GaN EPITAXIAL SUBSTRATE
By introducing Fe concentration gradient or C-layer/Fe diffusion suppression layer into GaN-HEMT, the problem of Fe diffusion to the 2DEG region is solved, device performance and design freedom are improved, and manufacturing cost is reduced.
Patent Information
- Application Number
- CN202380027130.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-14
- Filing Date
- 2023-03-10
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art cannot effectively inhibit Fe from diffusion into the 2DEG region in GaN-HEMT, resulting in a decrease in performance, design freedom and manufacturing cost.
By introducing a concentration gradient of Fe into the GaN substrate or buffer layer, or forming a C-containing layer or Fe diffusion suppression layer in the GaN buffer layer, the diffusion of Fe is hindered and precise control of Fe concentration is achieved.
Effectively inhibit Fe diffusion to the 2DEG region, improves the performance and design freedom of GaN-HEMT, reduces manufacturing costs, and achieves precise control of Fe concentration.
Smart Images

Figure CN119013443A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a GaN epitaxial substrate. Background Art
[0002] In recent years, GaN-based high electron mobility transistors (HEMTs) (hereinafter sometimes referred to as "GaN-HEMTs") have been actively developed as devices for high frequencies ranging from tens of GHz to hundreds of GHz. Silicon, silicon carbide (SiC), GaN, etc. have been studied as substrates for GaN-HEMTs, and GaN-HEMTs using GaN substrates can be expected to have superior performance compared to cases where other substrates are used. Although GaN-HEMTs repeatedly turn current on and off at high frequencies, it is ideal that current does not flow at all in the OFF state. Therefore, when using a GaN substrate in a GaN-HEMT, it is preferred that the GaN substrate be semi-insulated.
[0003] As a method for making a GaN substrate semi-insulating, a method of doping with transition metal elements and Group 12 elements is known. Transition metal elements and Group 12 elements act as acceptors, and therefore have the effect of compensating for background donors that are unintentionally introduced into the GaN substrate and reducing the carrier concentration in the GaN substrate. Such transition metal elements and Group 12 elements are called compensating impurities.
[0004] For example, in the invention described in Non-Patent Document 1, a GaN substrate doped with Fe and Mn as compensation impurities is obtained. In addition, although not an example using a GaN substrate, in the inventions described in Patent Documents 1 to 3, Fe is doped in a GaN buffer layer as a compensation impurity.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application No. 2016-511545
[0008] Patent Document 2: Japanese Patent Application Publication No. 2018-041786
[0009] Patent Document 3: Japanese Patent Application Publication No. 2017-085054
[0010] Non-patent literature
[0011] Non-patent literature 1: M Iwinska et al., Iron and manganese as dopants used in the crystallization of highly resistive HVPE-GaN on native seeds, Japanese Journal of Applied Physics, Vol. 58 SC1047, 2019 Summary of the invention
[0012] Problems to be solved by the invention
[0013] The present inventors initially studied a GaN substrate doped with Fe in order to obtain a GaN substrate that can be suitably used in a GaN-HEMT.
[0014] In this process, when a HEMT structure is formed using a GaN substrate doped with Fe, it is confirmed that Fe can diffuse in the GaN buffer layer. In particular, if Fe diffuses into the region of the HEMT device where a two-dimensional electron gas (hereinafter sometimes referred to as "2DEG") is generated as an electron channel, the performance as a transistor deteriorates as the electron mobility decreases, and there is a risk that high electron mobility operation as a HEMT cannot be achieved.
[0015] Therefore, it is necessary to suppress and prevent Fe from diffusing into the region where 2DEG is generated.
[0016] Therefore, an object of the present invention is to provide a GaN epitaxial substrate which contains Fe as a compensating impurity, in which diffusion of Fe is suppressed, and in which the degree of freedom in device design and manufacturing cost are excellent.
[0017] It should be noted that, although Patent Document 1 focuses on eliminating the problem of large-scale capture caused by the memory effect peculiar to Fe doping, it does not mention the problem of Fe diffusion in the solid at all, and does not recognize the problem caused by Fe diffusion. In addition, in Patent Document 1, the residual Fe after stopping Fe doping and the unintentional doping of the residual Fe itself are still maintained. Therefore, it is impossible to obtain a GaN epitaxial substrate in which Fe diffusion to the region generating 2DEG is suppressed.
[0018] In Patent Document 2, in order to suppress the diffusion of Fe, a GaN buffer layer not doped with Fe is grown on a GaN buffer layer doped with Fe (Fe-doped GaN buffer layer) at a temperature lower than the growth temperature of the Fe-doped GaN buffer layer. That is, Patent Document 2 suppresses the diffusion of Fe by lowering the growth temperature of the GaN buffer layer.
[0019] However, the crystal growth temperature is determined by the growth conditions of the metal organic chemical vapor deposition (Metal Organic Chemical VaporDeposition, MOCVD) method, so it is difficult to change the temperature only. In addition, from the viewpoint of obtaining good crystals, the growth temperature has certain restrictions, so in fact, the reduction of Fe concentration has a limit. In addition, in patent documentation 2, the residual of Fe after stopping doping Fe and the unintentional doping of residual Fe itself are also maintained. As a result, it can not be considered that the diffusion of Fe can be fully suppressed in patent documentation 2.
[0020] In addition, by lowering the growth temperature, the result is that the GaN buffer layer on the Fe-doped GaN buffer layer contains 1×10 19 atoms / cm 3 Although the high concentration of C can be used, there are risks such as leakage current caused by C itself and reduction in crystal quality.
[0021] Patent Document 3 discloses a semiconductor device in which a channel layer doped with Al at a certain concentration is formed on a GaN buffer layer doped with Fe in order to suppress the diffusion of Fe. However, it is not considered that Patent Document 3 can sufficiently suppress the diffusion of Fe.
[0022] In addition to the methods disclosed in the above-mentioned patent documents 1 to 3, based on the fact that the longer the diffusion distance, the lower the Fe concentration, the following method is also considered: after forming a GaN buffer layer doped with Fe, a sufficiently thick undoped GaN buffer layer is provided thereon, thereby reducing the Fe reaching the region where 2DEG is generated and reducing the Fe concentration in the region. However, in this method, the longer the diffusion distance, the thicker the undoped GaN buffer layer is required, so the design freedom of the HEMT device is impaired or the manufacturing cost is increased.
[0023] As described above, a GaN epitaxial substrate which can suppress the diffusion of Fe into the region where 2DEG is generated and which is excellent in the degree of freedom in device design and the manufacturing cost and which can be suitably used for GaN-HEMT has not been obtained so far.
[0024] In addition, as described above, the conventional technology cannot achieve precise control of the Fe concentration in the HEMT device.
[0025] Solutions to the problem
[0026] In view of the above problems, the present inventors have conducted in-depth research and, as a first method, have focused on the fact that the Fe concentration distribution can be more effectively suppressed by intentionally hindering the movement of Fe in the GaN substrate or the GaN buffer layer, compared with the conventional method of simply suppressing the thermal diffusion of Fe. Further research has been conducted and it has been found that the above problems can be solved by making the concentration gradient of Fe from the GaN substrate containing Fe or the GaN buffer layer containing Fe to the
[0001] axis direction very steep, thereby completing the present invention.
[0027] In addition, the present inventors conducted in-depth research on the above-mentioned problems, and found that as a second method, by setting the GaN substrate or the GaN buffer layer to include an Fe-doped layer doped with Fe, and the GaN buffer layer to include a C-containing layer with a specific C concentration or an Fe diffusion suppression layer containing C, the movement of Fe can be effectively hindered, the above-mentioned problems can be solved, and the present invention was completed.
[0028] That is, the gist of the first aspect of the present invention is as follows.
[0029] A first aspect of the present invention relates to a GaN epitaxial substrate comprising a GaN substrate and a GaN buffer layer epitaxially grown on the GaN substrate, wherein the GaN epitaxial substrate comprises a point A and a point B, wherein the point B is located on a straight line passing through the point A and parallel to the
[0001] axis and exists in the
[0001] axis direction relative to the point A, the point A exists in the GaN substrate or in the GaN buffer layer, the point B exists in the GaN buffer layer, and the Fe concentration [Fe] at the point B is B The Fe concentration at point A [Fe] A The ratio ([Fe] B / [Fe] A ) is 1 / 100, and the distance between the above-mentioned point A and the above-mentioned point B is less than 0.2μm.
[0030] A second aspect of the present invention relates to a GaN epitaxial substrate comprising a GaN substrate and a GaN buffer layer epitaxially grown on the GaN substrate, the GaN epitaxial substrate comprising a point A' and a point B', the point B' being located on a straight line passing through the point A' and parallel to the
[0001] axis and existing in the
[0001] axis direction relative to the point A', the point A' existing in the GaN substrate or in the GaN buffer layer, the point B' existing in the GaN buffer layer, and the Fe concentration [Fe] at the point B' being B’ The Fe concentration at point A' [Fe] A’ The ratio ([Fe] B’ / [Fe] A’) is 1 / 10, and the distance between the above-mentioned point A' and the above-mentioned point B' is less than 0.1 μm.
