Outer window film

By using a specific proportion of urethane acrylate resin, hindered amine light stabilizer and ultraviolet absorber in the hard coating of the outer window film, combined with the photopolymerization initiator and the preferred substrate, the hard coating is solved when winding is carried out. The problem of insufficient cracks and weather resistance achieves high transparency and excellent weather resistance.

CN119013143AActive Publication Date: 2024-11-22LINTEC CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202380032846.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-29
Publication Date
2024-11-22
Estimated Expiration
2043-03-29

AI Technical Summary

Technical Problem

The hard coating of the outer window film is prone to cracks when wound into a roll, resulting in reduced transparency and reduced performance, and is difficult to transport and install as much as possible in one operation, and is insufficient weather resistance.

Method used

The hard coating layer containing a urethane (meth)acrylate resin, a hindered amine light stabilizer and an ultraviolet absorber is composed of 2.0 mass of the hindered amine light stabilizer relative to 100.0 mass parts of the methacrylate resin. Parts or more and less than 15.0 parts by mass, and the ratio of the ultraviolet absorber is 5.0 parts by mass and less than 30.0 parts by mass, the photopolymerization initiator is combined to improve flexibility and light resistance, and the overall performance is improved by a preferred base material.

Benefits of technology

Effectively prevent cracks from occurring during winding of hard coating, maintain transparency, and at the same time improve the weather resistance and light resistance of the outer window film, ensuring stable performance in harsh environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013143A_ABST
    Figure CN119013143A_ABST
Patent Text Reader

Abstract

The exterior window film of the present invention includes a base material, a hard coating layer provided on one side of the base material, and an adhesive layer provided on a side of the base material opposite to the side of the hard coating layer. The hard coat layer is formed from a material containing a (meth) acrylate resin having a urethane (meth) acrylate as a constituent component, a hindered amine light stabilizer, and an ultraviolet absorber. The exterior window film according to the present invention is characterized in that, with respect to 100.0 parts by mass of a (meth) acrylate resin, the proportion of a hindered amine light stabilizer is 2.0 parts by mass or more and 15.0 parts by mass or less, and the proportion of an ultraviolet light absorber is 5.0 parts by mass or more and 30.0 parts by mass or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an exterior window film. Background Art

[0002] Window films are adhesive films applied to window glass in vehicles such as cars, ships, trains, and buildings such as homes, apartments, and office buildings. Window films are widely used to block ultraviolet and / or infrared rays from sunlight, protect privacy, prevent crime, prevent glass breakage, and for decoration.

[0003] For example, a window film includes a transparent substrate, a hard coating layer placed on one side of the substrate, and an adhesive layer on the other side of the hard coating layer relative to the substrate. In addition, the window film is also used to effectively cut off ultraviolet rays by adding an ultraviolet absorber to the adhesive layer. (For example, Patent Document 1).

[0004] In the inner window film attached to the indoor side of the window glass, sunlight is transmitted in the order of window glass / adhesive layer / substrate / hard coating layer / indoor. In this case, since the adhesive layer can block ultraviolet rays, thereby protecting the hard coating layer from the influence of ultraviolet rays, it is possible to suppress the degradation of the hard coating layer caused by ultraviolet rays.

[0005] On the other hand, for customers who want to stick window films from the outside of the window due to the structure of the building, an exterior window film that is stuck on the outside of the window glass has also been developed.

[0006] In this exterior window film, sunlight is transmitted in the order of hard coating / substrate / adhesive layer / window glass / indoor. Therefore, the adhesive layer cannot block ultraviolet rays and protect the hard coating from ultraviolet rays, resulting in the degradation of the hard coating due to ultraviolet rays.

[0007] Furthermore, in exterior window films, in addition to sunlight, rain, wind, temperature changes, etc. can also cause degradation of the hard coat layer.

[0008] Furthermore, since a crane or the like is used when installing the window film from the outside, it is desirable to transport as much window film as possible to the installation location in one operation.

[0009] Therefore, in order to make the hard coating layer of the window film be located on the outside, the window film is transported in a rolled state. At this time, cracks must not appear in the hard coating layer.

[0010] If cracks form in the hard coating, problems such as reduced transparency and reduced appearance and performance may occur.

[0011] [Reference technical literature]

[0012] [Patent Document]

[0013] [Patent Document 1] See Patent Publication No. 2018 / 1173979. Summary of the invention

[0014] [Problems to be Solved by the Invention]

[0015] An object of the present invention is to provide an exterior window film having a hard coating layer, which can maintain transparency, prevent cracks from being generated in the hard coating layer when being wound into a roll, and has excellent weather resistance.

[0016] [Methods of solving the problem]

[0017] This object is achieved by the present invention having the following structures. In addition, in the present invention, these structures can be arbitrarily combined.

[0018] The exterior window film of the present invention includes a substrate, a hard coating layer provided on one side of the substrate, and an adhesive layer provided on the side of the substrate opposite to the side provided with the hard coating layer.

[0019] The hard coating layer is composed of a material containing a (meth)acrylate resin having urethane (meth)acrylate as a constituent component, a hindered amine light stabilizer, and a UV absorber.

[0020] The invention is characterized in that the ratio of the hindered amine light stabilizer is 2.0 parts by mass to 15.0 parts by mass, and the ratio of the ultraviolet absorber is 5.0 parts by mass to 30.0 parts by mass, based on 100.0 parts by mass of the (meth)acrylate resin.

[0021] In the present invention, it is preferred that the ultraviolet absorber contains a compound having a benzophenone structure and a compound having a hydroxyphenyltriazine structure.

[0022] In the present invention, the ratio of the content of the compound having a benzophenone structure to the content of the compound having a hydroxyphenyltriazine structure in the hard coat layer is preferably 1.0:2.0 or more and 2.0:1.0 or less in terms of mass ratio.

[0023] In the present invention, the (meth)acrylate resin preferably has a structure obtained by polymerizing urethane (meth)acrylate using a photopolymerization initiator.

[0024] In the present invention, the photopolymerization initiator is preferably a triphenylphosphine oxide-based compound because the ultraviolet absorption wavelength thereof is biased toward the longer wavelength side than that of the ultraviolet absorber.

[0025] In the present invention, the thickness of the hard coat layer is preferably 0.1 μm or more and 20 μm or less.

[0026] In the present invention, the substrate is preferably composed of a material containing polyester.

