Solid composition, circuit board, and method for producing solid composition

By melt-blending perfluorinated fluoropolymers with surface-treated anisotropic fillers, a solid composition with low linear expansion and good formability is formed, which solves the problems of formability and linear expansion of fluoropolymers in the prior art and is suitable for circuit boards made of low dielectric materials.

CN119013345APending Publication Date: 2024-11-22DAIKIN INDUSTRIES LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380032842.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-07
Filing Date
2023-03-27
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing technologies struggle to provide solid compositions and circuit boards with low linear expansion and good formability, especially when using fluoropolymers, where it is difficult to reduce the linear expansion.

Method used

A solid composition is formed by using perfluorinated fluoropolymers and surface-treated anisotropic fillers, such as talc and boron nitride, surface-treated with a silane coupling agent, and then melt-blending them.

Benefits of technology

A solid composition with low linear expansion and good formability has been achieved, which is suitable for circuit boards. It has the characteristics of low dielectric constant and low dielectric loss tangent, and is suitable for printed circuit boards, laminated circuit boards and high frequency boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005072973670000071
    Figure BDA0005072973670000071
  • Figure BDA0005072973670000072
    Figure BDA0005072973670000072
  • Figure BDA0005072973670000191
    Figure BDA0005072973670000191
Patent Text Reader

Abstract

Provided are a solid composition having a low linear expansion coefficient and good moldability, a circuit board, and a method for producing the solid composition. A solid composition containing a perfluorinated fluororesin and an anisotropic filler surface-treated with a silane coupling agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a solid composition, a circuit substrate, and a method for producing the solid composition. Background Art

[0002] As communication speeds up, low-dielectric and low-loss materials are required for circuit boards used in electrical equipment, electronic equipment, communication equipment, etc. Fluororesins have been studied as such materials, but the problem of using fluororesins is to reduce the linear expansion coefficient.

[0003] Patent Document 1 describes a dielectric resin composition containing an inorganic substance dispersed in a thermoplastic resin and / or a thermosetting resin.

[0004] Patent Document 2 describes a dispersion containing a tetrafluoroethylene polymer powder, an anisotropic filler, and a liquid dispersion medium.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2015-40296

[0008] Patent Document 2: International Publication No. 2021 / 112164 Summary of the invention

[0009] Problems to be solved by the invention

[0010] An object of the present disclosure is to provide a solid composition having a low linear expansion coefficient and good moldability, a circuit board, and a method for producing the solid composition.

[0011] Means for solving problems

[0012] This disclosure (1)

[0013] A solid composition (hereinafter also referred to as "the solid composition of the present disclosure") contains a perfluoro-based fluororesin and an anisotropic filler surface-treated with a silane coupling agent.

[0014] This disclosure (2)

[0015] The solid composition as described in (1) of the present disclosure, wherein the anisotropic filler is talc and / or boron nitride.

[0016] This disclosure (3)

[0017] The solid composition according to (1) or (2) of the present disclosure, wherein the anisotropic filler has a Mohs hardness of 4 or less.

[0018] This disclosure (4)

[0019] The solid composition according to any one of (1) to (3) of the present disclosure, wherein the silane coupling agent has at least one selected from the group consisting of a fluorine-containing group, an amino group, a vinyl group, and an epoxy group.

[0020] This disclosure (5)

[0021] The solid composition as described in any one of (1) to (4) of the present disclosure, wherein the unstable terminal groups of the perfluoro-based fluororesin are 6 The number of carbon atoms is less than 50.

[0022] The unstable terminal group is at least one selected from the group consisting of -CF2H, -COF, -COOH, -COOCH3, -CONH2 and -CH2OH present at the main chain terminal of the perfluoro-based fluororesin.

[0023] This disclosure (6)

[0024] The solid composition according to any one of (1) to (5) of the present disclosure, wherein the perfluoro-based fluororesin is at least one selected from the group consisting of polytetrafluoroethylene, tetrafluoroethylene / perfluoro(alkyl vinyl ether) copolymers, and tetrafluoroethylene / hexafluoropropylene copolymers.

[0025] This disclosure (7)

[0026] The solid composition according to any one of (1) to (6) of the present disclosure, wherein in an image analysis using laser microscope observation, voids with a width of 30 μm or more are present per 1 mm 2 There are less than 30 of them in the area.

[0027] This disclosure (8)

[0028] The solid composition as described in any one of (1) to (7) of the present disclosure, wherein the reduction rate of the linear expansion coefficient of the solid composition at 20°C to 200°C is 25% or more relative to the linear expansion coefficient of the perfluoro-based fluororesin at 20°C to 200°C.

[0029] This disclosure (9)

[0030] The solid composition according to any one of (1) to (8) of the present disclosure, wherein the dielectric loss tangent at 25° C. and 10 GHz is 0.003 or less.

[0031] This disclosure (10)

[0032] The solid composition according to any one of (1) to (9) of the present disclosure, which is a film or a sheet.

[0033] This disclosure (11)

[0034] The solid composition according to any one of (1) to (10) of the present disclosure is an insulating material for a circuit board.

[0035] This disclosure (12)

[0036] The solid composition as described in (11) of the present disclosure, wherein the insulating material of the circuit substrate is a low dielectric material.

[0037] This disclosure (13)

[0038] A circuit board (hereinafter also referred to as "circuit board of the present disclosure") comprising the solid composition according to any one of (1) to (12) of the present disclosure and a conductive layer.

[0039] This disclosure (14)

[0040] The circuit substrate as described in (13) of the present disclosure, wherein the conductive layer is made of metal.

[0041] This disclosure (15)

[0042] The circuit board according to the present disclosure (14), wherein the surface roughness Rz of the metal surface on the solid composition side is 2.0 μm or less.

[0043] This disclosure (16)

[0044] The circuit substrate according to (14) or (15) of the present disclosure, wherein the metal is copper.

[0045] This disclosure (17)

[0046] The circuit substrate as described in any one of (13) to (16) of the present disclosure is a printed circuit board, a laminated circuit board or a high-frequency board.

[0047] This disclosure (18)

[0048] A method for producing a solid composition (hereinafter also referred to as "the production method of the present disclosure") is the method for producing a solid composition according to any one of (1) to (12) of the present disclosure, wherein the perfluoro-based fluororesin and the anisotropic filler are melt-kneaded to obtain the solid composition.

[0049] Effects of the Invention

[0050] According to the present disclosure, a solid composition having a low linear expansion coefficient and good moldability, a circuit board, and a method for producing the solid composition can be provided. DETAILED DESCRIPTION

[0051] In the present specification, the "organic group" refers to a group containing one or more carbon atoms, or a group formed by removing one hydrogen atom from an organic compound.