[0031] A third aspect of the present invention relates to a GaN epitaxial substrate, comprising a GaN substrate and a GaN buffer layer epitaxially grown on the GaN substrate, wherein the GaN epitaxial substrate comprises a point A" and a point B", the point B" being located on a straight line passing through the point A" and parallel to the
[0001] axis and existing in the
[0001] axis direction relative to the point A", the point A" existing in the GaN substrate or in the GaN buffer layer, the point B" existing in the GaN buffer layer, and the Fe concentration at the point A" being 1×10 17 atoms / cm 3 The Fe concentration at point B" is 1×10 15 atoms / cm 3 Hereinafter, the distance between the point A" and the point B" is less than 0.2 μm.
[0032] A fourth aspect of the present invention relates to a GaN epitaxial substrate, comprising a GaN substrate and a GaN buffer layer epitaxially grown on the GaN substrate, wherein the GaN epitaxial substrate comprises a point A'' and a point B'', wherein the point B'' is located on a straight line passing through the point A'' and parallel to the
[0001] axis and exists in the
[0001] axis direction relative to the point A'', the point A'' exists in the GaN substrate or in the GaN buffer layer, the point B'' exists in the GaN buffer layer, and the Fe concentration at the point A'' is 1×10 17 atoms / cm 3 The Fe concentration at point B'' is 1×10 16 atoms / cm 3 Hereinafter, the distance between the point A''' and the point B'''' is 0.1 μm or less.
[0033] A fifth aspect of the present invention relates to the GaN epitaxial substrate of the first aspect or the second aspect, wherein the above-mentioned [Fe] A or the above [Fe] A’ 1×10 17 atoms / cm 3 above.
[0034] A sixth aspect of the present invention is directed to the GaN epitaxial substrate of any one of aspects 1 to 5, wherein the point A, the point A′, the point A″ or the point A′″ exists in the GaN substrate.
[0035] A seventh aspect of the present invention relates to a GaN epitaxial substrate according to any one of the first to sixth aspects, wherein the GaN buffer layer contains a C concentration of 1×1016 ~1×10 18 atoms / cm 3 The C-containing region includes the point B, the point B', the point B", or the point B'", or is located on the (000-1) plane side relative to the plane parallel to the (0001) plane and including the point B, the point B', the point B", or the point B''.
[0036] Aspect 8 of the present invention relates to the GaN epitaxial substrate of any one of aspects 1 to 7, wherein at least one of the GaN substrate and the GaN buffer layer includes an Fe-doped layer doped with Fe.
[0037] Aspect 9 of the present invention relates to a GaN epitaxial substrate of any one of aspects 1 to 8, wherein the GaN substrate includes an Fe-doped layer doped with Fe, and the point A, the point A', the point A", or the point A'" exists in the Fe-doped layer.
[0038] A tenth aspect of the present invention is the GaN epitaxial substrate of any one of aspects 7 to 9, wherein the GaN buffer layer includes an i-GaN layer in the
[0001] axis direction relative to the C-containing region.
[0039] Aspect 11 of the present invention relates to the GaN epitaxial substrate of any one of aspects 1 to 10, further comprising a nitride semiconductor barrier layer on the GaN buffer layer.
[0040] In addition, the gist of the second aspect of the present invention is as follows.
[0041] A twelfth aspect of the present invention relates to a GaN epitaxial substrate comprising a GaN substrate and a GaN buffer layer epitaxially grown on the GaN substrate, wherein at least one of the GaN substrate and the GaN buffer layer comprises an Fe-doped layer doped with Fe, and the GaN buffer layer comprises a C-containing layer, wherein the C-containing layer is present in the
[0001] axis direction relative to the Fe-doped layer and has a C concentration of 1×10 16 ~1×10 18 atoms / cm 3 .
[0042] Mode 13 of the present invention relates to a GaN epitaxial substrate, which includes a GaN substrate and a GaN buffer layer formed by epitaxial growth on the above-mentioned GaN substrate, wherein the above-mentioned GaN substrate or the above-mentioned GaN buffer layer includes an Fe-doped layer doped with Fe, and the above-mentioned GaN buffer layer includes an Fe diffusion suppression layer that exists in the
[0001] axis direction relative to the above-mentioned Fe-doped layer and contains C to suppress the diffusion of Fe.
[0043] Aspect 14 of the present invention relates to the GaN epitaxial substrate of aspect 13, wherein the C concentration of the Fe diffusion suppression layer is 1×10 18 atoms / cm 3 the following.
[0044] A fifteenth aspect of the present invention relates to the GaN epitaxial substrate of any one of the twelfth to the fourteenth aspect, wherein the GaN substrate includes the Fe-doped layer.
[0045] Aspect 16 of the present invention relates to the GaN epitaxial substrate of any one of aspects 12 to 15, wherein the Fe concentration of the Fe-doped layer is 1×10 17 atoms / cm 3 above.
[0046] A seventeenth aspect of the present invention is directed to the GaN epitaxial substrate of any one of aspects 12 to 16, wherein the C-containing layer or the Fe-diffusion suppression layer is a C-doped layer.
[0047] Aspect 18 of the present invention relates to a GaN epitaxial substrate according to any one of aspects 12 to 17, wherein the Fe concentration in the C-containing layer or the Fe diffusion suppression layer in the GaN buffer layer, or in a GaN region located in the
[0001] axis direction relative to the C-containing layer or the Fe diffusion suppression layer is less than 1×10 17 atoms / cm 3 .
[0048] A 19th aspect of the present invention relates to a GaN epitaxial substrate according to any one of aspects 12 to 18, wherein the GaN substrate or the GaN buffer layer includes a point A, the GaN buffer layer includes a point B, the point B is located on a straight line passing through the point A and parallel to the
[0001] axis, and exists in the
[0001] axis direction relative to the point A, and the Fe concentration [Fe] at the point B is B The Fe concentration at point A [Fe] A The ratio ([Fe] B / [Fe] A ) is 1 / 100, and the distance between the above-mentioned point A and the above-mentioned point B is less than 0.2μm.
[0049] Aspect 20 of the present invention relates to the GaN epitaxial substrate of any one of aspects 12 and 15 to 19, wherein the GaN buffer layer includes an i-GaN layer in the
[0001] axis direction relative to the C-containing region.
[0050] Aspect 21 of the present invention relates to the GaN epitaxial substrate of any one of aspects 12 to 20, further comprising a nitride semiconductor barrier layer on the GaN buffer layer.
[0051] Effects of the Invention
[0052] The GaN epitaxial substrate of this embodiment can suppress the diffusion of Fe into the region other than the GaN substrate or GaN buffer layer that has been intentionally made highly resistive, and the device design freedom and manufacturing cost are also good. Therefore, it is very suitable as a substrate for a nitride semiconductor device with a horizontal device structure such as GaN-HEMT. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] Figure 1 : is the Fe concentration curve at the interface between the Fe-doped layer and the C-containing region in the GaN epitaxial substrate. The solid line is based on the measured result obtained by SIMS measurement of Example 1, and the dotted line is based on the calculated result obtained using the diffusion equation which is equivalent to the result of Comparative Example 2 without the C-containing region.
[0054] Figure 2 It is the Fe concentration curve at the interface between the Fe-doped layer and the undoped GaN buffer layer in the GaN epitaxial substrate of Comparative Example 1. The solid line is based on the measured result obtained by SIMS measurement of Comparative Example 1, and the dotted line is the fitting result obtained by using the diffusion equation for the above measured result.
[0055] Figure 3 It is expressed in logarithm Figure 1 The vertical axis is the Fe concentration curve, and Figure 1 Likewise, the solid line is based on the actual measurement result obtained by SIMS measurement of Example 1, and the dotted line is based on the calculation result obtained by using the diffusion equation which is equivalent to the result of Comparative Example 2 having no C-containing region. DETAILED DESCRIPTION
[0056] Hereinafter, the present invention will be described in detail, but the present invention is not limited to the following embodiments and can be implemented with various modifications within the scope of the gist of the invention.
[0057] In this specification, the crystal axis parallel to the
[0001] axis is called the c-axis, the crystal axis parallel to the <10-10> axis is called the m-axis, and the crystal axis parallel to the <11-20> axis is called the a-axis. The crystal plane orthogonal to the c-axis is called the c-plane, the crystal plane orthogonal to the m-axis is called the m-plane, and the crystal plane orthogonal to the a-axis is called the a-plane.
[0058] The Miller index (hkil) of the hexagonal crystal has the relationship of h+k=-i, and therefore, it is sometimes expressed as (hkl) using three digits. For example, if (0004) is expressed as (004) using three digits.
[0059] In this specification, when referring to crystal axes, crystal planes, crystal orientations, etc., unless otherwise specified, they refer to the crystal axes, crystal planes, crystal orientations, etc. in the GaN epitaxial substrate, that is, the GaN substrate, and the GaN buffer layer, respectively.