[0027] [Effects of the invention]

[0028] According to the present invention, in an exterior window film provided with a hard coating layer, it is possible to provide an exterior window film which can ensure transparency, prevent the occurrence of cracks in the hard coating layer when being wound into a roll, and has excellent weather resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a cross-sectional view showing an example of the structure of the outer window film of the present invention.

[0030] Figure 2 This is a surface micrograph of the exterior window film of Example 1 after being subjected to an accelerated aging test.

[0031] Figure 3 This is a surface micrograph of the exterior window film of Example 1 after the accelerated aging test.

[0032] Figure 4 This is a surface micrograph of the exterior window film of Example 3 after the accelerated aging test.

[0033] Figure 5 This is a surface micrograph of the exterior window film of Example 6 after the accelerated aging test.

[0034] Figure 6 This is a surface micrograph of the exterior window film of Comparative Example 1 before the accelerated aging test. DETAILED DESCRIPTION

[0035] Hereinafter, preferred embodiments of the present invention will be described in detail.

[0036] [1] Window film

[0037] Figure 1 It is a cross-sectional view showing an example of the structure of the outer window film of the present invention.

[0038] The outer window film 1 includes a substrate 2, a hard coating layer 3 disposed on one side of the substrate 2, and an adhesive layer 4 on the opposite side of the hard coating layer 3 side of the substrate 2. The hard coating layer 3 is formed of a material containing a (meth) acrylate resin having urethane (meth) acrylate as a constituent component, a hindered amine light stabilizer, and an ultraviolet light absorber. In addition, relative to 100.0 parts by mass of the (meth) acrylate resin, the proportion of the hindered amine light stabilizer is 2.0 parts by mass or more and 15.0 parts by mass or less, and the proportion of the ultraviolet light absorber is 5.0 parts by mass or more and 30.0 parts by mass or less.

[0039] As described above, in the hard coating layer 3, the (meth)acrylate resin contains urethane (meth)acrylate as a constituent component. This imparts flexibility to the hard coating layer 3 and helps prevent cracks from occurring in the hard coating layer 3 when the outer window film 1 is wound into a roll.

[0040] In addition, the hard coating layer 3 contains a hindered amine light stabilizer, which contributes to improving the light resistance of the outer window film 1 and helps to suppress the reduction in transparency of the outer window film 1 .

[0041] In addition, since the hard coating layer 3 contains an ultraviolet absorber, the hard coating layer 3 can block ultraviolet rays. As a result, the proportion of ultraviolet rays in the light passing through the outer window film 1 can be reduced. In addition, when the outer window film 1 is attached to an adherend, ultraviolet rays can be blocked by the hard coating layer 3 as the outermost layer. This also helps to suppress the deterioration of the adhesive layer 4 and the substrate 2.

[0042] Moreover, the ratio of the hindered amine light stabilizer is 2.0 parts by mass or more and 15.0 parts by mass or less, and the ratio of the ultraviolet absorber is 5.0 parts by mass or more and 30.0 parts by mass or less, based on 100.0 parts by mass of the (meth)acrylate resin.

[0043] The hard coating layer 3 contains a predetermined ratio of a hindered amine light stabilizer and an ultraviolet absorber, thereby ensuring the transparency of the outer window film 1 and preventing cracks from occurring in the hard coating layer 3 when the outer window film 1 is wound into a roll, thereby improving the weather resistance of the outer window film 1 .

[0044] When the outer window film 1 has the above structure, the preferred effect of the present invention can be obtained, while when the outer window film 1 does not have the above structure, the preferred effect of the present invention cannot be obtained.

[0045] For example, if the (meth)acrylate resin constituting the hard coat layer does not contain urethane (meth)acrylate as a constituent component, the occurrence of cracks in the hard coat layer cannot be sufficiently prevented when the outer window film is wound into a roll.

[0046] Furthermore, if the hard coating layer does not contain a hindered amine light stabilizer, the light resistance of the exterior window film will be significantly reduced, and the transparency of the exterior window film 1 will be significantly reduced.

[0047] Furthermore, even if the hard coat layer contains a hindered amine light stabilizer, if the ratio thereof is less than the above lower limit, the light resistance of the outer window film cannot be sufficiently improved even if the hard coat layer contains a high content of ultraviolet absorber. As a result, the decrease in the transparency of the outer window film 1 cannot be sufficiently suppressed.

[0048] Furthermore, if the proportion of the hindered amine light stabilizer in the hard coat layer exceeds the above upper limit, there is a concern that the hindered amine light stabilizer may segregate on the surface and the outer window film may have a poor appearance.

[0049] Furthermore, if the hard coat does not contain a UV absorber, the weatherability of the exterior window film will be significantly reduced.

[0050] Furthermore, even if the hard coat layer contains an ultraviolet absorber, if the ratio thereof is less than the above lower limit, the weather resistance of the outer window film cannot be sufficiently improved even if the hard coat layer contains a relatively high content of the hindered amine light stabilizer.

[0051] If the ratio of the ultraviolet absorber in the hard coat layer exceeds the upper limit, ultraviolet rays may be excessively absorbed during the curing reaction of the urethane (meth)acrylate, which may result in poor curing of the urethane (meth)acrylate.

[0052] [1-1] Base material

[0053] The substrate 2 has the function of supporting the hard coat layer 3 and the adhesive layer 4 .

[0054] The substrate 2 may be made of any material. For example, the constituent material of the substrate 2 includes various resin materials. However, the substrate 2 is preferably composed of a material containing polyester, and more preferably mainly composed of polyester.

[0055] As a result, the workability of the outer window film 1 is improved, and the bonding operation of the outer window film 1 and the adherend etc. is more convenient. In addition, the durability of the outer window film 1 is improved.

[0056] In the present specification, "mainly" refers to a site having the highest content rate among target sites.

[0057] In particular, the content of the polyester in the substrate 2 is preferably 90 wt % or more, more preferably 95 wt % or more.

[0058] Examples of the polyester constituting the substrate 2 include polyethylene terephthalate and polybutylene terephthalate. Among them, polyethylene terephthalate is preferred.

[0059] As a result, the operability of the outer window film 1 becomes good, and the bonding operation of the outer window film 1 and the adherend etc. becomes more convenient. In addition, the durability of the outer window film 1 becomes better. In addition, the adhesion with the hard coating layer 3 and the adhesive layer 4 composed of the materials described later is improved.

[0060] The substrate 2 may contain components other than those described below.