[0052] Examples of the "organic group" include:

[0053] an alkyl group which may have one or more substituents,

[0054] an alkenyl group which may have one or more substituents, an alkynyl group which may have one or more substituents, a cycloalkyl group which may have one or more substituents, a cycloalkenyl group which may have one or more substituents, a cycloalkadienyl group which may have one or more substituents, an aryl group which may have one or more substituents, an aralkyl group which may have one or more substituents, a non-aromatic heterocyclic group which may have one or more substituents, a heteroaryl group which may have one or more substituents, a cyano group,

[0055] Formyl,

[0056] RaO-,

[0057] RaCO-,

[0058] RaSO2-,

[0059] RaCOO-

[0060] RaNRaCO-,

[0061] RaCONRa-

[0062] RaOCO-,

[0063] RaOSO2-, and

[0064] RaNRbSO2-

[0065] (In these formulas, Ra is independently an alkyl group which may have one or more substituents, an alkenyl group which may have one or more substituents, an alkynyl group which may have one or more substituents, a cycloalkyl group which may have one or more substituents, a cycloalkenyl group which may have one or more substituents, a cycloalkadienyl group which may have one or more substituents, an aryl group which may have one or more substituents, an aralkyl group which may have one or more substituents,

[0066] A non-aromatic heterocyclic group which may have one or more substituents, or

[0067] a heteroaryl group which may have one or more substituents,

[0068] Rb is independently H or an alkyl group which may have one or more substituents).

[0069] As the organic group, an alkyl group which may have one or more substituents is preferred.

[0070] The present disclosure is described in detail below.

[0071] The solid composition disclosed herein contains a perfluoro-based fluororesin and an anisotropic filler surface-treated with a silane coupling agent.

[0072] The solid composition of the present disclosure contains the anisotropic filler, and thus has a low linear expansion coefficient and good moldability despite containing a perfluoro-based fluororesin.

[0073] Furthermore, by blending the anisotropic filler, when the solid composition of the present disclosure is made into pellets, the internal voids are reduced, thereby improving the mechanical properties of a film or sheet formed from the pellets.

[0074] Furthermore, by blending the above-mentioned anisotropic filler, electrical properties can be improved.

[0075] In addition, as described in Patent Document 1, when anisotropic fillers are melt-kneaded with fluororesins, strong stress is usually required, which sometimes impairs the properties of the anisotropic fillers (such as the effect of improving electrical properties). However, since the anisotropic fillers are surface-treated with a silane coupling agent, their properties can be maintained even when melt-kneaded with fluororesins. Moreover, by melt-kneading, the anisotropic fillers can be well dispersed in the fluororesins, making the electrical properties and the like better.

[0076] Furthermore, since the solid composition of the present disclosure is solid, it has advantages in that the production process is reduced and the film thickness can be easily increased compared to the dispersion described in Patent Document 2.

[0077] Furthermore, since the solid composition of the present disclosure uses a perfluorinated fluororesin, it is possible to obtain excellent electrical properties compared to other fluororesins such as ethylene / tetrafluoroethylene copolymer (ETFE).

[0078] The above-mentioned perfluorinated fluororesin is a copolymer with a fluorinated monomer such as a perfluorinated monomer as the main component. It is a fluorinated resin with very few hydrogen atoms bonded to carbon atoms in the repeating units constituting the main chain, and may also have hydrogen atoms bonded to carbon atoms in positions other than the repeating units constituting the main chain, such as the terminal structure. In addition, if the content of the fluorinated monomer in the resin is 90 mol% or more, monomers other than the fluorinated monomer may also be copolymerized. The content of the fluorinated monomer is preferably 95 mol% or more, more preferably 99 mol% or more, and may also be 100 mol%.

[0079] As the perfluoro-based fluororesin, a polymer of tetrafluoroethylene [TFE] as a perfluoromonomer, a copolymer of tetrafluoroethylene [TFE] and a comonomer copolymerizable with TFE, or the like can be used.

[0080] It should be noted that, in the present specification, the above-mentioned “perfluoromonomer” refers to a monomer in which all hydrogen atoms bonded to carbon atoms are substituted with fluorine atoms.

[0081] The comonomer is not particularly limited as long as it is a monomer that can copolymerize with TFE and does not contain a hydrogen atom bonded to a carbon atom constituting the main chain, and examples thereof include hexafluoropropylene [HFP], fluoroalkyl vinyl ethers described below, fluoroalkyl ethylenes, and the general formula (100): CH2=CFRf 101 (Where Rf 101 The fluorinated monomers may be fluorinated monomers represented by a fluorinated monomer represented by a linear or branched fluorinated alkyl group having 1 to 12 carbon atoms, fluorinated alkyl allyl ethers, etc. In addition, monomers other than the fluorinated monomers may include itaconic anhydride, citraconic anhydride, 5-norbornene-2,3-dicarboxylic anhydride, maleic anhydride, etc. The above-mentioned comonomers may be used alone or in combination of two or more.

[0082] As the fluoroalkyl vinyl ether, for example, at least one selected from the group consisting of the following substances is preferred:

[0083] General formula (110): CF2=CF-ORf 111

[0084] (Where Rf 111 represents a perfluorinated organic group. ) represents a fluorinated monomer;

[0085] General formula (120): CF2=CF-OCH2-Rf 121

[0086] (Where Rf 121 represents a fluorinated monomer represented by a perfluoroalkyl group having 1 to 5 carbon atoms;

[0087] General formula (130): CF2=CFOCF2ORf 131

[0088] (Where Rf 131 A fluorine-containing monomer represented by a linear or branched perfluoroalkyl group having 1 to 6 carbon atoms, a cyclic perfluoroalkyl group having 5 to 6 carbon atoms, or a linear or branched perfluorooxyalkyl group having 2 to 6 carbon atoms and containing 1 to 3 oxygen atoms;

[0089] General formula (140): CF2=CFO(CF2CF(Y 141 )O) m (CF2) n F

[0090] (Where Y 141 represents a fluorine atom or a trifluoromethyl group. m is an integer from 1 to 4. n is an integer from 1 to 4. ) represents a fluorine-containing monomer; and

[0091] General formula (150): CF2=CF-O-(CF2CFY 151 -O) n -(CFY 152 ) m -A 151

[0092] (Where Y 151 represents a fluorine atom, a chlorine atom, a -SO2F group or a perfluoroalkyl group. The perfluoroalkyl group may contain an ether oxygen and a -SO2F group. n represents an integer of 0 to 3. 151 Can be the same or different. 152 represents a fluorine atom, a chlorine atom or a -SO2F group. m represents an integer of 1 to 5. m Y 152 Can be the same or different. 151 Represents -SO2X 151 、-COZ 151 or-POZ 152 Z 153 .X 151 Indicates F, Cl, Br, I, -OR 151 or -NR 152 R 153 . Z 151 , Z 152 and Z 153 Same or different, indicates -NR 154 R 155 OR 156 . R 151 , R 152 , R 153 , R 154 , R 155 and R 156 are the same or different and represent H, ammonium, an alkali metal, an alkyl group containing or not containing a fluorine atom, an aryl group or a sulfonyl group-containing group. ) is a fluorine-containing monomer.