[0060] In this specification, the Fe concentration and the C concentration at a specific position are values determined from respective detection amounts using secondary ion mass spectrometry (SIMS).
[0061] In the present specification, when the expression "to" is used, it is used as an expression including the numerical values or physical property values before and after it. That is, "A to B" means A or more and B or less.
[0062] In the HEMT structure, a crystal layer composed of GaN epitaxially grown on a substrate is generally referred to as a GaN buffer layer. Accordingly, in this specification, a crystal layer composed of GaN epitaxially grown on a GaN substrate is referred to as a "GaN buffer layer".
[0063] The First Way
[0064] [GaN epitaxial substrate]
[0065] The GaN epitaxial substrate of the first embodiment in the first mode includes a GaN substrate and a GaN buffer layer epitaxially grown on the GaN substrate. The GaN epitaxial substrate includes a point A and a point B, wherein the point B is located on a straight line passing through the point A and parallel to the
[0001] axis and exists in the
[0001] axis direction relative to the point A, and the point A exists in the GaN substrate or the GaN buffer layer, and the point B exists in the GaN buffer layer. The Fe concentration at the point B [Fe] B and the Fe concentration at point A [Fe] A The ratio ([Fe] B / [Fe] A ) is 1 / 100, and the distance between point A and point B is less than 0.2μm.
[0066] Point B exists in the
[0001] axis direction relative to point A, which means that point B exists in the +c axis direction, that is, the Ga polarity plane direction of the crystal, compared to point A. The same is true for the relationship between point A' and point B' in the second embodiment of the first mode described later, point A" and point B" in the third embodiment of the first mode, and point A"' and point B"' in the fourth embodiment of the first mode.
[0067] The GaN epitaxial substrate includes point A and point B, which means that there is at least one group of point A and point B satisfying the above relationship in the GaN epitaxial substrate. That is, the GaN epitaxial substrate of the first embodiment of the first mode only needs to have at least one group of point A and point B satisfying the above relationship. Preferably, the GaN epitaxial substrate has three or more groups of point A and point B satisfying the above relationship on the same plane parallel to the (0001) plane, and each group is located at a position more than 1 mm away from each other. In addition, the same is true for the relationship between point A' and point B' in the second embodiment of the first mode described later, point A" and point B" in the third embodiment of the first mode, and point A"' and point B"' in the fourth embodiment of the first mode.
[0068] [Fe] B / [Fe] A The distance between point A and point B being 1 / 100 of 0.2 μm or less means that the Fe concentration gradient between point A and point B is steep, which can appropriately inhibit the diffusion of Fe. This ensures the semi-insulating property brought about by Fe and inhibits the diffusion of Fe to the region where 2DEG is generated in the GaN-HEMT structure.
[0069] From the perspective of ensuring sufficient semi-insulation, the Fe concentration at point A [Fe] A Preferably 1×10 17 atoms / cm 3 ~1×10 20 atoms / cm 3 , more preferably 5×10 17 ~1×10 19 atoms / cm 3 , more preferably 1×10 18 ~5×10 18 atoms / cm 3 Here, 1×10 17 atoms / cm 3 More preferably 5×10 17 atoms / cm 3 More preferably, 1×10 18 atoms / cm 3 In addition, from the perspective of maintaining good crystal quality, [Fe] A Preferably 1×10 20 atoms / cm 3 Less than, more preferably 1×10 19 atoms / cm 3 Below, more preferably 5×10 18atoms / cm 3 the following.
[0070] Since the Fe concentration at point B [Fe] B is the Fe concentration at point A [Fe] A 1 / 100 of the point, therefore, [Fe] B The preferred range of [Fe] A Change accordingly.
[0071] The distance between point A and point B is preferably 0.2 μm or less, and is preferably 0.15 μm or less, more preferably 0.13 μm or less, and further preferably 0.12 μm or less from the viewpoint of making the concentration gradient of Fe steeper. In addition, although the shorter the distance between point A and point B, the more preferred, it is usually 0.01 μm or more from the viewpoint of feasibility.
[0072] Point A only needs to be present in the GaN substrate or in the GaN buffer layer, and preferably exists in the GaN substrate from the viewpoint of ease of production.
[0073] On the other hand, point B exists in the GaN buffer layer.
[0074] It should be noted that the above-mentioned ease of manufacturing is explained. When point A exists in the GaN buffer layer, both point A and point B are included in the GaN buffer layer formed by epitaxial growth by MOCVD method or the like. When Fe doping is used as a method to achieve the Fe concentration at point A, the Fe dopant gas used remains in the reaction tube, and sometimes Fe that was originally unintentionally doped is introduced when forming the area where point B exists. If such an unexpected introduction of Fe occurs, it is difficult to obtain an Fe concentration within a range of 0.2μm or less from point A to become the Fe concentration at point A [Fe] A In order to control the concentration gradient of Fe, a further process is required. In contrast, if point A exists in the GaN substrate, the above-mentioned unexpected introduction of Fe can be prevented, so point B can be easily obtained within a range of 0.2 μm or less from point A, and as a result, the GaN epitaxial substrate of this embodiment in the first mode can be easily manufactured.
[0075] However, the Fe concentration in the GaN substrate is high, and Fe also thermally diffuses into the GaN buffer layer, resulting in the existence of point A and point B in the GaN buffer layer sometimes even without Fe doping. In this case, the introduction of Fe that was originally unintentionally doped when forming the region where point B exists can be ignored.
[0076] It is preferred that at least one of the GaN substrate and the GaN buffer layer includes an Fe-doped layer doped with Fe. From the viewpoint of ease of manufacturing, it is more preferred that the GaN substrate includes the Fe-doped layer. In addition, it is more preferred that point A exists in the Fe-doped layer in the GaN substrate. However, the presence of point A in the GaN buffer layer due to thermal diffusion of Fe from the Fe-doped layer in the GaN substrate is not excluded.
[0077] It should be noted that, in this specification, the Fe-doped layer doped with Fe refers to a layer having an Fe concentration of 1×10 17 atoms / cm 3 The above region can be distinguished from the case where Fe is unintentionally introduced during the process of manufacturing the GaN epitaxial substrate.
[0078] In the case where the GaN substrate includes an Fe-doped layer, the upper end face of the Fe-doped layer is preferably located at a position consistent with the (0001) surface of the GaN substrate. The thickness of the Fe-doped layer in the c-axis direction does not need to be consistent with the thickness of the GaN substrate in the c-axis direction. For example, relative to the overall thickness of the GaN substrate of 400 μm, the thickness of the Fe-doped layer is sufficient as long as it is 100 μm of the surface layer of the GaN substrate. Of course, the thickness of the Fe-doped layer is not limited to the above thickness, and the case of being thicker or thinner than the above thickness is not excluded. In addition, the GaN substrate may be composed of an Fe-doped layer as a whole in the thickness direction of the GaN substrate.
[0079] When the GaN substrate includes an Fe-doped layer, the thickness of the Fe-doped layer may be 50 μm to 500 μm. When the GaN substrate includes an Fe-doped layer, the thickness of the Fe-doped layer may be 50 μm or more, 80 μm or more, or 100 μm or more. On the other hand, it may be 500 μm or less.
[0080] When the GaN substrate includes an Fe-doped layer, the C concentration in the Fe-doped layer is preferably 5×10 16 atoms / cm 3 In the case where the GaN substrate includes an Fe-doped layer, the C concentration in the Fe-doped layer may be 4×10 16 atoms / cm 3 Below, or 3×10 16 atoms / cm 3 Below, or 2×10 16 atoms / cm 3 the following.
[0081] The GaN buffer layer preferably contains a C concentration of 1×10 16 ~1×10 18 atoms / cm 3The presence of the C-containing region can hinder the movement of Fe between different regions defined by the C-containing region.
[0082] The movement of Fe in the GaN epitaxial substrate usually occurs due to thermal diffusion defined by the diffusion equation. Therefore, the concentration distribution of Fe in the GaN epitaxial substrate should be described by the diffusion equation. However, it was found that in the presence of a C-containing region, the concentration distribution of Fe around the C-containing region deviates from the behavior predicted by the diffusion equation and exhibits a steep Fe concentration gradient. Therefore, it can be considered that the presence of a C-containing region can effectively hinder the movement of Fe in the GaN epitaxial substrate.
[0083] The C concentration of the C-containing region is preferably 1×10 16 atoms / cm 3 Above and 1×10 18 atoms / cm 3 Less than, more preferably 5×10 16 atoms / cm 3 Above and 1×10 18 atoms / cm 3 Below, more preferably 1×10 17 atoms / cm 3 Above and 8×10 17 atoms / cm 3 Below, particularly preferably 1×10 17 atoms / cm 3 Above and 5×10 17 atoms / cm 3 Here, the C concentration of the C-containing region is preferably 1×10 16 atoms / cm 3 From the viewpoint of further inhibiting the movement of Fe, 5×10 16 atoms / cm 3 More preferably, 1×10 17 atoms / cm 3 In addition, from the viewpoint of preventing the occurrence of defects such as threading dislocations and preventing leakage current caused by C, the C concentration in the C-containing region is preferably 1×10 18 atoms / cm 3 Less than 1×10 18 atoms / cm 3 , more preferably 8×10 17 atoms / cm 3 Below, particularly preferably 5×10 17 atoms / cm 3the following.
