1 mL of IPA solvent to prepare an organic precursor solution, which is then spin-coated on the mercapto acid intermediate layer and annealed at 130° C. for 15 min in nitrogen to prepare a perovskite film with a thickness of 630 nm.
[0108] Step 5: Dissolve 73.2 mg of Spiro-OMeTAD in 1 mL of chlorobenzene to prepare a spiro-OMeTAD solution. Dissolve 520 mg of lithium bis(trifluoromethanesulfonyl)amide in 1 mL of anhydrous acetonitrile to obtain a lithium bis(trifluoromethanesulfonyl)amide solution, and add 17.6 μL of lithium bis(trifluoromethanesulfonyl)amide solution and 28.8 μL of TBP solution to the above spiro-OMeTAD solution to prepare a hole transport layer precursor solution. Spin coat the hole transport layer precursor solution on the perovskite film to prepare a hole transport layer with a thickness of 80 nm.
[0109] Step 6: The thin film prepared above is subjected to thermal evaporation process to deposit a metal electrode Au with a thickness of 110 nm to prepare a formal perovskite solar cell.
[0110] Example 2
[0111] Step 1: Preparation of NiO on FTO conductive substrate by magnetron sputtering x The film is used to prepare a hole transport layer.
[0112] Step 2: 605.3 mg of lead iodide was dissolved in 1 mL of DMF solvent to prepare a lead iodide precursor solution, which was then spin-coated on the hole transport layer and annealed at 80° C. in nitrogen for 1 min to prepare a lead iodide film with a thickness of 400 nm.
[0113] Step 3: Dissolve 0.85 mg of 4-mercaptobutyric acid in 1 mL of IPA solvent to prepare a mercapto acid solution with a concentration of 0.85 mg / mL, and then spin-coat the mercapto acid solution on the lead iodide film to prepare a mercapto acid intermediate layer with a thickness of 35 nm.
[0114] Step 4: Dissolve 85 mg of iodoformamide, 15 mg of chloromethylamine, and 12 mg of bromomethylamine in 1 mL of IPA solvent to prepare an organic precursor solution, which is then spin-coated on the mercapto acid intermediate layer and annealed at 140° C. in nitrogen for 15 min to prepare a perovskite film with a thickness of 720 nm.
[0115] Step 5: Dissolve 50 mg of PCBM in 2 mL of o-dichlorobenzene to prepare an electron transport layer precursor solution. Spin-coat the electron transport layer precursor solution on the perovskite film and anneal at 120° C. for 8 min in nitrogen to prepare an electron transport layer with a thickness of 50 nm.
[0116] Step 6: Dissolve 20 mg of BCP in 2 mL of isopropanol to prepare a buffer layer precursor solution. Spin-coat the buffer layer precursor solution on the perovskite film and anneal at 100° C. for 10 min in nitrogen to prepare a buffer layer with a thickness of 30 nm.
[0117] Step 7: The thin film prepared above is subjected to thermal evaporation process to deposit a metal electrode Au with a thickness of 90 nm to prepare an inverted perovskite solar cell.
[0118] Example 3
[0119] Step 1: Same as step 1 in Example 1.
[0120] Step 2: Same as step 2 in Example 1.
[0121] Step 3: Dissolve 0.6 mg of 4-mercaptobutyric acid in 1 mL of IPA solvent to prepare a mercapto acid solution with a concentration of 0.6 mg / mL, and then spin-coat the mercapto acid solution on the lead iodide film to prepare a mercapto acid intermediate layer with a thickness of 25 nm.
[0122] Step 4: Dissolve 80 mg of iodoformamide and 15 mg of chloromethylamine in 1 mL of IPA solvent to prepare an organic precursor solution, which is then spin-coated on the mercapto acid intermediate layer and annealed at 130° C. for 15 min in nitrogen to prepare a perovskite film with a thickness of 630 nm.
[0123] Step 5: Dissolve 73.2 mg of Spiro-OMeTAD in 1 mL of chlorobenzene to prepare a spiro-OMeTAD solution. Dissolve 520 mg of lithium bis(trifluoromethanesulfonyl)imide in 1 mL of anhydrous acetonitrile, and add 17.6 μL of lithium bis(trifluoromethanesulfonyl)imide solution and 28.8 μL of TBP solution to the spiro-OMeTAD solution to prepare a hole transport layer precursor solution. Spin-coat the hole transport layer precursor solution on the perovskite film to prepare a hole transport layer with a thickness of 80 nm.
[0124] Step 6: The thin film prepared above is subjected to thermal evaporation process to deposit a metal electrode Au with a thickness of 110 nm to prepare a formal perovskite solar cell (the battery is stored in a dryer for 15 days, and the drying temperature is set to room temperature).