[0093] In the present specification, the "perfluoroorganic group" refers to an organic group in which all hydrogen atoms bonded to carbon atoms are substituted with fluorine atoms. The perfluoroorganic group may have an ether oxygen.

[0094] Examples of the fluorinated monomer represented by the general formula (110) include Rf 111 A fluorine-containing monomer having a perfluoroalkyl group having 1 to 10 carbon atoms. The perfluoroalkyl group preferably has 1 to 5 carbon atoms.

[0095] Examples of the perfluoro organic group in the general formula (110) include a perfluoromethyl group, a perfluoroethyl group, a perfluoropropyl group, a perfluorobutyl group, a perfluoropentyl group, and a perfluorohexyl group.

[0096] Examples of the fluorine-containing monomer represented by the general formula (110) include the following fluorine-containing monomers:

[0097] In the above general formula (110), Rf 111 A fluorinated monomer which is a perfluoro(alkoxyalkyl) group having 4 to 9 carbon atoms;

[0098] R 111 Is the following formula:

[0099] [Chemistry 1]

[0100]

[0101] (wherein m represents 0 or an integer of 1 to 4.) a fluorine-containing monomer of a group represented by;

[0102] R 111 Is the following formula:

[0103] [Chemistry 2]

[0104]

[0105] (wherein n represents an integer of 1 to 4); and the like.

[0106] As the fluorinated monomer represented by the general formula (110), perfluoro(alkyl vinyl ether) [PAVE] is preferred, and the general formula (160): CF2=CF-ORf is more preferred. 161

[0107] (Where Rf 161 represents a perfluoroalkyl group having 1 to 10 carbon atoms. ) is a fluorine-containing monomer. Rf 161 A perfluoroalkyl group having 1 to 5 carbon atoms is preferred.

[0108] The fluoroalkyl vinyl ether is preferably at least one selected from the group consisting of fluorinated monomers represented by general formulae (160), (130) and (140).

[0109] As the fluorinated monomer (PAVE) represented by the general formula (160), it is preferred to select at least one from the group consisting of perfluoro(methyl vinyl ether) [PMVE], perfluoro(ethyl vinyl ether) [PEVE] and perfluoro(propyl vinyl ether) [PPVE], and more preferably to select at least one from the group consisting of perfluoro(methyl vinyl ether) and perfluoro(propyl vinyl ether).

[0110] The fluorinated monomer represented by the general formula (130) is preferably at least one selected from the group consisting of CF2=CFOCF2OCF3, CF2=CFOCF2OCF2CF3 and CF2=CFOCF2OCF2CF2OCF3.

[0111] The fluorinated monomer represented by the general formula (140) is preferably at least one selected from the group consisting of CF2=CFOCF2CF(CF3)O(CF2)3F, CF2=CFO(CF2CF(CF3)O)2(CF2)3F and CF2=CFO(CF2CF(CF3)O)2(CF2)2F.

[0112] The fluorine-containing monomer represented by the general formula (150) is preferably at least one selected from the group consisting of CF2=CFOCF2CF2SO2F, CF2=CFOCF2CF(CF3)OCF2CF2SO2F, CF2=CFOCF2CF(CF2CF2SO2F)OCF2CF2SO2F and CF2=CFOCF2CF(SO2F)2.

[0113] As the fluorinated monomer represented by the general formula (100), Rf is preferably 101 A fluorinated monomer which is a linear fluoroalkyl group, more preferably Rf 101 It is a fluorinated monomer containing a straight-chain perfluoroalkyl group. 101 The number of carbon atoms is preferably 1 to 6. Examples of the fluorinated monomer represented by the general formula (100) include CH2=CFCF3, CH2=CFCF2CF3, CH2=CFCF2CF2CF3, CH2=CFCF2CF2CF3, CH2=CFCF2CF2CF2H, CH2=CFCF2CF2CF2CF3, CHF=CHCF3 (E-form), CHF=CHCF3 (Z-form), etc. Among them, 2,3,3,3-tetrafluoropropylene represented by CH2=CFCF3 is preferred.

[0114] As the fluoroalkylethylene, preferably

[0115] General formula (170): CH2=CH-(CF2) n -X 171

[0116] (Where X 171 is H or F, n is an integer of 3 to 10), more preferably selected from CH2=CH-C4F9 and CH2=CH-C6F 13 At least one of the group consisting of.

[0117] Examples of the fluoroalkyl allyl ether include

[0118] General formula (170): CF2=CF-CF2-ORf 111

[0119] (Where Rf 111 represents a perfluorinated organic group. ) represents a fluorinated monomer.

[0120] Rf of general formula (170) 111 With the Rf of general formula (110) 111 Same as Rf 111 , preferably a perfluoroalkyl group having 1 to 10 carbon atoms or a perfluoroalkoxyalkyl group having 1 to 10 carbon atoms. As the fluoroalkyl allyl ether represented by the general formula (170), at least one selected from the group consisting of CF2=CF-CF2-O-CF3, CF2=CF-CF2-O-C2F5, CF2=CF-CF2-O-C3F7 and CF2=CF-CF2-O-C4F9 is preferred, at least one selected from the group consisting of CF2=CF-CF2-O-C2F5, CF2=CF-CF2-O-C3F7 and CF2=CF-CF2-O-C4F9 is more preferred, and CF2=CF-CF2-O-CF2CF3 is further preferred.

[0121] As the above-mentioned comonomer, from the aspect of being able to reduce the deformation of the solid composition and the aspect of being able to reduce the linear expansion coefficient, a monomer having a perfluorovinyl group is preferred, more preferably at least one selected from the group consisting of perfluoro(alkyl vinyl ether) (PAVE), hexafluoropropylene (HFP) and perfluoroallyl ether, further preferably at least one selected from the group consisting of PAVE and HFP, and from the aspect of being able to suppress the deformation of the solid composition during solder processing, PAVE is particularly preferred.

[0122] The perfluorinated fluororesin preferably contains the comonomer units totaling 0.1% by mass or more of the total monomer units, more preferably 1.0% by mass or more, and further preferably 1.1% by mass or more. In addition, the total amount of the comonomer units is preferably 30% by mass or less of the total monomer units, more preferably 20% by mass or less, and further preferably 15% by mass or less.

[0123] The amount of the above comonomer units is determined by 19 The measurement was carried out by F-NMR method.