[0061] Such components include, for example, colorants, antioxidants, ultraviolet absorbers, light stabilizers, softeners, modifiers, rust inhibitors, fillers, surface lubricants, corrosion inhibitors, heat stabilizers, lubricants, antistatic agents, inhibitors, crosslinking agents, catalysts, leveling agents, thickeners and dispersants.

[0062] The substrate 2 preferably contains an ultraviolet absorber. This can improve the light resistance of the substrate 2 itself and the light resistance of the outer window film 1 as a whole. In addition, the ultraviolet absorber contained in the substrate 2 and the ultraviolet absorber contained in the hard coating layer 3 can be the same or different, but are preferably different. This can more significantly exert the above-mentioned effect.

[0063] In particular, it is preferred that the substrate 2 has polyethylene terephthalate as a main component and contains an ultraviolet absorber. This can more significantly exert the above-mentioned effects.

[0064] Examples of the ultraviolet absorber include salicylic acid ultraviolet absorbers such as p-butylphenyl salicylate and p-octylphenyl salicylate; benzophenone ultraviolet absorbers such as 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxy-5-sulfobenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, and bis(2-methoxy-4-hydroxy-5-benzoylphenyl)methane; benzotriazole ultraviolet absorbers such as 2-(2'-hydroxy-5'-methylphenyl)benzotriazole and 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazole-2-phenol]; 2-p-nitrophenyl-3,1-benzoxazin-4-one, 2-(p-benzoylphenyl)-3,1-benzoxazin-4-one, Benzoxazinone-based ultraviolet light absorbers such as benzoxazinone, 2-(2-naphthyl)-3,1-benzoxazine-4-one, 2,2'-(p-phenylene)bis(3,1-benzoxazine-4-one), and 2,2'-(2,6-naphthylene)bis(3,1-benzoxazine-4-one); inorganic ultraviolet light absorbers such as titanium dioxide, cerium oxide, zinc oxide, iron oxide, and barium sulfate, for example, one or a combination of two or more selected from these can be used. Among them, from the viewpoint of being able to be melt-mixed with polyethylene terephthalate, benzoxazinone-based ultraviolet light absorbers are preferred. Examples of benzoxazinone-based (organic) ultraviolet light absorbers include 2,2'-(1,4-phenylene)bis[4H-3,1-benzoxazine-4-one], 2,6-naphthalenebis(1,3-benzoxazine-4-one)

[0065] The substrate 2 may have a generally uniform composition as a whole, or may have portions with different compositions. For example, the substrate 2 may be a laminate including a plurality of layers, the plurality of layers having portions with different compositions from each other (including, for example, resin materials with different molecular weights). In addition, the substrate 2 may be made of a gradient material having a gradient change in composition along the thickness direction.

[0066] The substrate 2 may be surface treated to improve adhesion with the hard coat layer 3 and the adhesive layer 4 .

[0067] Examples of such surface treatments include corona treatment and application of an adhesive resin.

[0068] Examples of the easy-adhesive resin include polyester resins, polyurethane resins, acrylic resins, and the like.

[0069] The thickness of the substrate 2 is not particularly limited, but is preferably 10 μm or more and 300 μm or less, more preferably 15 μm or more and 200 μm or less, and further preferably 20 μm or more and 100 μm or less.

[0070] As a result, the durability of the outer window film 1 can be obtained, and the operability of the outer window film 1 is improved, and the operation of pasting to the adherend can be easily performed. In addition, the shape following ability to the curved adherend is improved, and wrinkles are effectively prevented from being generated in the outer window film 1.

[0071] [1-2] Hard coating

[0072] The hard coating layer 3 has better wear resistance than the substrate 2 , and has, for example, a function of improving the wear resistance of the entire outer window film 1 .

[0073] Thus, after the outer window film 1 is pasted on the adherend, excellent wear resistance can be exhibited. In particular, the outer window film 1 has a high chance of contacting and colliding with sand, dust and various flying objects, and the hard coating layer 3 is an important part that ensures that it is difficult to be scratched and has sufficient durability even in such a use environment. In addition, damage during the work of adhering the outer window film 1 to the adherend can be effectively prevented.

[0074] In addition, the hard coating layer 3 is formed of a material containing a hindered amine light stabilizer and an ultraviolet light absorber. Thus, ultraviolet rays can be blocked, and the proportion of ultraviolet rays in the light passing through the outer window film 1 can be reduced. In addition, when the outer window film 1 is attached to an adherend, ultraviolet rays can be blocked by the hard coating layer 3 as the outermost layer. Therefore, the hard coating layer 3 can help to suppress the deterioration of the adhesive layer 4 and the substrate 2, and also has the function of improving the weather resistance of the outer window film 1.

[0075] [1-2-1] (Meth)acrylate resin

[0076] The hard coat layer 3 contains a (meth)acrylate resin having urethane (meth)acrylate as a constituent component, that is, a polymerizable component.

[0077] By making the (meth)acrylate resin contain urethane (meth)acrylate as a constituent component, flexibility can be imparted to the hard coat layer 3. In particular, by satisfying the prescribed content relationship of the hindered amine light stabilizer and the ultraviolet absorber described later, flexibility can be imparted to the hard coat layer 3 and cracks in the hard coat layer 3 can be effectively prevented.

[0078] Urethane (meth)acrylate is an oligomer having at least a (meth)acryloyl group and a urethane bond, and has a property of being polymerized and cured by energy ray irradiation.

[0079] The (meth)acrylate resin constituting the hard coat layer 3 may contain components other than the urethane (meth)acrylate. Examples of such components include (meth)acrylates having no urethane group.

[0080] Among them, the ratio of urethane (meth)acrylate in the (meth)acrylate resin constituting the hard coat layer 3 is preferably 10.0 wt % or more, more preferably 30.0 wt % or more, more preferably 50.0 wt % or more, and more preferably 50.0 wt % or more.

[0081] Chapter 0061

[0082] The content of the (meth)acrylate resin in the hard coat layer 3 is preferably 50.0 wt % or more and 93.0 wt % or less, more preferably 60.0 wt % or more and 90.0 wt % or less, and more preferably 70.0 wt % or more and 86.0 wt % or less.

[0083] When the hard coat layer 3 contains a plurality of types of (meth)acrylate resins, the content of the (meth)acrylate resin in the hard coat layer 3 is the total of these contents.

[0084] [1-2-2] Hindered Amine Light Stabilizer

[0085] The hard coating layer 3 contains a hindered amine light stabilizer.

[0086] First, the function of the hindered amine light stabilizer will be described.