[0125] Example 4
[0126] Step 1: Dissolve 20 mg NiOx in 1 mL deionized water and stir magnetically for 5 h to prepare a hole transport layer precursor solution. Then, spin coat the hole transport layer precursor solution on an ITO conductive substrate and anneal at 200 ° C in nitrogen for 20 min to prepare a hole transport layer with a thickness of 20 nm.
[0127] Step 2: Dissolve 701.5 mg of lead iodide in 1 mL of DMF solvent to prepare a lead iodide precursor solution, which is then spin-coated on the hole transport layer and annealed in nitrogen at 70° C. for 1 min to prepare a lead iodide film with a thickness of 450 nm.
[0128] Step 3: Dissolve 1.35 mg of 4-mercapto-4-methylpentanoic acid in 1 mL of IPA solvent to prepare a mercapto acid solution with a concentration of 1.35 mg / mL, and then spin-coat the mercapto acid solution on the lead iodide film to prepare a mercapto acid intermediate layer with a thickness of 20 nm.
[0129] Step 4: Dissolve 90 mg of iodoformamidine, 35 mg of iodomethylamine, 10 mg of chloromethylamine, and 10 mg of bromomethylamine in 1 mL of IPA solvent to prepare an organic precursor solution, which is then spin-coated on the mercapto acid intermediate layer and annealed at 170° C. in dry air for 15 min to prepare a perovskite film with a thickness of 760 nm.
[0130] Step 5: C is deposited on the perovskite film by thermal evaporation process. 60 , an electron transport layer with a thickness of 80 nm was prepared.
[0131] Step 6: The thin film prepared above is subjected to thermal evaporation process to deposit a metal electrode Cu with a thickness of 110 nm to prepare an inverted perovskite solar cell.
[0132] Example 5
[0133] Step 1: Mix the SnO2 nanoparticle solution and deionized water in a volume ratio of 1:5 to prepare a SnO2 solution, then spin-coat the SnO2 solution on a PEN / ITO flexible conductive substrate, anneal at 180°C in air for 30 minutes to prepare an electron transport layer with a thickness of 60 nm.
[0134] Step 2: Dissolve 688.5 mg of lead iodide in 1 mL of DMF solvent to prepare a lead iodide precursor solution, then spin-coat it on the electron transport layer, and anneal it at 80° C. in nitrogen for 1 min to prepare a lead iodide film with a thickness of 430 nm.
[0135] Step 3: Dissolve 1.5 mg of 3-mercaptoisobutyric acid in 1 mL of IPA solvent to prepare a mercapto acid solution with a concentration of 1.5 mg / mL, and then spin-coat the mercapto acid solution on the lead iodide film to prepare a mercapto acid intermediate layer with a thickness of 50 nm.
[0136] Step 4: Dissolve 90 mg of iodoformamide, 15 mg of chloromethylamine, and 15 mg of bromomethylamine in 1 mL of IPA solvent to prepare an organic precursor solution, which is then spin-coated on the mercapto acid intermediate layer and annealed at 150° C. in nitrogen for 10 min to prepare a perovskite film with a thickness of 800 nm.
[0137] Step 5: Dissolve 73.2 mg of Spiro-OMeTAD in 1 mL of chlorobenzene to prepare a spiro-OMeTAD solution. Dissolve 520 mg of lithium bis(trifluoromethanesulfonyl)imide in 1 mL of anhydrous acetonitrile, and add 17.6 μL of lithium bis(trifluoromethanesulfonyl)imide solution and 28.8 μL of TBP solution to the spiro-OMeTAD solution to prepare a hole transport layer precursor solution. Spin-coat the hole transport layer precursor solution on the perovskite film to prepare a hole transport layer with a thickness of 80 nm.
[0138] Step 6: The thin film prepared above is subjected to thermal evaporation process to deposit metal electrode Ag with a thickness of 100 nm to prepare a flexible formal perovskite solar cell.
[0139] Example 6
[0140] Step 1: Prepare a NiOx thin film on a PEN / ITO flexible conductive substrate by magnetron sputtering to obtain a hole transport layer with a thickness of 40 nm.
[0141] Step 2: 655.4 mg of lead iodide was dissolved in 1.35 mL of a mixed solvent of DMF and NMP (solution volume ratio DMF:NMP=1:0.35) to prepare a lead iodide precursor solution, which was then spin-coated on the hole transport layer and annealed in nitrogen at 70° C. for 1 min to prepare a lead iodide film with a thickness of 320 nm.