[0124] As the above-mentioned perfluoro-based fluororesin, from the aspect of being able to reduce the deformation of the solid composition and being able to reduce the linear expansion coefficient, it is preferably at least one selected from the group consisting of polytetrafluoroethylene (PTFE), tetrafluoroethylene (TFE) / perfluoro(alkyl vinyl) ether (PAVE) copolymer (PFA) and tetrafluoroethylene (TFE) / hexafluoropropylene (HFP) copolymer (FEP), more preferably at least one selected from the group consisting of PFA and FEP, and even more preferably PFA.

[0125] In the case where the perfluorinated fluororesin is PFA containing TFE units and PAVE units, it is preferred to contain 0.1% to 12% by mass of PAVE units relative to all polymerized units. The amount of PAVE units relative to all polymerized units is more preferably 0.3% by mass or more, further preferably 0.7% by mass or more, further more preferably 1.0% by mass or more, particularly preferably 1.1% by mass or more, and more preferably 8.0% by mass or less, further preferably 6.5% by mass or less, particularly preferably 6.0% by mass or less.

[0126] It should be noted that the amount of the above PAVE unit is 19 The measurement was carried out by F-NMR method.

[0127] When the perfluororesin is FEP containing TFE units and HFP units, the mass ratio of TFE units to HFP units (TFE / HFP) is preferably 70 to 99 / 1 to 30 (mass %), and more preferably 85 to 95 / 5 to 15 (mass %).

[0128] The FEP contains 1% by mass or more, preferably 1.1% by mass or more, of HFP units based on all monomer units.

[0129] The above-mentioned FEP preferably contains TFE units, HFP units, and perfluoro(alkyl vinyl ether) [PAVE] units.

[0130] Examples of the PAVE unit contained in the FEP include the same units as those constituting the PFA, among which PPVE is preferred.

[0131] The above-mentioned PFA does not include an HFP unit, and thus is different from FEP including a PAVE unit in this point.

[0132] When the FEP contains TFE units, HFP units, and PAVE units, the mass ratio (TFE / HFP / PAVE) is preferably 70 to 99.8 / 0.1 to 25 / 0.1 to 25 (mass %). Within the above range, excellent heat resistance and chemical resistance are achieved.

[0133] The mass ratio (TFE / HFP / PAVE) is more preferably 75 to 98 / 1.0 to 15 / 1.0 to 10 (mass %).

[0134] The FEP contains HFP units and PAVE units in an amount of 1% by mass or more, preferably 1.1% by mass or more, of all monomer units in total.

[0135] In the FEP comprising TFE units, HFP units, and PAVE units, the HFP units preferably account for 25% by mass or less of all monomer units.

[0136] When the content of the HFP unit is within the above range, a solid composition having excellent heat resistance can be obtained.

[0137] The content of the HFP unit is more preferably 20% by mass or less, further preferably 18% by mass or less, and particularly preferably 15% by mass or less. In addition, the content of the HFP unit is preferably 0.1% by mass or more, more preferably 1% by mass or more, and particularly preferably 2% by mass or more.

[0138] It should be noted that the content of HFP units can be 19 The measurement was carried out by F-NMR method.

[0139] The content of the PAVE unit is more preferably 20% by mass or less, and further preferably 10% by mass or less. It is particularly preferably 3% by mass or less. In addition, the content of the PAVE unit is preferably 0.1% by mass or more, and more preferably 1% by mass or more. It should be noted that the content of the PAVE unit can be determined by 19 The measurement was carried out by F-NMR method.

[0140] The above-mentioned FEP may further contain other ethylenic monomer (α) units.

[0141] As other olefinic monomer (α) units, there are no particular limitations as long as they are monomer units copolymerizable with TFE, HFP and PAVE, and examples thereof include fluorinated olefinic monomers such as vinyl fluoride [VF], vinylidene fluoride [VdF], and chlorotrifluoroethylene [CTFE]; and non-fluorinated olefinic monomers such as ethylene, propylene, and alkyl vinyl ether.

[0142] When the FEP contains TFE units, HFP units, PAVE units and other ethylenic monomer (α) units, the mass ratio (TFE / HFP / PAVE / other ethylenic monomer (α)) is preferably 70 to 98 / 0.1 to 25 / 0.1 to 25 / 0.1 to 10 (mass %).

[0143] The FEP contains monomer units other than TFE units in an amount of 1% by mass or more, preferably 1.1% by mass or more, of all monomer units.

[0144] The perfluorinated fluorine resin is preferably the PFA and the FEP. In other words, the PFA and the FEP may be mixed and used. The mass ratio of the PFA to the FEP (PFA / FEP) is preferably 90 / 10 to 30 / 70, more preferably 90 / 10 to 50 / 50.

[0145] The PFA and FEP can be produced, for example, by appropriately mixing monomers to be the constituent units and additives such as a polymerization initiator and subjecting them to conventionally known methods such as emulsion polymerization and suspension polymerization.

[0146] The unstable terminal groups of the above perfluorinated fluororesin are relative to each 1×10 6 The number of carbon atoms is preferably less than 700, more preferably less than 300, further preferably less than 100, and particularly preferably less than 50. The lower limit is not particularly limited. Within the above range, the electrical properties become better.

[0147] It should be noted that, from the perspective of electrical properties (particularly dielectric loss tangent), the unstable terminal group is preferably at least one selected from the group consisting of -CF2H, -COF, -COOH, -COOCH3, -CONH2 and -CH2OH present at the main chain terminal of the perfluorinated fluororesin. They can associate with water.

[0148] The -CF2H terminal of the above-mentioned perfluorinated fluororesin is relative to 1×10 6 The number of carbon atoms is preferably less than 600, more preferably less than 200, further preferably less than 100, and particularly preferably less than 30. The lower limit is not particularly limited. Within the above range, electrical properties (particularly dielectric loss tangent) become better.

[0149] The number of the unstable terminal groups can be reduced by, for example, subjecting the perfluorinated fluororesin to a fluorination treatment.

[0150] The fluorination treatment can be carried out by a known method, for example, by bringing a fluorine-containing compound into contact with a fluorine-containing resin that has not been fluorinated.

[0151] In addition, as the above-mentioned fluorine-containing compounds, there can be mentioned fluorine radical sources that generate fluorine radicals under fluorination treatment conditions, such as F2 gas, CoF3, AgF2, UF6, OF2, N2F2, CF3OF and fluorinated halogens (such as IF5, ClF3) and the like.

[0152] The number of the above-mentioned unstable terminal groups can be measured by infrared spectroscopy. Specifically, first, a film-like sample with a thickness of 0.25 mm to 0.3 mm composed of the above-mentioned perfluoro-based fluororesin is prepared. The sample is analyzed by Fourier transform infrared spectroscopy to obtain the infrared absorption spectrum of the above-mentioned copolymer, and a differential spectrum with the background spectrum of complete fluorination treatment without the presence of unstable terminal groups is obtained. According to the following formula (A), the number of unstable terminal groups per 10 in the above-mentioned copolymer is calculated from the absorption peak of the specific unstable terminal group shown in the differential spectrum. 6 The number N of unstable terminal groups per carbon atom.