[0087] That is, the hindered amine light stabilizer has an effect of returning the energy state of a substance excited by ultraviolet irradiation to a ground state and releasing the returned energy in the form of heat.

[0088] Therefore, chemical reactions caused by substances excited by ultraviolet irradiation can be suppressed, and deterioration of weather resistance such as yellowing of the outer window film 1 can be effectively suppressed.

[0089] The hindered amine light stabilizer contained in the hard coat layer 3 has a function of improving the weather resistance of the hard coat layer 3 and suppressing the deterioration of the characteristics due to light irradiation or the like over time.

[0090] The hindered amine light stabilizer has at least one group (hindered amine group) represented by the following formula (1) in one molecule.

[0091] [Chemical formula 1]

[0092]

[0093] In formula (1), R 1 represents a hydrogen atom, an alkyl group or an alkoxy group. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, a butyl group and the like. Examples of the alkoxy group include a methoxy group and an ethoxy group.

[0094] When there are multiple groups represented by formula (1) in one molecule, R 1 Can be the same or different.

[0095] Examples of such hindered amine light stabilizers include dimethyl succinate-1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidine condensate, poly{[6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidinyl))imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidinyl)imino], poly{[6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidinyl))imino} Morpholino-s-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidinyl)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidinyl)imino, N,N',N",N"'-tetrakis(4,6-bis(butyl-(N-methyl-2,2,6,6-tetramethylpiperidin-4-yl)amino)triazine-2-yl)-4,7-diazadecane-1,10-diamine, bis(1,2,2, 6,6-pentamethyl-4-piperidinyl)[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]butyl malonate, reaction products of cyclohexane and n-butyl peroxide, reaction products of 2,2,6,6-tetramethyl-4-piperidinamine-2,4,6-trichloro-1,3,5-triazine and 2-aminoethanol, bis(2,2,6,6-tetramethyl-1-(octyloxy)-4-piperidinyl) sebacate, 1,1-dimethoxyphenyl The reaction product of methyl ethyl hydroperoxide and octane, a mixture of bis(1,2,2,6,6-pentamethyl-piperidinyl) sebacate and 1,2,2,6,6-pentamethyl-4-piperidinyl sebacate methyl ester, a mixture of bis(1,2,2,6,6-pentamethyl-piperidinyl) sebacate and 1,2,2,6,6-pentamethyl-4-piperidinyl sebacate methyl ester, bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, etc. These can be used alone or in combination of two or more.

[0096] Among them, from the viewpoint of excellent performance as a light stabilizer and improved weather resistance, R in formula (1) is preferably 1 The hindered amine light stabilizer having a tertiary hindered amine group has particularly excellent performance as a light stabilizer, making the above effect more significant.

[0097] Examples of such hindered amine light stabilizers include: N,N',N",N"'-tetrakis(4,6-bis(butyl-(N-methyl-2,2,6,6-tetramethylpiperidin-4-piperidinyl))amino)triazine-2-piperidinyl)-4,7-diazadecane-1,10-diamine, bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, a mixture of bis(1,2,2,6,6-pentamethyl-piperidinyl) sebacate and 1,2,2,6,6-pentamethyl-4-piperidinyl sebacate and the like.

[0098] Examples of such hindered amine light stabilizers include a commercial product manufactured by BASF Corporation under the trade name “Tinuvin (registered trademark) 292” (a mixture of bis(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate and 1,2,2,6,6-pentamethyl-4-piperidinyl sebacate methyl ester).

[0099] As described above, the hindered amine light stabilizer is present in a ratio of 2.0 parts by mass or more and 15.0 parts by mass or less relative to 100.0 parts by mass of the (meth)acrylate resin in the hard coat layer 3. The ratio of the hindered amine light stabilizer to 100.0 parts by mass of the (meth)acrylate resin is preferably 3.0 parts by mass or more and 14.0 parts by mass or less, more preferably 4.0 parts by mass or more and 12.0 parts by mass or less, and further preferably 5.0 parts by mass or more and 10.0 parts by mass or less.

[0100] Thereby, the effects of the present invention described above can be more significantly exhibited.

[0101] The content of the hindered amine light stabilizer in the hard coat layer 3 is preferably 1.5 wt % to 12.5 wt %, more preferably 2.2 wt % to 11.5 wt %, and further preferably 4.0 wt % to 8.3 wt %.

[0102] Thereby, the effects of the present invention described above can be more significantly exhibited.

[0103] When the hard coat layer 3 contains a plurality of hindered amine light stabilizers, the content of the hindered amine light stabilizer in the hard coat layer 3 is the total of these contents.

[0104] [1-2-3] Ultraviolet light absorber

[0105] The hard coat layer 3 contains an ultraviolet absorber.

[0106] UV absorbers protect human bodies and objects from the effects of UV rays by absorbing UV rays and converting them into energy such as heat.

[0107] The ultraviolet absorber is preferably an acetonitrile solution with a concentration of 0.1 wt % having a maximum absorption wavelength of 380 nm or less in the wavelength range of 200 nm to 500 nm or less.

[0108] When there are a plurality of maximum absorption wavelengths of absorbance in the wavelength range of 200 nm to 500 nm, at least one maximum absorption wavelength may be within the above range.

[0109] Thus, when irradiated with ultraviolet rays, the acrylic polymer can be sufficiently cured without being hindered by the ultraviolet absorber.

[0110] On the other hand, from the viewpoint of preventing the influence of ultraviolet rays on the human body and articles, the lower limit of the maximum absorption wavelength is preferably 280 nm or more.

[0111] Examples of the ultraviolet absorber include compounds such as benzophenone, benzotriazole, benzoate, benzoxazinone, triazine, phenyl salicylate, cyanoacrylate, and nickel complex salts, and any one of these may be used alone or in combination of two or more.

[0112] Among the above-mentioned ultraviolet absorbers, compounds having a benzophenone structure or a hydroxyphenyltriazine structure are preferably used.

[0113] These compounds have excellent compatibility with the above-mentioned (meth) acrylic resin and the like, and also have a high ultraviolet absorption function. Therefore, the hard coat layer 3 formed using these compounds is likely to satisfy the above-mentioned optical characteristics.

[0114] In particular, the hard coat layer 3 preferably contains a compound having a benzophenone structure and a compound having a hydroxyphenyltriazine structure as the ultraviolet absorber.

[0115] Therefore, the above-mentioned effects of the present invention can be more significantly exerted.