[0084] It is preferred that the C-containing region includes point B, or is located on the (000-1) plane side relative to the plane parallel to the (0001) plane and including point B. In other words, it is preferred that point B exists in the C-containing region, or that the C-containing region exists between the plane parallel to the (0001) plane and including point A, and the plane parallel to the (0001) plane and including point B.
[0085] The thickness of the C-containing region in the c-axis direction is preferably 50 to 900 nm, more preferably 100 to 600 nm, and further preferably 200 to 500 nm. Here, from the perspective of normal device production, the thickness of the C-containing region is preferably 50 nm or more, more preferably 100 nm or more, and further preferably 200 nm or more. In addition, from the perspective of reducing leakage current, the thickness of the C-containing region is preferably 900 nm or less, more preferably 600 nm or less, and further preferably 500 nm or less.
[0086] The thickness of the C-containing region in the c-axis direction is preferably 5 to 90% of the total film thickness of the GaN buffer layer, more preferably 10 to 80%, and further preferably 20 to 70%. Here, from the perspective of normal device production, the above thickness is preferably more than 5% of the total film thickness of the GaN buffer layer, more preferably more than 10%, and further preferably more than 20%. In addition, from the same point of view, the above thickness is preferably less than 90% of the total film thickness of the GaN buffer layer, more preferably less than 80%, and further preferably less than 70%. It should be noted that when the GaN buffer layer includes an Fe-doped layer, a C-containing region, an i-GaN layer, etc. as described later, the total film thickness of the GaN buffer layer refers to the total thickness in the c-axis direction including them.
[0087] The GaN epitaxial substrate of the second embodiment of the first embodiment includes a GaN substrate and a GaN buffer layer epitaxially grown on the GaN substrate. The GaN epitaxial substrate includes a point A' and a point B', wherein the point B' is located on a straight line passing through the point A' and parallel to the
[0001] axis and exists in the
[0001] axis direction relative to the point A', and the point A' exists in the GaN substrate or the GaN buffer layer, and the point B' exists in the GaN buffer layer. Fe concentration [Fe] at point B' B’ and the Fe concentration at point A' [Fe] A’ The ratio ([Fe] B’ / [Fe] A’ ) is 1 / 10, and the distance between point A' and point B' is less than 0.1 μm.
[0088] [Fe] B’ / [Fe] A’The fact that the distance between point A' and point B' is 0.1 μm or less means that the Fe concentration gradient between points A' and B' is steep, which can appropriately inhibit the diffusion of Fe. This ensures the semi-insulation brought about by Fe and inhibits the diffusion of Fe to the region where 2DEG is generated in the GaN-HEMT structure.
[0089] Fe concentration at point A' [Fe] A’ Preferably 1×10 17 ~1×10 20 atoms / cm 3 , more preferably 5×10 17 ~1×10 19 atoms / cm 3 , more preferably 1×10 18 ~5×10 18 atoms / cm 3 Here, from the perspective of ensuring sufficient semi-insulation, the above-mentioned [Fe] A’ Preferably 1×10 17 atoms / cm 3 More preferably 5×10 17 atoms / cm 3 More preferably, 1×10 18 atoms / cm 3 In addition, from the perspective of maintaining good crystal quality, the above [Fe] A’ Preferably 1×10 20 atoms / cm 3 Less than, more preferably 1×10 19 atoms / cm 3 Below, more preferably 5×10 18 atoms / cm 3 the following.
[0090] Since the Fe concentration at point B' [Fe] B’ is the Fe concentration at point A' [Fe] A’ 1 / 10 of the point, therefore, [Fe] B’ The preferred range of [Fe] A’ Change accordingly.
[0091] The distance between point A' and point B' may be 0.1 μm or less, preferably 0.08 μm or less, more preferably 0.05 μm or less from the viewpoint of making the Fe concentration gradient steeper. In addition, although the shorter the distance between point A' and point B', the better, it is usually 0.01 μm or more from the viewpoint of feasibility.
[0092] Point A' only needs to be present in the GaN substrate or the GaN buffer layer, and preferably exists in the GaN substrate from the viewpoint of ease of production. The ease of production described above is the same as point A in the first embodiment of the first aspect.
[0093] On the other hand, point B' exists in the GaN buffer layer.
[0094] It is preferred that at least one of the GaN substrate and the GaN buffer layer includes an Fe-doped layer doped with Fe. From the viewpoint of ease of manufacturing, it is more preferred that the GaN substrate includes the Fe-doped layer. In addition, it is more preferred that point A' exists in the Fe-doped layer in the GaN substrate. However, it is not excluded that point A' exists in the GaN buffer layer due to thermal diffusion of Fe from the Fe-doped layer in the GaN substrate.
[0095] In the case where the GaN substrate includes an Fe-doped layer, the upper end face of the Fe-doped layer is preferably present at a position consistent with the (0001) surface of the GaN substrate. The thickness of the Fe-doped layer in the c-axis direction does not need to be consistent with the thickness of the GaN substrate in the c-axis direction. For example, relative to the overall thickness of the GaN substrate of 400 μm, the thickness of the Fe-doped layer is sufficient as long as it is 100 μm of the surface layer of the GaN substrate. Of course, the thickness of the Fe-doped layer is not limited to the above thickness, and the case of being thicker or thinner than the above thickness is not excluded. In addition, the GaN substrate may be a substrate composed of an Fe-doped layer as a whole in the thickness direction.
[0096] When the GaN substrate includes an Fe-doped layer, the thickness of the Fe-doped layer may be 50 μm to 500 μm. When the GaN substrate includes an Fe-doped layer, the thickness of the Fe-doped layer may be 50 μm or more, 80 μm or more, or 100 μm or more. On the other hand, it may be 500 μm or less.
[0097] When the GaN substrate includes an Fe-doped layer, the C concentration in the Fe-doped layer is preferably 5×10 16 atoms / cm 3 In the case where the GaN substrate includes an Fe-doped layer, the C concentration in the Fe-doped layer may be 4×10 16 atoms / cm 3 Below, or 3×10 16 atoms / cm 3 Below, or 2×10 16 atoms / cm 3 Below, or less than 1×10 16 atoms / cm 3 .
[0098] The GaN buffer layer preferably contains a C concentration of 1×1016 ~1×10 18 atoms / cm 3 The presence of the C-containing region can hinder the movement of Fe between different regions defined by the C-containing region.
[0099] It is preferred that the C-containing region includes point B', or is located on the (000-1) plane side relative to the plane parallel to the (0001) plane and including point B'. In other words, it is preferred that point B' exists in the C-containing region, or that the C-containing region exists between the plane parallel to the (0001) plane and including point A', and the plane parallel to the (0001) plane and including point B'.
[0100] In addition, the preferred C concentration and thickness of the C-containing region are respectively the same as the preferred C concentration and thickness of the C-containing region of the first embodiment in the first aspect.
[0101] The GaN epitaxial substrate of the third embodiment in the first mode includes a GaN substrate and a GaN buffer layer epitaxially grown on the GaN substrate. The GaN epitaxial substrate includes a point A" and a point B", the point B" is located on a straight line passing through the point A" and parallel to the
[0001] axis, and exists in the
[0001] axis direction relative to the point A", respectively, the point A" exists in the GaN substrate or the GaN buffer layer, and the point B" exists in the GaN buffer layer. The Fe concentration at the point A" is 1×10 17 atoms / cm 3 Above, the Fe concentration at point B" is 1×10 15 atoms / cm 3 Hereinafter, the distance between point A" and point B" is less than 0.2 μm.
[0102] The Fe concentration at point A" is preferably 1×10 17 ~1×10 20 atoms / cm 3 , more preferably 5×10 17 ~1×10 19 atoms / cm 3 , more preferably 1×10 18 ~5×10 18 atoms / cm 3 Here, from the perspective of ensuring sufficient semi-insulation, the Fe concentration at point A" is 1×10 17 atoms / cm 3 Above, preferably 5×10 17 atoms / cm 3 More preferably 1×10 18 atoms / cm 3In addition, from the perspective of maintaining good crystal quality, the Fe concentration at point A" is preferably 1×10 20 atoms / cm 3 Less than, more preferably 1×10 19 atoms / cm 3 Below, more preferably 5×10 18 atoms / cm 3 the following.