[0153] N=I×K / t(A)

[0154] I: Absorbance

[0155] K: Correction coefficient

[0156] t: film (sample) thickness (mm)

[0157] The sample is a sample cut out from a pellet or a sheet obtained by molding the perfluorinated fluororesin.

[0158] The melting point of the perfluorinated fluororesin is preferably 240° C. to 340° C. This allows easy melt kneading.

[0159] The melting point of the perfluorinated fluororesin is more preferably 318°C or lower, further preferably 315°C or lower, and more preferably 245°C or higher, further preferably 250°C or higher.

[0160] The melting point of the perfluorinated fluororesin is a temperature corresponding to the maximum value in the heat of fusion curve when the temperature is increased at a rate of 10° C. / min using a differential scanning calorimeter [DSC].

[0161] The perfluoro-based fluororesin preferably has a melt flow rate (MFR) of 0.1 g / 10 min to 100 g / 10 min at 372° C. This allows easy melt kneading.

[0162] The MFR is more preferably 0.5 g / 10 min or more, and even more preferably 1.5 g / 10 min or more, and is more preferably 80 g / 10 min or less, and even more preferably 40 g / 10 min or less.

[0163] MFR is a value obtained as the mass (g / 10 minutes) of a polymer flowing out from a nozzle having an inner diameter of 2 mm and a length of 8 mm at 372° C. and a load of 5 kg per 10 minutes using a melt flow indexer (manufactured by Yasuda Seiki Co., Ltd.) in accordance with ASTM D1238.

[0164] The relative dielectric constant and dielectric loss tangent of the above-mentioned perfluorinated fluororesin are not particularly limited. At 25°C and a frequency of 10 GHz, the relative dielectric constant can be 4.5 or less, preferably 4.0 or less, more preferably 3.5 or less, and further preferably 2.5 or less. In addition, the dielectric loss tangent can be 0.01 or less, preferably 0.008 or less, and more preferably 0.005 or less. Their lower limits are not particularly limited. For example, the relative dielectric constant can be 1.0 or more, and the dielectric loss tangent can be 0.0001 or more.

[0165] The content of the perfluorinated fluororesin is preferably 40% to 90% by mass relative to the solid composition. The content of the perfluorinated fluororesin is more preferably 50% by mass or more, further preferably 60% by mass or more, particularly preferably 70% by mass or more, and more preferably 85% by mass or less, more preferably 80% by mass or less.

[0166] The anisotropic filler is a particle having anisotropic shape (diameter varies depending on the direction), and examples thereof include carbon, mica, clay, talc, etc. In addition, nitrides such as boron nitride and silicon nitride may also be used. Among them, talc and boron nitride are preferred, and talc is more preferred, from the perspective of good moldability.

[0167] The above-mentioned anisotropic filler may be used alone or in combination of two or more.

[0168] From the viewpoint of good dispersibility, the Mohs hardness of the anisotropic filler is preferably 4 or less. The Mohs hardness of the anisotropic filler is more preferably 3 or less, and is preferably 1 or more.

[0169] The above-mentioned Mohs hardness is an old Mohs hardness with a scale of 1 to 10, and can be measured using a Mohs hardness meter.

[0170] The average particle size of the anisotropic filler is preferably 0.1 μm to 50 μm, more preferably 1 μm or more, further preferably 3 μm or more, particularly preferably 5 μm or more, and more preferably 30 μm or less, further preferably 20 μm or less, particularly preferably 15 μm or less.

[0171] The above average particle size is a value measured by a laser diffraction / scattering method.

[0172] The aspect ratio of the anisotropic filler is preferably 1 to 5000. The lower limit of the aspect ratio is more preferably 10, and even more preferably 20. The upper limit of the aspect ratio is more preferably 1000, and even more preferably 200.

[0173] The aspect ratio is a value obtained by dividing the average particle size of the anisotropic filler by the average minor diameter (the average value of the length in the short-side direction).

[0174] The shape of the anisotropic filler is not particularly limited, and examples thereof include flaky, plate-like, needle-like, granular, spherical, columnar, conical, truncated cone-like, polyhedral, and hollow shapes.

[0175] The anisotropic filler is surface treated with a silane coupling agent. The surface treatment method is not particularly limited, and a general method can be used.

[0176] The above-mentioned silane coupling agents may be used alone or in combination of two or more.

[0177] From the perspective of improving affinity with the resin, the functional group possessed by the above-mentioned silane coupling agent is preferably at least one selected from the group consisting of a fluorine-containing group, an amino group, a vinyl group and an epoxy group, more preferably at least one selected from the group consisting of a fluorine-containing group, an amino group and a vinyl group, and further preferably a fluorine-containing group and an amino group.

[0178] The content of the anisotropic filler is preferably 10% to 60% by mass relative to the solid composition, more preferably 15% by mass or more, further preferably 20% by mass or more, and more preferably 50% by mass or less, further preferably 45% by mass or less.

[0179] The solid composition of the present disclosure may contain other components as required. As other components, fillers, crosslinking agents, antistatic agents, heat stabilizers, foaming agents, foaming nucleating agents, antioxidants, surfactants, photopolymerization initiators, anti-wear agents, surface modifiers, resins (wherein, excluding the above-mentioned modified fluororesins), liquid crystal polymers and other additives may be cited.

[0180] As the other component, an inorganic filler other than the anisotropic filler is preferred. By including the inorganic filler, the effect of improving the strength and reducing the linear expansion coefficient can be obtained.

[0181] Specific examples of the above-mentioned inorganic fillers include inorganic compounds (excluding zinc oxide) such as zinc oxide, silicon dioxide (more specifically, crystalline silicon dioxide, fused silica, spherical fused silica, etc.), titanium oxide, zirconium oxide, tin oxide, silicon nitride, silicon carbide, boron nitride, calcium carbonate, calcium silicate, potassium titanate, aluminum nitride, indium oxide, aluminum oxide, antimony oxide, cerium oxide, magnesium oxide, iron oxide, and tin-doped indium oxide (ITO). In addition, minerals such as montmorillonite, talc, mica, boehmite, kaolin, montmorillonite, xonotlite, vermiculite, and sericite can be cited. Other inorganic fillers include carbon compounds such as carbon black, acetylene black, ketjen black, and carbon nanotubes; metal hydroxides such as aluminum hydroxide and magnesium hydroxide; various glasses such as glass beads, glass flakes, and glass balls.

[0182] The inorganic filler may be one kind or two or more kinds.

[0183] The inorganic filler may be used directly in the form of powder or in the form of a powder dispersed in a resin.