[0116] When the hard coating layer 3 contains a compound having a benzophenone structure and a compound having a hydroxyphenyltriazine structure as ultraviolet absorbers, the ratio of the content of the compound having a benzophenone structure to the content of the compound having a benzophenone structure in the hard coating layer 3; the hydroxyphenyltriazine structure is preferably 1.0:2.0 or more and 2.0:1.0 or less, more preferably 1.0:1.5 or more and 1.0:1.0 or less, and further preferably 1.0:1.2 or more and 1.2:1.0 or less.

[0117] As a result, the above-mentioned effects are more significantly exerted.

[0118] Specific examples of the ultraviolet absorber include compounds represented by the following formulae (2) to (13). Among them, compounds represented by the following formulae (8) to (13) are preferred from the viewpoint of more significantly exhibiting the above-mentioned effects.

[0119] [Chemical formula 2]

[0120]

[0121] [Chemical formula 3]

[0122]

[0123] [Chemical formula 4]

[0124]

[0125] [Chemical formula 5]

[0126]

[0127] [Chemical formula 6]

[0128]

[0129] [Chemical formula 7]

[0130]

[0131] [Chemical formula 8]

[0132]

[0133] [Chemical formula 9]

[0134]

[0135] [Chemical formula 10]

[0136]

[0137] [Chemical formula 11]

[0138]

[0139] (In formula (11), R is an alkyl group having 10 or more carbon atoms and 12 or less carbon atoms)

[0140] [Chemical formula 12]

[0141]

[0142] [Chemical formula 13]

[0143]

[0144] Commercial products of the above-mentioned ultraviolet absorbers include, for example, products manufactured by BASF under the trade names of "Tinuvin (registered trademark) PS", "Tinuvin (registered trademark) 460", "Tinuvin (registered trademark) 477", "Tinuvin (registered trademark) 400" and "Tinuvin (registered trademark) 384-2". Also included are, for example, products manufactured by Shipro Kasei under the trade names of "SEESORB SB701", "SEESORB SB704", "SEESORB SB706", "SEESORB SB707", "SEESORB SB709", "SEESORB SB107", and "SEESORB SB106". Among them, from the viewpoint of more significantly exerting the above-mentioned effects, "Tinuvin (registered trademark) 460", "Tinuvin (registered trademark) 477", "Tinuvin (registered trademark) 400", "SEESORB SB107", and "SEESORB SB106" are preferred.

[0145] As described above, the hard coat layer 3 contains an ultraviolet absorber in a ratio of 5.0 parts by mass or more and 30.0 parts by mass or less relative to 100.0 parts by mass of the (meth)acrylate resin. However, the ratio of the ultraviolet absorber is preferably 7.0 parts by mass or more and 28.0 parts by mass or less, more preferably 8.0 parts by mass or more and 25.0 parts by mass or less, and further preferably 10.0 parts by mass or more and 20.0 parts by mass or less relative to 100.0 parts by mass of the (meth)acrylate resin.

[0146] Thereby, the effects of the present invention described above can be more significantly exhibited.

[0147] The content of the ultraviolet absorber in the hard coat layer 3 is preferably 4.1 wt % or more and 22.7 wt % or less, more preferably 5.7 wt % or more and 21.4 wt % or less, and further preferably 8.3 wt % or more and 16.0 wt % or less.

[0148] Thereby, the effects of the present invention described above can be more significantly exhibited.

[0149] When the hard coat layer 3 contains a plurality of types of ultraviolet absorbers, the content of the ultraviolet absorbers in the hard coat layer 3 is the total of these contents.

[0150] [1-2-4] Other ingredients

[0151] The hard coat layer 3 may contain components other than those described above. Hereinafter, such components will also be referred to as "other components" in this section.

[0152] Examples of such components include resin components other than the above-mentioned (meth)acrylate resins, light stabilizers other than hindered amine light stabilizers, antioxidants, silane coupling agents, leveling agents, antistatic agents, defoaming agents, and the like.

[0153] The proportion of other components in the hard coat layer 3 is preferably 10 wt % or less, more preferably 5 wt % or less, and further preferably 3 wt % or less.

[0154] [1-2-5] Other conditions

[0155] The thickness of the hard coat layer 3 is not particularly limited, but is preferably 0.1 μm or more and 20 μm or less, more preferably 0.2 μm or more and 15 μm or less, and further preferably 0.4 μm or more and 10 μm or less.

[0156] As a result, the hard coating layer 3 can be prevented from becoming too hard, and better wear resistance can be obtained, and the adhesion to the adherend and the workability of attaching the outer window film 1 can be improved. In addition, the generation of cracks and the like can be appropriately prevented.

[0157] [1-3] Adhesive layer

[0158] The pressure-sensitive adhesive layer 4 generally has excellent flexibility and is a portion that closely adheres to an adherend.

[0159] Examples of the adhesive constituting the adhesive layer 4 include acrylic adhesives, natural rubber adhesives, synthetic rubber adhesives, polyvinyl ether adhesives, polyurethane adhesives, silicone adhesives, etc. Among them, acrylic adhesives, polyurethane adhesives, and silicone adhesives are particularly preferred from the viewpoint of weather resistance.

[0160] Specific examples of the synthetic rubber adhesive include styrene-butadiene rubber, polyisobutylene rubber, isobutylene-isoprene, styrene-isoprene block copolymer, styrene-butadiene block copolymer, styrene-ethylene-butylene block copolymer and the like.

[0161] Specific examples of acrylic adhesives include butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, methyl (meth)acrylate, hydroxyethyl (meth)acrylate, and copolymers of (meth)acrylates in which two or more of various polymerization components such as hydroxybutyl acrylate are polymerized.

[0162] Specific examples of the polyvinyl ether binder include polyvinyl ether, polyvinyl isobutyl ether, and the like.

[0163] Specific examples of the silicone adhesive include dimethylpolysiloxane and the like.

[0164] These binders may be used alone or in combination of two or more.

[0165] The adhesive layer 4 only needs to contain an adhesive as a main component, and may contain components other than the adhesive.

[0166] Such components include, for example, UV absorbers, tackifiers, fillers, softeners, antioxidants, light stabilizers, crosslinking agents, colorants, modifiers, rust inhibitors, flame retardants, hydrolyzing agents, etc. Examples include inhibitors, surface lubricants, corrosion inhibitors, heat stabilizers, lubricants, antistatic agents, polymerization inhibitors, catalysts, leveling agents, thickeners, dispersants, defoamers, etc.