[0103] If the Fe concentration at point B" is 1×10 15 atoms / cm 3 In the following, the Fe concentration gradient is steep in relation to point A", and it is considered that the diffusion of Fe can be appropriately inhibited. That is, the diffusion of Fe to the region where 2DEG is generated can be suppressed in the GaN-HEMT structure. The Fe concentration at point B" is preferably less than 1×10 15 atoms / cm 3 , more preferably less than 8×10 14 atoms / cm 3 , and more preferably less than 5×10 14 atoms / cm 3 In addition, the lower limit of the Fe concentration at point B" is not particularly limited, and the detection limit of Fe is usually consistent with the lower limit.
[0104] Fe concentration at point B" [Fe] B” and the Fe concentration at point A” [Fe] A” The ratio ([Fe] B” / [Fe] A” ) is 1 / 100 or less, from the viewpoint that the concentration gradient of Fe is steep and the diffusion of Fe can be more appropriately suppressed, [Fe] B” / [Fe] A” Preferably, it is 1 / 500 or less, and more preferably, it is 1 / 1000 or less. B” / [Fe] A” There is no particular lower limit, but the actual achievable value is about 1 / 3000.
[0105] The distance between point A" and point B" may be 0.2 μm or less, and from the viewpoint of making the concentration gradient of Fe steeper, it is preferably 0.15 μm or less, more preferably 0.13 μm or less, and further preferably 0.12 μm or less. In addition, although the shorter the distance between point A" and point B", the better, it is usually 0.01 μm or more from the viewpoint of feasibility.
[0106] Point A" only needs to exist in the GaN substrate or the GaN buffer layer. From the perspective of ease of manufacturing, it is preferably present in the GaN substrate. Regarding the ease of manufacturing mentioned above, it is the same as point A of the first embodiment in the first mode.
[0107] On the other hand, point B" exists in the GaN buffer layer.
[0108] It is preferred that at least one of the GaN substrate and the GaN buffer layer includes an Fe-doped layer doped with Fe. From the viewpoint of ease of manufacturing, it is more preferred that the GaN substrate includes an Fe-doped layer. In addition, it is more preferred that point A" exists in the Fe-doped layer. However, it is not ruled out that point A" exists in the GaN buffer layer due to thermal diffusion of Fe from the Fe-doped layer in the GaN substrate.
[0109] In the case where the GaN substrate includes an Fe-doped layer, the upper end face of the Fe-doped layer is preferably present at a position consistent with the (0001) surface of the GaN substrate. The thickness of the Fe-doped layer in the c-axis direction does not need to be consistent with the thickness of the GaN substrate in the c-axis direction. For example, relative to the overall thickness of the GaN substrate of 400 μm, the thickness of the Fe-doped layer is sufficient as long as it is 100 μm of the surface layer of the GaN substrate. Of course, the thickness of the Fe-doped layer is not limited to the above thickness, and the case of being thicker or thinner than the above thickness is not excluded. In addition, the GaN substrate may be a substrate composed of an Fe-doped layer as a whole in the thickness direction.
[0110] When the GaN substrate includes an Fe-doped layer, the thickness of the Fe-doped layer may be 50 μm to 500 μm. When the GaN substrate includes an Fe-doped layer, the thickness of the Fe-doped layer may be 50 μm or more, 80 μm or more, or 100 μm or more. On the other hand, it may be 500 μm or less.
[0111] When the GaN substrate includes an Fe-doped layer, the C concentration in the Fe-doped layer is preferably 5×10 16 atoms / cm 3 In the case where the GaN substrate includes an Fe-doped layer, the C concentration in the Fe-doped layer may be 4×10 16 atoms / cm 3 Below, or 3×10 16 atoms / cm 3 Below, or 2×10 16 atoms / cm 3 Below, or less than 1×10 16 atoms / cm 3 .
[0112] The GaN buffer layer preferably contains a C concentration of 1×10 16~1×10 18 atoms / cm 3 The presence of the C-containing region can hinder the movement of Fe between different regions defined by the C-containing region.
[0113] It is preferred that the C-containing region includes point B'', or is located on the (000-1) plane side relative to the plane parallel to the (0001) plane and including point B''. That is, it is preferred that point B'' exists in the C-containing region, or that the C-containing region exists between the plane parallel to the (0001) plane and including point A'', and the plane parallel to the (0001) plane and including point B''.
[0114] The preferred C concentration and thickness of the C-containing region are respectively the same as the preferred C concentration and thickness of the C-containing region of the first embodiment in the first aspect.
[0115] The GaN epitaxial substrate of the fourth embodiment in the first mode includes a GaN substrate and a GaN buffer layer epitaxially grown on the GaN substrate. The GaN epitaxial substrate includes a point A'' and a point B''', the point B''' is located on a straight line passing through the point A'' and parallel to the
[0001] axis, and exists in the
[0001] axis direction relative to the point A''', respectively, the point A''' exists in the GaN substrate or the GaN buffer layer, and the point B''' exists in the GaN buffer layer. The Fe concentration at the point A''' is 1×10 17 atoms / cm 3 Above, the Fe concentration at point B'' is 1×10 16 atoms / cm 3 Hereinafter, the distance between point A''' and point B'''' is less than 0.1 μm.
[0116] The Fe concentration at point A'' is preferably 1×10 17 ~1×10 20 atoms / cm 3 , more preferably 5×10 17 ~1×10 19 atoms / cm 3 , more preferably 1×10 18 ~5×10 18 atoms / cm 3 Here, from the perspective of ensuring sufficient semi-insulation, the Fe concentration at point A'' is 1×10 17 atoms / cm 3 Above, preferably 5×10 17 atoms / cm 3 More preferably 1×10 18 atoms / cm 3In addition, from the perspective of maintaining good crystal quality, the Fe concentration at point A'' is preferably 1×10 20 atoms / cm 3 Less than, more preferably 1×10 19 atoms / cm 3 Below, more preferably 5×10 18 atoms / cm 3 the following.
[0117] If the Fe concentration at point B'' is 1×10 16 atoms / cm 3 In the following, the Fe concentration gradient is steep in relation to point A'', and it is considered that the diffusion of Fe can be appropriately inhibited. That is, the diffusion of Fe to the region where 2DEG is generated can be suppressed in the GaN-HEMT structure. The Fe concentration at point B'' is preferably 5×10 15 atoms / cm 3 Less than, more preferably 1×10 15 atoms / cm 3 In addition, the lower limit of the Fe concentration at point B'' is not particularly limited, and the detection limit of Fe is usually consistent with the lower limit.
[0118] Fe concentration at point B''[Fe] B ”' and the Fe concentration at point A”' [Fe] A ”' ratio ([Fe] B ”' / [Fe] A ”') is 1 / 10 or less. From the viewpoint that the concentration gradient of Fe is steep and the diffusion of Fe can be more appropriately suppressed, [Fe] B”’ / [Fe] A”’ Preferably, it is 1 / 100 or less, and more preferably, it is 1 / 500 or less. B”’ / [Fe] A”’ There is no particular lower limit, but the actual achievable value is about 1 / 3000.
[0119] The distance between point A'' and point B''' may be 0.1 μm or less, and from the viewpoint of making the concentration gradient of Fe steeper, it is preferably 0.08 μm or less, and more preferably 0.05 μm or less. In addition, although the shorter the distance between point A''' and point B''', the more preferred, from the viewpoint of feasibility, it is usually 0.01 μm or more.
[0120] Point A''' only needs to be in the GaN substrate or in the GaN buffer layer, and preferably exists in the GaN substrate from the perspective of ease of manufacturing. The ease of manufacturing described above is the same as point A in the first embodiment of the first mode.
[0121] On the other hand, point B'" exists in the GaN buffer layer.
[0122] It is preferred that at least one of the GaN substrate and the GaN buffer layer includes an Fe-doped layer doped with Fe. From the viewpoint of ease of manufacturing, it is more preferred that the GaN substrate includes an Fe-doped layer. In addition, it is more preferred that point A'' exists in the Fe-doped layer in the GaN substrate. However, the presence of point A''' in the GaN buffer layer due to thermal diffusion of Fe from the Fe-doped layer in the GaN substrate is not excluded.
[0123] In the case where the GaN substrate includes an Fe-doped layer, the upper end face of the Fe-doped layer is preferably present at a position consistent with the (0001) surface of the GaN substrate. The thickness of the Fe-doped layer in the c-axis direction does not need to be consistent with the thickness of the GaN substrate in the c-axis direction. For example, relative to the overall thickness of the GaN substrate of 400 μm, the thickness of the Fe-doped layer is sufficient as long as it is 100 μm of the surface layer of the GaN substrate. Of course, the thickness of the Fe-doped layer is not limited to the above thickness, and the case of being thicker or thinner than the above thickness is not excluded. In addition, the GaN substrate may be composed of an Fe-doped layer as a whole in the thickness direction of the GaN substrate.
[0124] When the GaN substrate includes an Fe-doped layer, the thickness of the Fe-doped layer may be 50 μm to 500 μm. When the GaN substrate includes an Fe-doped layer, the thickness of the Fe-doped layer may be 50 μm or more, 80 μm or more, or 100 μm or more. On the other hand, it may be 500 μm or less.