[0184] The inorganic filler preferably has ultraviolet light absorptivity. Having ultraviolet light absorptivity means that the absorbance of light having a wavelength of 355 nm is 0.1 or more.

[0185] The light absorbance is a value measured in a reflection arrangement using an ultraviolet-visible-near-infrared spectrophotometer (eg, "V-770" manufactured by JASCO Corporation) on the inorganic filler powder filled to a thickness of 100 μm.

[0186] Examples of the inorganic filler having ultraviolet light absorbing properties include zinc oxide and titanium oxide, and zinc oxide is preferred.

[0187] The shape of the inorganic filler is not particularly limited, and the same shapes as those of the anisotropic filler may be mentioned.

[0188] When the solid composition of the present disclosure contains the above-mentioned inorganic filler, the content of the above-mentioned inorganic filler is preferably 0.01% by mass to 5.0% by mass relative to the above-mentioned solid composition. The content of the above-mentioned inorganic filler is more preferably 0.1% by mass or more, further preferably 0.3% by mass or more, and more preferably 4.0% by mass or less, further preferably 3.0% by mass or less.

[0189] The average particle size of the inorganic filler is preferably 0.01 μm to 20 μm. If the average particle size is within the above range, there is less aggregation and good surface roughness can be obtained. The lower limit of the average particle size is more preferably 0.02 μm, and more preferably 0.03 μm. The upper limit of the average particle size is more preferably 5 μm, and more preferably 2 μm.

[0190] The above average particle size is a value measured by a laser diffraction / scattering method.

[0191] The inorganic filler may be a surface-treated inorganic filler, for example, an inorganic filler surface-treated with an organic silicon compound. The surface treatment with the organic silicon compound can reduce the dielectric constant of the inorganic filler.

[0192] The organosilicon compound is not particularly limited, and any conventionally known organosilicon compound can be used. For example, it is preferred that the organosilicon compound contains at least one selected from the group consisting of a silane coupling agent and an organosilazane.

[0193] The surface treatment amount of the above-mentioned organic silicon compound is preferably the amount of the surface treatment agent reacted on the surface of the inorganic filler per unit surface area (nm 2 ) is 0.1 to 10, more preferably 0.3 to 7.

[0194] The solid composition disclosed herein preferably has a void with a width of 30 μm or more per 1 mm in image analysis observed under a laser microscope. 2The number of voids is preferably 30 or less in the area. The number of voids is more preferably 25 or less, further preferably 20 or less, and may be 0. If it is within the above range, the formability (particularly the sheet formability and the wire drawing stability) becomes better.

[0195] It should be noted that the above-mentioned image analysis by laser microscope observation is performed on the cross section of pelletized solid composition of the present disclosure.

[0196] The linear expansion coefficient of the solid composition of the present disclosure at 20° C. to 200° C. is preferably 160 ppm / ° C. or less, and more preferably 120 ppm / ° C. or less. The lower limit is not particularly limited, and may be, for example, 100 ppm / ° C.

[0197] In addition, the reduction rate of the linear expansion coefficient of the solid composition of the present disclosure at 20°C to 200°C is preferably 25% or more, more preferably 40% or more, and further preferably 50% or more relative to the linear expansion coefficient of the above-mentioned perfluorinated fluororesin at 20°C to 200°C. The upper limit is not particularly limited, and may be, for example, 60%.

[0198] The relative dielectric constant of the solid composition of the present disclosure at 25°C and 10 GHz is preferably 5.0 or less, more preferably 4.0 or less, and further preferably 3.5 or less. The lower limit is not particularly set, and may be 1.0, for example. Within the above range, the composition can be suitably used for a circuit board.

[0199] The dielectric loss tangent of the solid composition of the present disclosure at 25°C and 10 GHz is preferably 0.003 or less, more preferably 0.002 or less, and further preferably 0.0015 or less. The lower limit is not particularly limited, and may be 0.0001, for example. Within the above range, the solid composition can be suitably used for a circuit board.

[0200] The shape of the solid composition of the present disclosure is not particularly limited, and examples thereof include pellets, films, sheets, etc. When used for a circuit board, films and sheets are preferred. Pellets can be used as a molding material.

[0201] The solid composition of the present disclosure can be suitably produced by a production method of obtaining the solid composition by melt-kneading the perfluoro-based fluororesin and the anisotropic filler. The present disclosure also provides the above production method.

[0202] It should be noted that the solid composition of the present disclosure can be manufactured by methods other than the above-mentioned manufacturing methods, such as injection molding, blow molding, inflation molding, vacuum / gas pressure molding. In addition, as long as it is dispersed or dissolved in a solvent, it can also be manufactured by paste extrusion, casting method, etc.

[0203] The apparatus used for the melt-kneading is not particularly limited, and a twin-screw extruder, a single-screw extruder, a multi-screw extruder, a tandem extruder, or the like can be used.

[0204] The melt kneading time is preferably 1 to 1800 seconds, more preferably 60 to 1200 seconds. If the time is too long, the fluororesin may be degraded, and if the time is too short, the zinc oxide may not be sufficiently dispersed.

[0205] The temperature of the melt kneading may be equal to or higher than the melting points of the perfluoro-based fluororesin and the anisotropic filler, and is preferably 240°C to 450°C, more preferably 260°C to 400°C.

[0206] The present inventors have found that the solid composition of the present disclosure comprising a perfluoro-based fluororesin and an anisotropic filler has a low linear expansion coefficient, excellent moldability, and good dispersibility. These properties are suitable for a material for a circuit board.

[0207] That is, the solid composition of the present disclosure is suitable for use as an insulating material (especially a low dielectric material) or a thermal conductive material for a circuit board.

[0208] It should be noted that, in this specification, "low dielectric material" refers to a material whose relative dielectric constant at 25°C and 10 GHz is less than 5.0 and whose dielectric loss tangent at 25°C and 10 GHz is less than 0.003, more preferably a material whose relative dielectric constant at 25°C and 10 GHz is less than 4.0 and whose dielectric loss tangent at 25°C and 10 GHz is less than 0.002, and further preferably a material whose relative dielectric constant at 25°C and 10 GHz is less than 3.5 and whose dielectric loss tangent at 25°C and 10 GHz is less than 0.0012.

[0209] The circuit substrate of the present disclosure comprises the solid composition of the present disclosure and a conductive layer.

[0210] As the conductive layer, metal is preferably used.

[0211] Examples of the metal include copper, stainless steel, aluminum, iron, silver, gold, and ruthenium. In addition, alloys thereof may also be used. Among them, copper is preferred.

[0212] As the copper, rolled copper, electrolytic copper, or the like can be used.

[0213] The surface roughness Rz of the metal on the side of the solid composition is preferably 2.0 μm or less. This improves the transmission loss when the solid composition and the metal are bonded together.