[0167] The thickness of the adhesive layer 4 is not particularly limited, but is, for example, preferably 1 μm or more and 100 μm or less, more preferably 5 μm or more and 80 μm or less, and further preferably 10 μm or more and 60 μm or less.

[0168] Thus, the durability of the outer window film 1 is improved, the operability of the outer window film 1 is improved, and the attachment operation to the adherend can be easily performed. In addition, the shape-following ability to the curved adherend is improved, and wrinkles are effectively prevented from being generated in the outer window film 1.

[0169] [1-4] Other conditions

[0170] The thickness (total thickness) of the outer window film 1 is not particularly limited, but is preferably 11 μm to 400 μm, more preferably 18 μm to 230 μm, and further preferably 20 μm to 100 μm.

[0171] Thus, the durability and ultraviolet absorption function of the outer window film 1 are improved, and the operability of the outer window film 1 is improved, making it easier to attach the film to an adherend. In addition, the shape-following ability of a curved adherend is improved, effectively preventing wrinkles from forming in the outer window film 1.

[0172] Here, "total thickness" refers to the total thickness of the outer window film 1 in a state of being attached to an adherend. Therefore, for example, even if a release liner 10 described later is provided on the adhesive layer 4 during storage of the outer window film 1, the thickness of the release liner 10 is not included in the total thickness of the outer window film 1.

[0173] In order not to damage the appearance of the adherend, the outer window film 1 is preferably transparent.

[0174] In this specification, "transparent" means that the transmittance in the visible light region is 60% or more (upper limit 100%), preferably 80% or more (upper limit 100%). The transmittance of the exterior window film 1 can be measured by a method according to JIS A5759:2016 (film for architectural window glass - visible light transmittance test).

[0175] The yellowness index (YI) of the outer window film 1 is preferably 4 or less, more preferably 1 or more and 3.5 or less, and further preferably 1.5 or more and 2.5 or less.

[0176] As a result, the coloring of the exterior window film 1 is suppressed. Thus, the exterior window film 1 can obtain excellent transparency and colorlessness, and can be suitably used as an exterior window film.

[0177] It should be noted that the yellowness index (YI) of the exterior window film 1 can be measured by a method in accordance with JIS K 7373:2006.

[0178] The haze of the outer window film 1 measured according to JIS K 7136:2000 is preferably close to the haze of the substrate 2 alone, and is preferably 2.0% or less, more preferably 1.8% or less, and further preferably 1.5% or less.

[0179] Thus, the outer window film 1 can have excellent transparency.

[0180] [2] Release liner

[0181] A release liner 10 may be provided on the adhesive layer 4 of the outer window film 1 .

[0182] When the outer window film 1 is attached to an adherend, the release liner 10 is peeled off from the adhesive layer 4 .

[0183] The release liner 10 is not particularly limited and may have a structure commonly used in the field of window films. The release liner 10 may have, for example, a structure in which a release layer is provided on the surface of a paper substrate or a resin film substrate.

[0184] As the material constituting the resin film substrate, for example, polyethylene terephthalate, polypropylene, etc. Examples of the material constituting the paper substrate include polyethylene laminated paper, polypropylene laminated paper, clay coated paper, resin coated paper, glass paper, and wood-free paper.

[0185] Examples of the composition of the release layer (b) include a composition containing a release agent such as silicone, a long-chain alkyl resin, or a fluororesin.

[0186] The thickness of the release liner 10 is not particularly limited, but is preferably, for example, 10 μm or more and 400 μm or less. When the release liner 10 has the release layer, the thickness of the release layer is, for example, preferably 0.01 μm or more and 5 μm or less.

[0187] [3] Method for manufacturing window film

[0188] Next, a method of manufacturing the exterior window film will be described.

[0189] First, for example, a liquid composition (coating liquid) for forming a hard coating layer 3 is applied to one side of the substrate 2 to form the hard coating layer 3. Next, a liquid composition (coating liquid) for forming an adhesive layer 4 is applied to the other side of the substrate 2 to form the adhesive layer 4. Thus, the outer window film 1 can be manufactured. In such a method, the order of forming the hard coating layer 3 and the adhesive layer 4 is not particularly limited.

[0190] The liquid composition for forming the hard coating layer 3 can be applied by a known method, for example, a bar coating method, a doctor blade coating method, a roll coating method, a knife coating method, a die coating method, a gravure coating method, or the like.

[0191] The adhesive layer 4 can be formed by irradiating a liquid composition for forming the adhesive layer 4 applied on the substrate 2 with ultraviolet rays or electron beams, or by heating and curing the liquid composition.

[0192] In the liquid composition for forming the hard coat layer 3 , it is preferred to add the above-mentioned photopolymerization initiator from the viewpoint of shortening the polymerization time due to light irradiation and reducing the light irradiation amount for forming the hard coat layer 3 .

[0193] In other words, the (meth)acrylate resin preferably has a structure in which urethane (meth)acrylate is polymerized using the above-mentioned photopolymerization initiator.

[0194] The content of the photopolymerization initiator in the liquid composition for forming the hard coat layer 3 is preferably 0.05 mass parts to 15.0 mass parts, more preferably 0.1 mass parts to 10.0 mass parts, and further preferably 0.3 mass parts to 5.0 mass parts, based on 100.0 mass parts of the urethane (meth)acrylate.

[0195] Thereby, the above-mentioned effect is more significantly exerted.

[0196] The liquid composition for forming the hard coat layer 3 may contain components other than the above components as necessary. Examples of such components include a thermal curing catalyst and a solvent.

[0197] The liquid composition for forming the adhesive layer 4 can be obtained by dissolving or suspending the above-mentioned materials constituting the adhesive layer 4 in an appropriate solvent. Examples of the solvent include esters such as ethyl acetate and butyl acetate; aromatic hydrocarbons such as methyl isobutyl ketone, methyl ethyl ketone, and cyclohexanone; aromatic hydrocarbons such as toluene and xylene, and the like, and a combination of one or two selected from these can be used.

[0198] The liquid composition for forming the adhesive layer 4 can be applied by a known method, for example, it can be a method using various coaters such as an air knife coater, a blade coater, a rod coater, a gravure coater, a roll coater, a roll knife coater, a curtain coater, a die coater, a knife coater, a screen coater, a Meyer rod coater, a kiss coater, etc.

[0199] The amount of the liquid composition for forming the adhesive layer 4 can be appropriately adjusted so that the thickness of the adhesive layer 4 after drying falls within the above range. The drying conditions of the liquid composition for forming the adhesive layer 4 are not particularly limited, but the drying temperature can be, for example, 70° C. or higher and 130° C. or lower, and the drying time can be, for example, 1 minute and 5 minutes or less.