[0125] When the GaN substrate includes an Fe-doped layer, the C concentration in the Fe-doped layer is preferably 5×10 16 atoms / cm 3 In the case where the GaN substrate includes an Fe-doped layer, the C concentration in the Fe-doped layer may be 4×10 16 atoms / cm 3 Below, or 3×10 16 atoms / cm 3 Below, or 2×10 16 atoms / cm 3 Below, or less than 1×10 16 atoms / cm 3 .
[0126] The GaN buffer layer preferably contains a C concentration of 1×10 16 ~1×10 18 atoms / cm 3 The presence of the C-containing region can hinder the movement of Fe between different regions defined by the C-containing region.
[0127] It is preferred that the C-containing region includes point B'", or is located on the (000-1) plane side relative to the plane parallel to the (0001) plane and including point B'". That is, it is preferred that point B'' exists in the C-containing region, or that the C-containing region exists between the plane parallel to the (0001) plane and including point A'', and the plane parallel to the (0001) plane and including point B''.
[0128] The preferred C concentration and thickness of the C-containing region are respectively the same as the preferred C concentration and thickness of the C-containing region of the first embodiment in the first aspect.
[0129] In any of the first to fourth embodiments described above in the first aspect (hereinafter sometimes referred to as “this embodiment”), the GaN epitaxial substrate also includes a GaN buffer layer epitaxially grown on the GaN substrate.
[0130] In the present embodiment of the first mode, a GaN substrate is used instead of a SiC substrate or the like which has been widely used in the past. As a result, defects are less likely to be generated at the interface with the GaN buffer layer to be formed later, and a high-concentration carrier compensation layer for suppressing leakage current is not required, so that the drain leakage current during the transistor operation of the GaN-HEMT can be suppressed.
[0131] In order to suppress the doping concentration of the compensating impurities, the total donor impurity concentration of the GaN substrate of the present embodiment in the first embodiment is preferably less than 4.0×10 16 atoms / cm 3 , more preferably less than 2.0×10 16 atoms / cm 3 .
[0132] The total donor impurity concentration refers to the sum of the concentrations of the donor impurities contained in the GaN substrate of the present embodiment in the first mode. As impurities that act as donors for GaN, O (oxygen), Si (silicon), S (sulfur), Ge (germanium), or Sn (tin) are known. The total donor impurity concentration can be obtained by SIMS.
[0133] Of the two large-area surfaces of the GaN substrate, i.e., a pair of main surfaces, the (0001) surface is used as the front surface for epitaxial growth of the nitride semiconductor layer including the GaN buffer layer. The (0001) surface of the GaN substrate has been mirror-finished, and its root mean square (RMS) roughness measured by atomic force microscopy (AFM) is usually less than 2nm, preferably less than 1nm, and more preferably less than 0.5nm in a measurement range of 2μm×2μm.
[0134] The (000-1) surface of the GaN substrate is the back surface, and therefore, it may be mirror-finished or matte (rough-finished).
[0135] ·i-GaN layer
[0136] In the present embodiment of the first aspect, when the GaN buffer layer includes a C-containing region, the GaN buffer layer preferably has an i-GaN layer in the
[0001] axis direction relative to the C-containing region. More preferably, the i-GaN layer is directly disposed on the C-containing region.
[0137] Having an i-GaN layer in the
[0001] axis direction relative to the C-containing region means that the i-GaN layer exists in the +c axis direction, that is, the Ga polarity plane direction of the crystal, compared to the C-containing region. The i-GaN layer is a crystalline layer formed of GaN that is epitaxially grown without intentional impurity doping, and is distinguished from the C-containing region by the C concentration. That is, the C concentration of the i-GaN layer is less than 1×10 16 atoms / cm 3 When the GaN epitaxial substrate of the present embodiment in the first aspect is used for a HEMT, the i-GaN layer functions as a so-called channel layer.
[0138] In order to reduce the drain leakage current during HEMT operation, the thinner the thickness of the GaN buffer layer in the c-axis direction, the better. The thickness of the i-GaN layer in the GaN buffer layer in the c-axis direction is preferably 50 to 900 nm, more preferably 100 to 600 nm, and further preferably 200 to 500 nm. Here, from the perspective of normal device production, the thickness of the i-GaN layer is preferably greater than 50 nm, more preferably greater than 100 nm, and further preferably greater than 200 nm. In addition, from the perspective of reducing leakage current, the thickness of the i-GaN layer is preferably less than 900 nm, more preferably less than 600 nm, and further preferably less than 500 nm.
[0139] It is preferable that the upper end face of the i-GaN layer in the GaN buffer layer coincide with the upper end face of the GaN buffer layer.
[0140] Nitride semiconductor barrier layer
[0141] The GaN epitaxial substrate of the present embodiment in the first embodiment preferably further has a nitride semiconductor barrier layer on the GaN buffer layer, and more preferably the GaN buffer layer has the above-mentioned i-GaN layer, and further has a nitride semiconductor barrier layer on the above-mentioned i-GaN layer. Preferred examples of the nitride semiconductor barrier layer include Al x Ga 1-xThe N (0<x<1) layer may be an AlInGaN layer. 2DEG is generated in a region sandwiched between the i-GaN layer and the nitride semiconductor barrier layer.
[0142] As a typical example, Al2O3 is formed on a GaN substrate with the (0001) plane as the primary surface. x Ga 1-x In the heterostructure of N(0<x<1) / GaN, 2DEG is generated at the heterointerface by spontaneous polarization and piezoelectric polarization, and even without any doping, 1×10 13 cm -2 Therefore, when the GaN epitaxial substrate of the present embodiment in the first aspect is used for HEMT, it is necessary to include a nitride semiconductor barrier layer.
[0143] The thickness of the nitride semiconductor barrier layer in the c-axis direction is preferably 1 to 50 nm, more preferably 5 to 40 nm, and further preferably 10 to 30 nm. Here, from the perspective of normal device production, the thickness of the nitride semiconductor barrier layer is preferably 1 nm or more, more preferably 5 nm or more, and further preferably 10 nm or more. In addition, from the perspective of reducing leakage current, the thickness of the nitride semiconductor barrier layer is preferably 50 nm or less, more preferably 40 nm or less, and further preferably 30 nm or less.
[0144] GaN cap layer
[0145] In the case where the GaN epitaxial substrate of the present embodiment in the first mode has a nitride semiconductor barrier layer, a GaN cap layer may be provided on the nitride semiconductor barrier layer as required. The thickness of the GaN cap layer in the c-axis direction is preferably 0.1 to 10 nm, more preferably 0.5 to 8 nm, and further preferably 1 to 5 nm. Here, from the perspective of normal device fabrication, the thickness of the GaN cap layer is preferably greater than 0.1 nm, more preferably greater than 0.5 nm, and further preferably greater than 1 nm. In addition, from the perspective of reducing leakage current, the thickness of the GaN cap layer is preferably less than 10 nm, more preferably less than 8 nm, and further preferably less than 5 nm.
[0146] The GaN epitaxial substrate of the present embodiment in the first aspect can be preferably used for the production of a nitride semiconductor device, particularly a nitride semiconductor device having a horizontal device structure.
[0147] In the case of nitride semiconductor devices, one or more nitride semiconductor layers can be epitaxially grown on the above-mentioned GaN epitaxial substrate as needed. Nitride semiconductors are also called nitride III-V compound semiconductors, III-nitride compound semiconductors, GaN semiconductors, etc., and in addition to GaN, they also include compounds formed by replacing part or all of the gallium of GaN with other elements of Group 13 of the periodic table (B, Al, In, etc.).
[0148] Then, electrodes may be provided on the GaN epitaxial substrate according to the type of nitride semiconductor device to be manufactured.
[0149] A typical example of a nitride semiconductor device with a horizontal device structure is GaN-HEMT (High Electron Mobility Transistor).
[0150] [Method for manufacturing GaN epitaxial substrate]
[0151] The method for manufacturing the GaN epitaxial substrate of the present embodiment in the first embodiment is not particularly limited, and an embodiment thereof will be described below as an example. In addition, a preferred embodiment of the GaN epitaxial substrate obtained by the above manufacturing method is the same as the preferred embodiment described in the above [GaN epitaxial substrate].
[0152] The method for manufacturing a GaN epitaxial substrate according to the above-mentioned one embodiment as a first mode includes at least a step of preparing a GaN substrate and then a step of epitaxially growing a GaN buffer layer on the GaN substrate.
[0153] The GaN substrate used in the GaN epitaxial substrate of the present embodiment in the first embodiment may be a GaN substrate having an Fe-doped layer doped with Fe, or a GaN substrate without an Fe-doped layer, as described in the description of [GaN epitaxial substrate] in the first embodiment. When a GaN substrate without an Fe-doped layer is used, it is necessary to dope Fe in the GaN buffer layer in order to achieve semi-insulation using Fe, as described later.
[0154] The GaN substrate can be manufactured by a known method or a commercial product can be used. When manufacturing a GaN substrate, the step of preparing the GaN substrate becomes a step of manufacturing the GaN substrate, preferably a step of manufacturing a GaN substrate doped with Fe.