[0214] The surface roughness Rz is more preferably 1.8 μm or less, and further preferably 1.5 μm or less, and is more preferably 0.3 μm or more, and further preferably 0.5 μm or more.

[0215] In addition, the said surface roughness Rz is the value (maximum height roughness) calculated by the method of JIS C 6515-1998.

[0216] The thickness of the conductive layer may be, for example, 2 μm to 200 μm, and preferably 5 μm to 50 μm.

[0217] The conductive layer may be provided on only one surface of the layer including the solid composition of the present disclosure, or may be provided on both surfaces.

[0218] The thickness of the layer containing the solid composition of the present disclosure may be, for example, 1 μm to 1 mm, preferably 20 μm or more, more preferably 30 μm or more, further preferably 50 μm or more, and preferably 800 μm or less, more preferably 600 μm or less.

[0219] When forming a film from the dispersion described in Patent Document 2, it is generally difficult to make the film thickness 50 μm or more. However, when forming a film from the solid composition of the present disclosure, the film thickness can be easily made 50 μm or more.

[0220] The circuit board of the present disclosure may be a board in which a resin other than the perfluorinated fluororesin is further laminated on the solid composition of the present disclosure and the conductive layer.

[0221] As the resin other than the above-mentioned perfluorinated fluororesin, a thermosetting resin can be preferably used.

[0222] The thermosetting resin is preferably at least one selected from the group consisting of polyimide, modified polyimide, epoxy resin, and thermosetting modified polyphenylene ether, more preferably epoxy resin, modified polyimide, and thermosetting modified polyphenylene ether, and even more preferably epoxy resin and thermosetting modified polyphenylene ether.

[0223] The resin other than the above-mentioned perfluorinated fluororesin may be a resin other than a thermosetting resin.

[0224] As the resin other than the thermosetting resin, at least one selected from the group consisting of a liquid crystal polymer, polyphenylene ether, thermoplastic modified polyphenylene ether, a cycloolefin polymer, a cycloolefin copolymer, polystyrene, and syndiotactic polystyrene is preferred.

[0225] The thickness of the resin other than the perfluorinated fluororesin is preferably 5 μm or more, more preferably 10 μm or more, and is preferably 2000 μm or less, more preferably 1500 μm or less.

[0226] It should be noted that the resin other than the above-mentioned perfluororesin is preferably in the form of a sheet with a substantially constant thickness. However, when the above-mentioned perfluororesin has portions with different thicknesses, the above-mentioned thickness is obtained by measuring the thickness of the positions where the above-mentioned perfluororesin is divided into 10 portions at equal intervals along the length direction and averaging them.

[0227] The thickness of the circuit board of the present disclosure is preferably 20 μm or more, more preferably 30 μm or more, and is preferably 5000 μm or less, more preferably 3000 μm or less.

[0228] It should be noted that the shape of the circuit substrate of the present disclosure is preferably a sheet with a substantially constant thickness. However, when the substrate has portions with different thicknesses, the thicknesses of the portions where the substrate is divided into 10 portions at equal intervals along the length direction are measured and averaged.

[0229] The circuit board disclosed in the present invention is suitable for use as a printed circuit board, a laminated circuit board (multilayer board), or a high-frequency board.

[0230] The high-frequency circuit substrate is a circuit substrate that can work even in a high-frequency band. The high-frequency band can be a band above 1 GHz, preferably a band above 3 GHz, and more preferably a band above 5 GHz. The upper limit is not particularly limited, and can be a band below 100 GHz.

[0231] The circuit board of the present disclosure is preferably a sheet. The thickness of the circuit board of the present disclosure is preferably 10 μm to 3500 μm, more preferably 20 μm to 3000 μm.

[0232] Although the embodiments have been described above, it should be understood that various changes in the embodiments and details can be made without departing from the spirit and scope of the claims.

[0233] Example

[0234] Next, the present disclosure will be described in more detail with reference to Examples, but the present disclosure is not limited to these Examples.

[0235] The materials used in the examples are as follows.

[0236] (Perfluorinated fluororesin)

[0237] PFA1 (TFE / PAVE (mass %): 97.9 / 2.1, fluorine-containing monomer content: 100 mol%, melting point: 304°C, MFR: 29 g / 10 min, relative dielectric constant (25°C, 10 GHz): 2.1, dielectric loss tangent (25°C, 10 GHz): 0.0003)

[0238] PFA2 (TFE / PAVE (mass %): 97.9 / 2.1, fluorine-containing monomer content: 100 mol%, melting point: 303°C, MFR: 29 g / 10 min, relative dielectric constant (25°C, 10 GHz): 2.0, dielectric loss tangent (25°C, 10 GHz): 0.001)

[0239] FEP (TFE / HFP / PAVE (mass %): 87.5 / 11.5 / 1.0, fluorine-containing monomer content: 100 mol%, melting point: 255°C, MFR: 24 g / 10 min, relative dielectric constant (25°C, 10 GHz): 2.1, dielectric loss tangent (25°C, 10 GHz): 0.0008)

[0240] (filler)

[0241] Talc 1 (average particle size: 7 μm, aspect ratio: 45-50, Mohs hardness (old Mohs hardness): 1, surface treatment: treated with fluorosilane (silane coupling agent containing fluorine group))

[0242] Talc 2 (average particle size: 7 μm, aspect ratio: 30, Mohs hardness (old Mohs hardness): 1, surface treatment: treated with fluorosilane (silane coupling agent containing fluorine group))

[0243] Talc 3 (average particle size: 7 μm, aspect ratio: 30, Mohs hardness (old Mohs hardness): 1, surface treatment: treated with aminosilane (silane coupling agent containing amino group))

[0244] Talc 4 (average particle size: 7 μm, aspect ratio: 30, Mohs hardness (old Mohs hardness): 1, surface treatment: treated with vinyl silane (silane coupling agent containing vinyl group))

[0245] Talc 5 (average particle size: 5 μm, aspect ratio: 30, Mohs hardness (old Mohs hardness): 1, surface treatment: treated with fluorosilane (silane coupling agent containing fluorine group))

[0246] Talc 6 (average particle size: 7 μm, aspect ratio: 45-50, Mohs hardness (old Mohs hardness): 1, surface treatment: none)

[0247] Zinc oxide (average particle size: 0.035 μm, surface treatment: none, ultraviolet light absorption: yes (absorbance of 355 nm light is 0.1 or more))

[0248] The number of unstable terminal groups in the perfluororesin is shown in the table below. The measurement was performed using film-like samples cut out from pellets and sheets made of perfluororesin prepared in the same manner as in the examples described below.

[0249]

[0250] (Examples and Comparative Examples)

[0251] <Pelletization Methods Other Than Example 2>

[0252] A perfluoro-based fluororesin and a filler were melt-kneaded at a ratio (mass %) shown in the following table by a twin-screw extruder at 360°C, and then cooled in a water bath. The resulting solid composition (strand) was cut and pelletized.