[0200] Thus, the outer window film 1 can be obtained.

[0201] Furthermore, a release liner 10 may be laminated on the adhesive layer 4 of the outer window film 1 .

[0202] [4] Adhesive

[0203] Next, the adherend to which the outer window film 1 is attached will be described.

[0204] The exterior window film 1 is suitable for use in window glasses of buildings such as residences and buildings, and vehicles such as cars and trains.

[0205] Specifically, the exterior window film 1 of the present invention is applied to the outdoor side surface of the window glass. In such an exterior window film 1, sunlight is sequentially irradiated to the hard coating layer 3 / substrate 2 / adhesive layer 4 / window glass / interior. Therefore, the hard coating layer 3 can block ultraviolet rays and can appropriately suppress the degradation of the hard coating layer 3. In addition, the degradation of the substrate 2 and the adhesive layer 4 caused by ultraviolet rays can also be appropriately suppressed. In addition, in addition to ultraviolet rays, the degradation caused by rain, wind, temperature changes, etc. can also be appropriately suppressed.

[0206] As described above, since the exterior window film 1 has excellent weather resistance, it can be used as an exterior window film having a worse working environment than an interior window film.

[0207] [5] How to apply window film

[0208] Next, a method of attaching the exterior window film 1 will be described.

[0209] The case where the outer window film 1 is pasted to an adherend such as a window glass will be described. When the outer window film 1 has a release liner 10, the release liner 10 is first peeled off to expose the adhesive layer 4. By adhering the adhesive layer 4 to the adherend, the outer window film 1 can be adhered to the adherend. This pasting can be performed, for example, by a method known as a water bonding method. In the water bonding method, the adhesive layer 4 and the adherend are pasted by inserting a construction liquid with a surfactant added to water at the interface between the adhesive layer 4 and the adherend, and then the attachment operation is completed by scraping out the construction liquid using a fixture known as a scraper.

[0210] As mentioned above, although the preferred embodiment of the present invention was described, the present invention is not limited thereto.

[0211] For example, the outer window film may have a configuration other than the above. More specifically, for example, at least one intermediate layer may be provided between the substrate and the adhesive layer or between the substrate and the hard coating layer, or at least one coating layer may be provided on the outer surface of the hard coating layer.

[0212] Furthermore, the exterior window film of the present invention may be manufactured by any method and is not limited to the above-mentioned manufacturing method.

[0213] For example, the outer window film of the present invention can be formed by applying a transfer method. Specifically, first, a composition for forming an adhesive layer is applied to one side of a release liner to form an adhesive layer. Thereafter, the release liner provided with the adhesive layer is bonded to a substrate. In this way, an outer window film can be formed by applying a transfer method.

[0214] [example]

[0215] The present invention is described in detail below in conjunction with specific examples, but the present invention is not limited thereto. In the following examples, the treatments and measurements without indicating the temperature conditions were all carried out at room temperature (23°C).

[0216] [6] Exterior window film manufacturing

[0217] (Example 1)

[0218] First, a liquid composition (coating liquid) for forming a hard coat layer was prepared using BIMSET 575CB (manufactured by Arakawa Chemical Industries, Ltd.) containing urethane acrylate, Tinuvin 292 (manufactured by BASF) as a hindered amine light stabilizer, UV-24 (manufactured by Solvay) as a benzophenone-based ultraviolet absorber, Tinuvin 477 (manufactured by BASF) as an ultraviolet absorber, Omnirad TPO (manufactured by IGM Resins) as a photopolymerization initiator, and methyl ethyl ketone as a solvent.

[0219] In addition, Tinuvin 292 is a mixture of bis(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate and 1,2,2,6,6-pentamethyl-4-piperidinyl sebacate.

[0220] [Chemical formula 14]

[0221]

[0222] In addition, UV-24 is 2,2'-dihydroxy-4-methoxybenzophenone.

[0223] [Chemical formula 15]

[0224]

[0225] In addition, Tinuvin 477 is a mixture of hydroxyphenyltriazine UV absorber and 2-methoxy-1-methylethyl acetate. In addition, Omnirad TPO is 2,4,6-trimethylbenzoyldiphenylphosphine oxide, and its structure is shown below.

[0226] [Chemical formula 16]

[0227]

[0228] The liquid composition for forming a hard coating layer as described above was applied on one side of the substrate by a bar coating method, while adjusting the coating amount so that the film thickness after curing was 2.5 μm to obtain a coating film. The coating film was irradiated with a cumulative light intensity of 200 mJ / cm 2 This forms a hard coating.

[0229] As a substrate, a polyethylene terephthalate film having a thickness of 50 μm and containing an ultraviolet absorber (Toyobo Ester (registered trademark) Film HB3 manufactured by Toyobo Co., Ltd.) was used.

[0230] Next, an acrylic adhesive (butyl acrylate / acrylic acid = 90 parts by mass / 10 parts by mass copolymer (weight average molecular weight: 600,000) 100 parts by mass, isocyanate crosslinking agent 1 part by mass) was applied to the surface of the substrate opposite to the surface on which the hard coating layer was formed in such a manner that the thickness after drying was 25 μm to obtain a coating film. The coating film was dried at 100° C. for 1 minute to form an adhesive layer. In this way, an outer window film was manufactured. In addition, a release liner having a thickness of 38 μm was laminated on the adhesive layer of the outer window film.

[0231] (Examples 2 and 3)

[0232] The exterior treatment was performed in the same manner as in Example 1 except that the amount of each component in the hard coat layer-forming liquid composition was changed so that the content of each component satisfied the relationship shown in Table 1. An exterior window film was produced.

[0233] (Comparative Examples 1 to 6)

[0234] The exterior treatment was performed in the same manner as in Example 1 except that the amount of each component in the hard coat layer-forming liquid composition was changed so that the content of each component satisfied the relationship shown in Table 1. An exterior window film was produced.

[0235] [7] Evaluation of exterior window films

[0236] The obtained exterior window films were evaluated as follows.

[0237] [7-1] Weathering test of hard coating

[0238] Use an accelerated aging tester to perform accelerated aging tests.

[0239] The obtained outer window film was attached to a glass plate and placed in an accelerated weathering tester and exposed to an irradiance of 255 W / m 2 The accelerated aging test was carried out under the conditions of 300-400 nm, blackboard temperature of 63°C and humidity, in which the samples were placed for 1000 hours.