[0155] The Fe-doped GaN substrate can be obtained, for example, by growing an Fe-doped GaN crystal on a seed crystal by the HVPE method and performing processing such as slicing, grinding, and polishing.
[0156] ·GaN buffer layer formation method
[0157] The method for epitaxially growing the GaN buffer layer on the GaN substrate is not particularly limited, and various known methods can be used. Preferred examples include MOCVD and Molecular Beam Epitaxy (MBE).
[0158] When the MOCVD method is used, the raw material gas is not particularly limited as long as it contains a Ga source and an N source for forming GaN, and a known gas can be used.
[0159] In the case where the GaN substrate is a GaN substrate doped with Fe as described above, it is not necessary to dope the epitaxially grown GaN buffer layer with Fe. However, in the case of a GaN substrate that does not include an Fe-doped layer doped with Fe, a region doped with Fe is formed in the GaN epitaxial substrate by doping the epitaxially grown GaN buffer layer with Fe. In this case, it is considered that it is preferable for the manufacturing method of the GaN epitaxial substrate to include a step of doping with Fe in a part of the step of epitaxially growing the GaN buffer layer. In addition, it is preferable that the step of doping with Fe is performed before the step of forming the C-containing region described later.
[0160] In order to make the Fe concentration in the GaN epitaxial substrate of the present embodiment in the first mode satisfy the characteristics of any of the first to fourth embodiments described above, it is preferred that at least a part of the step of epitaxially growing the GaN buffer layer includes forming a GaN epitaxial substrate having a C concentration of 1×10 16 atoms / cm 3 The C-containing region is preferably formed by doping C in the epitaxially grown GaN buffer layer. It should be noted that, in the first embodiment of the first mode, the above-mentioned characteristics refer to [Fe] B / [Fe] A is 1 / 100, the distance between point A and point B is 0.2 μm or less, and in the second embodiment of the first aspect, it means [Fe] B’ / [Fe] A’ is 1 / 10, the distance between point A' and point B' is 0.1 μm or less, and in the third embodiment of the first embodiment, the Fe concentration at point A" is 1×10 17 atoms / cm 3 Above, the Fe concentration at point B" is 1×10 15 atoms / cm 3 Hereinafter, the distance between point A" and point B" is 0.2 μm or less, and in the fourth embodiment of the first embodiment, the Fe concentration at point A"' is 1×10 17atoms / cm 3 Above, the Fe concentration at point B'' is 1×10 16 atoms / cm 3 Hereinafter, the distance between point A''' and point B'''' is less than 0.1 μm.
[0161] It is preferred to dope C in a region existing in the
[0001] axis direction relative to a region doped with Fe. Therefore, when a GaN substrate includes a region doped with Fe, the C-containing region must exist in the
[0001] axis direction relative to the region doped with Fe. On the other hand, when a GaN buffer layer formed by epitaxial growth includes a region doped with Fe, it is preferred to perform a C doping step after performing a Fe doping step.
[0162] In the first embodiment to the fourth embodiment of the first mode, C is preferably doped in such a manner that the C-containing region includes point B, point B', point B", or point B'". In addition, it is also preferred to dope C on the (000-1) plane side relative to the plane parallel to the (0001) plane and including point B, the plane parallel to the (0001) plane and including point B', the plane parallel to the (0001) plane and including point B", or the plane parallel to the (0001) plane and including point B'". The latter is doped with C between the plane parallel to the (0001) plane and including point A, point A', point A", or point A'" and the plane parallel to the (0001) plane and including point B, point B', point B", or point B'"'.
[0163] In the case of C doping in the epitaxially grown GaN buffer layer, the C concentration is 1×10 16 atoms / cm 3 The thickness of the C-containing region in the c-axis direction (height in the thickness direction) is preferably 50 to 900 nm as described in the first embodiment of the [GaN epitaxial substrate] in the first embodiment. Here, from the perspective of normal device production, the thickness is preferably 50 nm or more, and from the perspective of reducing leakage current, it is preferably 900 nm or less.
[0164] The concentration of C in the C-containing region is 1×10 16 atoms / cm 3 The above concentration can be 5×10 16 atoms / cm 3 Above, 1×10 17 atoms / cm 3 Above and more.
[0165] In order to avoid a significant decrease in crystal quality due to overdoping, the C concentration in the GaN buffer layer including the C-containing region is preferably 1×10 18 atoms / cm3 Below, or less than 1×10 18 atoms / cm 3 , is 8×10 17 atoms / cm 3 Below, 5×10 17 atoms / cm 3 The following etc.
[0166] C can be doped by a conventionally known method, for example, preferably by MOCVD or MBE.
[0167] In the case of using the MOCVD method, as the raw material gas, for example, a hydrocarbon gas such as CH4 (methane) can be used. From the perspective of simplification, it is preferred to use a raw material gas that also contains a Ga source and an N source for forming GaN. From the above perspective, as the raw material gas of C, trimethylgallium (TMG) and triethylgallium (TEG) are preferably used, and TMG is more preferred. In addition, it is further preferred to use a mixed gas of TMG and ammonia (NH3) or a mixed gas of TEG and NH3.
[0168] When a mixed gas of trimethylgallium (TMG) and ammonia (NH3) is used, the supply rate of TMG is preferably 100 to 500 μmol / min, more preferably 200 to 300 μmol / min. Here, from the viewpoint of reducing the concentration of impurities such as Si, the supply rate of TMG is preferably 100 μmol / min or more, more preferably 200 μmol / min or more. In addition, from the viewpoint of film thickness controllability, the supply rate of TMG is preferably 500 μmol / min or less, more preferably 300 μmol / min or less.
[0169] From the viewpoint of controllability of C concentration, the supply rate ratio represented by TMG:NH3 is preferably 1:100 to 1:4000, more preferably 1:500 to 1:4000 or 1:100 to 1:2000, and further preferably 1:500 to 1:2000.
[0170] In the case where C is doped to form a C-containing region and Fe is also doped in the epitaxially grown GaN buffer layer, it is preferred that Fe doping and C doping are performed discontinuously from the viewpoint of reducing the memory effect between epitaxial growths. In other words, it is preferred to avoid continuously doping C after Fe doping. "Continuously performed" means, for example, that the Fe doping operation and the C doping operation are not purged or separated by an interval of more than several hours, and the C doping operation is performed after the Fe doping operation using the same growth device.
[0171] It should be noted that, when C is doped to form a C-containing region and a substrate having a region doped with Fe is used as a GaN substrate, it is natural that Fe doping and C doping are performed discontinuously in the entire manufacturing process.
[0172] As described above, as an epitaxial GaN buffer layer, an i-GaN layer can be formed after forming an Fe-doped region and a C-containing region doped with Fe as needed. When the GaN epitaxial substrate of this embodiment in the first mode is used for HEMT, the i-GaN layer functions as a so-called channel layer, so it is necessary to form an i-GaN layer. The method of forming the i-GaN layer is no different from the method of epitaxially growing the GaN buffer layer, except that it is not accompanied by intentional impurity doping. As preferred examples, MOCVD method and MBE method can be cited.
[0173] When the i-GaN layer is formed by MOCVD, a hydrocarbon gas such as CH4 (methane) can be used as a raw material gas. From the perspective of simplification, it is preferable to use a raw material gas that also contains a Ga source and an N source for forming GaN.
[0174] When a mixed gas of trimethylgallium (TMG) and ammonia (NH3) is used, the supply rate of TMG is preferably 50 to 250 μmol / min, and more preferably 100 to 150 μmol / min or less. Here, from the viewpoint of reducing the concentration of impurities such as Si, the supply rate of TMG is preferably 50 μmol / min or more, and more preferably 100 μmol / min or more. In addition, from the viewpoint of film thickness controllability, the supply rate of TMG is preferably 250 μmol / min or less, and more preferably 150 μmol / min or less.
[0175] From the viewpoint of reducing the C concentration, the supply rate ratio represented by TMG:NH3 is preferably 1:400 to 1:16000, more preferably 1:400 to 1:1800 or 1:2000 to 1:16000, and further preferably 1:2000 to 1:8000.
[0176] The thickness of the i-GaN layer in the GaN buffer layer in the c-axis direction is the same as that described in the present embodiment of the [GaN epitaxial substrate] in the first embodiment, and is preferably 50 to 900 nm. Here, from the perspective of normal device production, the above thickness is preferably 50 nm or more, and from the perspective of reducing leakage current, it is preferably 900 nm or less.
[0177] ·Method for forming nitride semiconductor barrier layer
[0178] After forming the above-mentioned epitaxial GaN buffer layer, a nitride semiconductor barrier layer may be formed. When the GaN epitaxial substrate of the present embodiment in the first mode is used for HEMT, a nitride semiconductor barrier layer needs to be formed in order to generate 2DEG. Preferred examples of the barrier layer include Al x Ga 1-x The N (0<x<1) layer may be an AlInGaN layer. 2DEG is generated in a region sandwiched by the GaN buffer layer and the nitride semiconductor barrier layer.