[0253] <Preparation method of pelletizing in Example 2>

[0254] A perfluoro-based fluororesin and a filler were melt-kneaded in the ratios (mass %) shown in the table below using a LABOPLASTOMILL MIXER (time: 600 seconds, temperature: 350° C.) and then naturally cooled to obtain a solid composition. The obtained solid composition was crushed and pelletized.

[0255] The pellets obtained above were press-molded at 350° C. to obtain a sheet having a thickness of 100 μm. The flowability of Comparative Example 4 was low and could not be formed into a sheet.

[0256] In Example 10, the sheet obtained in Example 1 is layered with Cu foil (electrolytic copper, thickness: 18 μm, surface roughness Rz: 1.4 μm on the side bonded to the sheet), and pressed for 5 minutes at a heating temperature of 320°C and a pressure of 15 kN to obtain a joint body in which the sheet is bonded to one side of the copper foil.

[0257] (Wire pulling stability)

[0258] The pulling stability of the strands when the pellets were formed was evaluated according to the following criteria.

[0259] ◎: Stable

[0260] 0:Occasionally disconnected

[0261] ×: The wire cannot be pulled

[0262] (Sheet formability)

[0263] The moldability when the above-mentioned sheet was formed was evaluated according to the following criteria.

[0264] ◎: No foaming (bubble)

[0265] ○: Partially no foaming

[0266] (Number of voids (Image analysis of laser microscope observation))

[0267] The following method was used to evaluate the 2The area is the number of voids with a width of 30 μm or more.

[0268] The pellets were cut with a razor and the cross section was observed with a laser microscope. The number of voids was 0.069 mm in an image measured at a magnification of 50 times. 2 The number of gaps per unit area (0.23 mm in length and 0.3 mm in width) was counted and converted into per 1 mm 2 The amount of area.

[0269] (Linear expansion coefficient (CTE) reduction rate)

[0270] The linear expansion rate (linear expansion coefficient) of the sheet was determined by TMA measurement in the following mode using TMA-7100 (manufactured by Hitachi High-Technologies Corporation).

[0271] Then, the same measurement was performed on the perfluorinated fluororesin, and the reduction rate relative to the linear expansion coefficient of the resin alone (linear expansion coefficient before adding filler) was calculated by the following calculation formula and evaluated according to the following criteria.

[0272] [Tensile mode measurement]

[0273] As a sample piece, an extruded film cut into a length of 20 mm, a width of 4 mm and a thickness of 25 μm was used. The linear expansion coefficient was determined from the displacement of the sample at 20° C. to 200° C. at a heating rate of 2° C. / min while being stretched at a load of 49 mN.

[0274] [Calculation formula for reduction rate]

[0275] (reduction rate / %) = (B1-B2) × 100 / B1

[0276] B1: Linear expansion rate before filler addition / ppm / ℃

[0277] B2: Linear expansion rate after filler addition / ppm / ℃

[0278] [Benchmark]

[0279] ◎:More than 50%

[0280] ○: Less than 50% and more than 25%

[0281] ×: Less than 25%

[0282] (Relative dielectric constant (Dk), dielectric loss tangent (Df))

[0283] The sheets were measured for Dk and Df at 25° C. and 10 GHz using a split cylinder type dielectric constant / dissipation factor measuring apparatus (manufactured by EM lab), and evaluated based on the following criteria.

[0284] [Standards for relative dielectric constant]

[0285] ◎: Less than 5

[0286] [Dielectric loss tangent standard]

[0287] ◎: less than 0.0012

[0288] ○: 0.0012 or more and less than 0.003

[0289] (Peel test)

[0290] The peel test (90 degree peel test) was carried out according to JIS C 6481-1996. The resin at the end of the joint body of Example 10 obtained above was peeled off by about 1 cm, clamped on the chuck of the tester, and the peel strength (unit: N / cm) was measured under the condition of a tensile speed (moving speed) of 50 mm / min, and evaluated according to the following criteria.

[0291] ◎: 10N / cm or more

[0292]

Claims

1. A solid composition comprising a perfluororesin and an anisotropic filler surface-treated with a silane coupling agent.

2. The solid composition according to claim 1, wherein The anisotropic filler is talc and / or boron nitride.

3. The solid composition according to claim 1 or 2, wherein The Mohs hardness of the anisotropic filler is 4 or less.

4. The solid composition according to any one of claims 1 to 3, wherein The silane coupling agent has at least one selected from the group consisting of a fluorine-containing group, an amino group, a vinyl group, and an epoxy group.

5. The solid composition according to any one of claims 1 to 4, wherein The unstable terminal groups of the perfluorocarbon resin are relative to each 1×10 6 The number of carbon atoms is less than 50. The unstable terminal group is at least one selected from the group consisting of -CF2H, -COF, -COOH, -COOCH3, -CONH2 and -CH2OH present at the main chain terminal of the perfluoro-based fluororesin.

6. The solid composition according to any one of claims 1 to 5, wherein The perfluoro-based fluororesin is at least one selected from the group consisting of polytetrafluoroethylene, tetrafluoroethylene / perfluoro(alkyl vinyl ether) copolymers, and tetrafluoroethylene / hexafluoropropylene copolymers.

7. The solid composition according to any one of claims 1 to 6, wherein In the image analysis of laser microscope observation, the number of voids with a width of 30 μm or more was found to be 1 mm. 2 There are less than 30 of them in the area.

8. The solid composition according to any one of claims 1 to 7, wherein The reduction rate of the linear expansion coefficient of the solid composition at 20°C to 200°C is 25% or more relative to the linear expansion coefficient of the perfluoro-based fluororesin at 20°C to 200°C.

9. The solid composition according to any one of claims 1 to 8, wherein The dielectric loss tangent at 25°C and 10 GHz is less than 0.

003. 10 . The solid composition according to claim 1 , which is a film or a sheet. 11 . The solid composition according to claim 1 , which is an insulating material for a circuit board.

12. The solid composition according to claim 11, wherein The insulating material of the circuit substrate is a low dielectric material. 13 . A circuit board comprising the solid composition according to claim 1 and a conductive layer.

14. The circuit substrate according to claim 13, wherein: The conductive layer is metal.

15. The circuit substrate according to claim 14, wherein: The surface roughness Rz of the metal surface on the solid composition side is 2.0 μm or less.

16. The circuit substrate according to claim 14 or 15, wherein: The metal is copper.

17. The circuit board according to claim 13 to 16, which is a printed circuit board, a laminated circuit board or a high-frequency board.

18. A method for producing a solid composition, which is the method for producing a solid composition according to any one of claims 1 to 12, wherein: The perfluoro-based fluororesin and the anisotropic filler are melt-kneaded to obtain the solid composition.