[0142] Step 3: Dissolve 1.7 mg of 4-mercapto-4-methylpentanoic acid in 1 mL of IPA solvent to prepare a mercapto acid solution with a concentration of 1.7 mg / mL, and then spin-coat the mercapto acid solution on the lead iodide film to prepare a mercapto acid intermediate layer with a thickness of 25 nm.
[0143] Step 4: Dissolve 90 mg of iodoformamide, 35 mg of iodomethylamine, 10 mg of chloromethylamine, and 10 mg of bromomethylamine in 1 mL of IPA solvent to prepare an organic precursor solution, which is then spin-coated on the lead iodide layer and annealed at 170° C. in dry air for 15 min to prepare a perovskite film with a thickness of 640 nm.
[0144] Step 5: Dissolve 50 mg of PCBM in 2 mL of o-dichlorobenzene to prepare an electron transport layer precursor solution. Spin-coat the electron transport layer precursor solution on the perovskite film and anneal at 120° C. for 8 min in nitrogen to prepare an electron transport layer with a thickness of 45 nm.
[0145] Step 6: Dissolve 20 mg of BCP in 2 mL of isopropanol to prepare a buffer layer precursor solution. Spin-coat the buffer layer precursor solution on the perovskite film and anneal at 100° C. for 10 min in nitrogen to prepare a buffer layer with a thickness of 30 nm.
[0146] Step 7: The thin film prepared above is subjected to thermal evaporation process to deposit metal electrode Ag with a thickness of 90 nm to prepare a flexible inverse perovskite solar cell.
[0147] Comparative Example 1
[0148] The only difference from Example 1 is that step 3 is omitted, and the remaining steps and parameters are the same as those of Example 1. (The battery is stored in a desiccator for 15 days, and the drying temperature is set to room temperature).
[0149] Test Example 1
[0150] The perovskite solar cells prepared in Example 1 and Comparative Example 1 were placed on a test bench simulating a solar light source and tested under standard light intensity. The test voltage range was -0.1V to 1.2V, with a step length of 0.015V. The test results are shown in Figure 2. Figure 7 As shown in the figure, it can be seen that when 3-mercaptoisobutyric acid is not added in Comparative Example 1, the open circuit voltage (V OC) is 1.147V, the short-circuit current density (J SC ) is 23.54 mA / cm 2 , the fill factor (FF) is 81.02%, and the photoelectric conversion efficiency (PCE) is 21.89%. In Example 1, when the concentration of added 3-mercaptoisobutyric acid is 0.5 mg / mL, the open circuit voltage (V OC ) is 1.157V, the short-circuit current density (J SC ) is 24.17 mA / cm 2 , the fill factor (FF) is 80.12%, and the photoelectric conversion efficiency (PCE) is 22.41%; when the concentration of added 3-mercaptoisobutyric acid is 1 mg / mL, the open circuit voltage (V OC ) is 1.157V, the short-circuit current density (J SC ) is 24.54 mA / cm 2 , the fill factor (FF) is 82.11%, and the photoelectric conversion efficiency (PCE) is 23.33%; when the concentration of added 3-mercaptoisobutyric acid is 2 mg / mL, the open circuit voltage (V OC ) is 1.096V, the short-circuit current density (J SC ) is 22.32 mA / cm 2 , the fill factor (FF) is 75.71%, and the photoelectric conversion efficiency (PCE) is 18.53%. The addition of 3-mercaptoisobutyric acid at a concentration of 1 mg / mL increases the cell efficiency from 21.89% to 23.33%.
[0151] Test Example 2
[0152] The perovskite solar cells prepared in Example 3 and Comparative Example 1 were placed on a test bench simulating a solar light source and tested under standard light intensity. The test voltage range was -0.1V to 1.2V, with a step length of 0.015V. The test results are shown in Figure 2. Figure 8 As shown in the figure, it can be seen that the photoelectric conversion efficiency (PCE) of the prepared battery of the perovskite solar cell without the addition of mercapto acid in comparative example 1 is 22.35%, 21.16%, 15.54% and 10.91% after storage for 0 days, 5 days, 10 days and 15 days, respectively. The photoelectric conversion efficiency (PCE) of the prepared battery of the perovskite solar cell with the addition of 4-mercaptobutyric acid in Example 3 is 23.98%, 23.27%, 22.86% and 21.95% after storage for 0 days, 5 days, 10 days and 15 days, respectively. The results show that the added 4-mercaptobutyric acid not only improves the stability of the perovskite solar cell, but also increases the battery efficiency from 22.35% to 23.98%.
[0153] Test Example 3
[0154] The perovskite solar cells prepared in Example 2, Example 4 and Example 5 were tested in the same manner as in Test Example 1. The results are as follows: Figure 9-11 As shown;
[0155] Fig. 9 This is the efficiency curve of the perovskite solar cell prepared in Example 2.