[0240] The surface of the hard coat layer was visually observed to evaluate the presence or absence of cracks.

[0241] A: No cracks

[0242] B: With cracks

[0243] [7-2] Crack resistance test of hard coating

[0244] The obtained outer window film was wound into a roll around a cylindrical core having an outer diameter of 20 mm so that the hard coating layer was located on the outside.

[0245] The core was taken out, a needle was inserted into the hard coating layer by 10 mm, and the damaged surface was visually observed to evaluate the presence or absence of cracks.

[0246] A: No cracks

[0247] B: With cracks

[0248] [7-3] Haze of exterior window film

[0249] The haze of the obtained exterior window film was measured using a haze meter (manufactured by Nippon Denshoku Kogyo Co., Ltd., NDH-5000) in accordance with JIS K7136:2000.

[0250] It can be said that the smaller this value is, the better the transparency of the exterior window film is.

[0251] Table 1 summarizes the conditions for forming the composition of the hard coat layer and the results of the above evaluation of each embodiment and comparative example. In Table 1, the content of each component is expressed in parts by mass. In addition, the content of the hindered amine light stabilizer and the ultraviolet absorber is expressed as a percentage relative to 100.0 parts by mass of the urethane acrylate contained in the formed hard coat layer. In addition, the content of the photopolymerization initiator is expressed as a percentage relative to 100.0 parts by mass of the urethane (meth) acrylate contained in the liquid composition for forming the hard coat layer.

[0252] Table 1

[0253]

[0254] As can be seen from Table 1, in Examples 1 to 3, good results were obtained in terms of weather resistance, crack resistance, and haze of the hard coat layer.

[0255] On the other hand, in each comparative example, no satisfactory results were obtained.

[0256] More specifically, in Comparative Examples 2 to 4 in which the hard coat layer did not contain a hindered amine light stabilizer, cracks occurred after the weathering test and the haze became larger. In addition, in Comparative Example 1 in which neither a hindered amine light stabilizer nor a UV absorber was contained, the haze became even larger. In addition, even if a hindered amine light stabilizer and a UV absorber were contained at the same time, Comparative Examples 5 and 6 in which the content of the hindered amine light stabilizer was small could not obtain sufficiently good results.

[0257] In addition, the surface micrographs of the outer window films of Example 1 and Comparative Examples 1, 3 and 6 after 1000 hours of accelerated aging test are shown in FIG. Figure 2 , 3 , 4 and 5.

[0258] also, Figure 6 Shown is a surface micrograph of the exterior window film of Comparative Example 1 before being subjected to accelerated aging testing.

[0259] Although no cracks were observed in Example 1, cracks were found to have occurred in Comparative Examples 1, 3, and 6.

[0260] When preparing a liquid composition for forming a hard coating layer, the ratio of the hindered amine light stabilizer to 100.0 parts by mass of the (meth)acrylate resin in the formed hard coating layer is 2.0 parts by mass, and the ratio of the ultraviolet light absorber in the liquid composition for forming the hard coating layer can be changed within the range of 5.0 parts by mass and 30.0 parts by mass. The ratio of the hindered amine light stabilizer and the ratio of the ultraviolet light absorber in the acrylate resin are changed in various ways. In addition, the same outer window film as the above-mentioned outer window film is manufactured and tested and evaluated with the same specifications, and the same results as above can still be obtained.

[0261] In addition, the mixing ratio of the ultraviolet absorber (UV-24) with a benzophenone structure and the ultraviolet absorber (Tinuvin 477) with a hydroxyphenyltriazine structure in the hard coating layer was variously changed in the range of 1.0:2.0d to 2.0:1.0 by mass ratio, and various changes were made in the range of 0 to 2.0:1.0. In addition, by manufacturing an outer window film of the same format as the above-mentioned outer window film and testing and evaluating it with the same specifications, the same results as above can still be obtained.

[0262] In addition, the thickness of the hard coating layer was varied in the range of 0.1 μm to 20 μm. In addition, the same results as above were obtained by manufacturing an exterior window film of the same specification as the above exterior window film and conducting tests and evaluations with the same specifications.

[0263] [Industrial Applicability]

[0264] According to the present invention, in an exterior window film provided with a hard coating layer, a exterior window film having excellent weather resistance and ensuring transparency, preventing cracks from being generated in the hard coating layer when rolled into a roll is provided. Therefore, the present invention has industrial applicability.

[0265] [Explanation of symbols]

[0266] 1: Exterior window film

[0267] 2: Base material

[0268] 3: Hard coating

[0269] 4: Adhesive layer

[0270] 10: Peel off liner.

Claims

1. An exterior window film, characterized in that: A method for preparing a substrate comprising: providing a substrate, a hard coating layer disposed on one side of the substrate, and an adhesive layer disposed on a side of the substrate opposite to the hard coating layer. The hard coating layer is composed of a material containing a (meth)acrylate resin having urethane (meth)acrylate as a constituent component, a hindered amine light stabilizer, and a UV absorber. The ratio of the hindered amine light stabilizer is 2.0 parts by mass or more and 15.0 parts by mass or less, and the ratio of the ultraviolet absorber is 5.0 parts by mass or more and 30.0 parts by mass or less, relative to 100.0 parts by mass of the (meth)acrylate resin. 2 . The exterior window film according to claim 1 , comprising a compound having a benzophenone structure and a compound having a hydroxyphenyltriazine structure as the ultraviolet absorber.

3. The exterior window film according to claim 2, wherein: The ratio of the content of the compound having a benzophenone structure to the content of the compound having a hydroxyphenyltriazine structure in the hard coating layer is 1.0:2.0 or more and 2.0:1.0 or less.

4. The exterior window film according to any one of claims 1 to 3, wherein: The (meth)acrylate resin is formed by polymerizing the urethane (meth)acrylate using a photopolymerization initiator.

5. The exterior window film according to claim 4, wherein: The photopolymerization initiator is a triphenylphosphine oxide compound. The exterior window film according to claim 1 , wherein the hard coating layer has a thickness of 0.1 μm or more and 20 μm or less.

7. The exterior window film according to claim 1, wherein: The substrate is made of a material containing polyester.

Citation Information

Patent Citations

  • Light-fast hard coat material

    CN109642000A

  • Hard coat film having ultraviolet absorptivity

    JP2009006513A

  • Method for manufacturing light control film

    JP2014137575A

  • Ultraviolet-curable resin composition and weather-resistant hard coat film

    JP2018100353A