[0156] Fig.10 This is the efficiency curve of the perovskite solar cell prepared in Example 4.
[0157] Fig.11 This is the efficiency curve of the perovskite solar cell prepared in Example 5.
[0158] The embodiments described above are only descriptions of the preferred embodiments of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for preparing a perovskite film, characterized in that: The following steps are involved: coating a mercapto acid solution on the lead iodide film to prepare a mercapto acid intermediate layer; coating an organic precursor solution on the mercapto acid intermediate layer, and then annealing to obtain the perovskite film; The solute in the mercapto acid solution is one or more of 3-mercaptoisobutyric acid, 4-mercaptobutyric acid, and 4-mercapto-4-methylpentanoic acid, and the solvent is one of benzyl alcohol, ethanol, and isopropanol; The solute in the organic precursor solution is one or more of iodoformamidine, iodomethylamine, chloromethylamine, and bromomethylamine, and the solvent is ethanol or isopropanol.
2. The method for preparing a perovskite thin film according to claim 1, characterized in that: The concentration of the mercapto acid solution is 0.5 to 2 mg / mL; The concentration of the organic precursor solution is 0.3 mmol / mL to 0.6 mmol / mL; The annealing temperature is 120-180° C. and the annealing time is 10-30 minutes.
3. The method for preparing a perovskite thin film according to claim 1, characterized in that: The lead iodide film is prepared by coating a lead iodide precursor solution on a substrate and annealing at 50 to 100° C. for 30 seconds to 3 minutes; The solute in the lead iodide precursor solution is lead iodide, and the solvent is at least one of N,N-dimethylformamide, N-methylpyrrolidone, and dimethyl sulfoxide; The concentration of the lead iodide precursor solution is 1.0 mmol / mL to 2.0 mmol / mL.
4. The perovskite film prepared according to the preparation method according to any one of claims 1 to 3.
5. Use of the perovskite film as claimed in claim 4 in the preparation of perovskite solar cells.
6. A perovskite solar cell, characterized in that: Comprising the perovskite film as described in claim 4.
7. The perovskite solar cell according to claim 6, characterized in that: Formal or trans structure; When the perovskite solar cell is a formal structure, it includes a substrate, an electron transport layer, a perovskite light absorption layer, a hole transport layer and an electrode arranged in sequence from bottom to top; When the perovskite solar cell is an inverted structure, it includes a substrate, a hole transport layer, a perovskite light absorption layer, an electron transport layer and an electrode arranged in sequence from bottom to top; The perovskite light absorbing layer is the perovskite thin film according to claim 4.
8. The perovskite solar cell according to claim 7, characterized in that: The substrate is a rigid conductive substrate or a flexible conductive substrate; The rigid conductive substrate is a flat glass on which a conductive film is coated, and the conductive film includes FTO or ITO; The flexible conductive substrate is one of PEN, PVA and PT; The electron transport layer is tin oxide, titanium oxide, PCBM, BCP, C 60 One of; The hole transport layer is one of Spiro-OMeTAD, PEDOT:PSS, nickel oxide, and molybdenum oxide; The electrode is one of gold, silver, copper and carbon.
9. A method for preparing a perovskite solar cell according to claim 7 or 8, characterized in that: When the perovskite solar cell is a formal structure, the preparation method comprises the following steps: preparing an electron transport layer on the surface of the substrate; Preparing a perovskite light absorbing layer on the surface of the electron transport layer; preparing a hole transport layer on the surface of the perovskite light absorbing layer; Prepare an electrode on the surface of the hole transport layer to obtain the perovskite solar cell; When the perovskite solar cell is an inverted structure, the preparation method comprises the following steps: preparing a hole transport layer on the surface of the substrate; Preparing a perovskite light absorbing layer on the surface of the hole transport layer; preparing an electron transport layer on the surface of the perovskite light absorbing layer; An electrode is prepared on the surface of the electron transport layer to obtain the perovskite solar cell.
10. The method for preparing a perovskite solar cell according to claim 9, characterized in that: The preparation method of the electron transport layer is any one of spin coating, chemical bath, and scraping; the preparation method of the air transport layer is any one of spin coating, chemical bath, scraping, and sputtering; the preparation method of the electrode is any one of evaporation, sputtering, and scraping.
Citation Information
Cited By
Solar cell based on perovskite thin film capable of inhibiting lead leakage and preparation method thereof
CN120302798A
Stabilizer, perovskite precursor solution, perovskite solar cell and preparation method thereof, perovskite laminated solar cell and photovoltaic module
CN122094392A