[0179] The method for forming the nitride semiconductor barrier layer is not particularly limited, and a conventionally known method can be adopted. Preferred examples include MOCVD and MBE.
[0180] The preferred thickness of the nitride semiconductor barrier layer on the GaN buffer layer in the c-axis direction is the same as that described in this embodiment of the [GaN epitaxial substrate] in the first aspect described above.
[0181] When the above-mentioned nitride semiconductor barrier layer is formed, a conventionally known layer such as a GaN cap layer may be formed by a conventionally known method as needed.
[0182] The Second Way
[0183] [GaN epitaxial substrate]
[0184] The GaN epitaxial substrate of the first embodiment in the second aspect includes a GaN substrate and a GaN buffer layer epitaxially grown on the GaN substrate. At least one of the GaN substrate and the GaN buffer layer includes an Fe-doped layer doped with Fe, and the GaN buffer layer includes a C-containing layer that is present in the
[0001] axis direction relative to the Fe-doped layer and has a C concentration of 1×10 16 ~1×10 18 atoms / cm 3 .
[0185] The C-containing layer exists in the
[0001] axis direction relative to the Fe-doped layer, which means that the C-containing layer exists in the +c axis direction, that is, the Ga polarity plane direction of the crystal, compared with the Fe-doped layer. The same also applies to the relationship between the C-containing layer and the GaN region described later, the relationship between the Fe-doped layer and the Fe diffusion suppression layer, the relationship between the Fe diffusion suppression layer and the GaN region in the second embodiment described later, the relationship between point A and point B, and the relationship between point A' and point B' in the first and second embodiments.
[0186] The Fe-doped layer doped with Fe means that the Fe concentration is 1×10 17 atoms / cm 3The above region can be distinguished from the case where Fe is unintentionally introduced during the process of manufacturing the GaN epitaxial substrate.
[0187] For the Fe-doped layer doped with Fe, by making the C concentration 1×10 16 ~1×10 18 atoms / cm 3 The C-containing layer exists in the
[0001] axis direction relative to the Fe-doped layer, thereby hindering the movement of Fe between different regions defined by the C-containing layer.
[0188] The movement of Fe in the GaN epitaxial substrate usually occurs due to thermal diffusion defined by the diffusion equation. Therefore, the concentration distribution of Fe in the GaN epitaxial substrate should be described by the diffusion equation. However, it was found that in the presence of a C-containing layer, the concentration distribution of Fe around the C-containing layer deviates from the behavior predicted by the diffusion equation and exhibits a steep Fe concentration gradient. Therefore, it can be considered that the presence of a C-containing layer can effectively hinder the movement of Fe in the GaN epitaxial substrate.
[0189] In the manufacturing method of GaN epitaxial substrate, C from impurities may be unintentionally introduced into the C-containing layer at a concentration above a certain level. In this case, if the C concentration is 1×10 16 ~1×10 18 atoms / cm 3 On the other hand, in the manufacturing method of GaN epitaxial substrate, the C concentration may not reach 1×10 16 atoms / cm 3 In this case, the C-containing layer is preferably a layer doped with C. As such a manufacturing method, for example, MOCVD method, molecular beam epitaxy (MBE) method, etc. It should be noted that it is not excluded that on the basis of the above-mentioned manufacturing method of unintentionally introducing C from impurities, C is further doped to make a C-containing layer.
[0190] The C concentration of the C-containing layer is preferably 1×10 16 atoms / cm 3 Above and 1×10 18 atoms / cm 3 Less than, more preferably 5×10 16 atoms / cm 3 More than and less than 1×10 18 atoms / cm 3 , more preferably 1×10 17 atoms / cm 3 Above and 8×10 17atoms / cm 3 Below, particularly preferably 1×10 17 atoms / cm 3 Above and 5×10 17 atoms / cm 3 Here, as long as the C concentration of the C-containing layer is 1×10 16 atoms / cm 3 From the viewpoint of further inhibiting the movement of Fe, 5×10 16 atoms / cm 3 More preferably 1×10 17 atoms / cm 3 In addition, from the viewpoint of preventing the occurrence of defects such as threading dislocations and preventing leakage current caused by C, the C concentration of the C-containing layer is 1×10 18 atoms / cm 3 Below, preferably less than 1×10 18 atoms / cm 3 , more preferably 8×10 17 atoms / cm 3 Below, more preferably 5×10 17 atoms / cm 3 the following.
[0191] The thickness of the C-containing layer in the c-axis direction is preferably 50 to 900 nm, more preferably 100 to 600 nm, and further preferably 200 to 500 nm. Here, from the perspective of normal device production, the thickness of the C-containing layer is preferably 50 nm or more, more preferably 100 nm or more, and further preferably 200 nm or more. In addition, from the perspective of reducing leakage current, the thickness of the C-containing layer is preferably 900 nm or less, more preferably 600 nm or less, and further preferably 500 nm or less.
[0192] The thickness of the C-containing layer in the c-axis direction is preferably 5 to 90% of the total film thickness of the GaN buffer layer, more preferably 10 to 80%, and further preferably 20 to 70%. Here, from the perspective of normal device production, the thickness of the C-containing layer in the c-axis direction is preferably more than 5% of the total film thickness of the GaN buffer layer, more preferably more than 10%, and further preferably more than 20%. In addition, from the same point of view, the above thickness is preferably less than 90% of the total film thickness of the GaN buffer layer, more preferably less than 80%, and further preferably less than 70%. It should be noted that, in the case where the GaN buffer layer includes an Fe-doped layer, a C-containing layer, an i-GaN layer, etc. as described later, the total film thickness of the GaN buffer layer refers to the total thickness in the c-axis direction including them.
[0193] It is sufficient that at least one of the GaN substrate and the GaN buffer layer includes an Fe-doped layer, and from the viewpoint of ease of production, it is preferably included in the GaN substrate.
[0194] The above-mentioned ease of manufacturing is explained. In the case where an Fe-doped layer doped with Fe exists in a GaN buffer layer, the Fe-doped layer and the C-containing layer are both included in the GaN buffer layer epitaxially grown by MOCVD method or the like. Sometimes, when forming the Fe-doped layer, the Fe dopant gas used for doping with Fe will remain in the reaction tube, and Fe will be unintentionally introduced into the region after the Fe-doped layer is formed. If such an unexpected introduction of Fe occurs, it will be difficult to obtain the effect of the present invention that the movement of Fe is effectively hindered by forming a C-containing layer containing a specific C concentration, and further steps are required to control the concentration gradient of Fe. In contrast, if an Fe-doped layer exists in the GaN substrate, the above-mentioned unexpected introduction of Fe can be prevented, and therefore, the GaN epitaxial substrate of the present embodiment in the second mode can be easily manufactured.
[0195] It should be noted that, in the case where the GaN buffer layer includes an Fe-doped layer doped with Fe, and the C-containing layer is a layer doped with C, from the viewpoint of reducing the memory effect during epitaxial growth, it is preferred that the Fe doping when forming the Fe-doped layer and the C doping when forming the C-containing layer are performed discontinuously. In other words, it is preferred to avoid continuously doping C after Fe doping. "Continuously performed" means, for example, that the Fe doping operation and the C doping operation are not purged or separated by an interval of more than several hours, and the C doping operation is performed after the Fe doping operation using the same growth device.
[0196] The Fe concentration of the Fe-doped layer doped with Fe is preferably 1×10 17 ~1×10 20 atoms / cm 3 , more preferably 5×10 17 ~1×10 19 atoms / cm 3 , more preferably 1×10 18 ~5×10 18 atoms / cm 3 Here, it is 1×10 17 atoms / cm 3 From the viewpoint of ensuring sufficient semi-insulation, the Fe concentration of the Fe-doped layer is preferably 5×10 17 atoms / cm 3 More preferably 1×10 18 atoms / cm 3In addition, from the viewpoint of maintaining good crystal quality, the Fe concentration of the Fe-doped layer is preferably 1×10 20 atoms / cm 3 Less than, more preferably 1×10 19 atoms / cm 3 Below, more preferably 5×10 18 atoms / cm 3 the following.
[0197] The thickness of the Fe-doped layer in the c-axis direction is preferably 50 to 500 μm, more preferably 80 to 450 μm, and further preferably 100 to 400 μm. Here, from the perspective of reducing the drain leakage current during transistor operation, the thickness of the Fe-doped layer is preferably 50 μm or more, more preferably 80 μm or more, and further preferably 100 μm or more. In addition, from the perspective of shortening the substrate thinning time during chip processing, the thickness of the Fe-doped layer is preferably 500 μm or less, more preferably 450 μm or less, and further preferably 400 μm or less.
[0198] In the case where the GaN substrate includes an Fe-doped layer, the upper end face of the Fe-doped layer is preferably present at a position consistent with the (0001) surface of the GaN substrate. The thickness of the Fe-doped layer in the c-axis direction does not need to be consistent with the thickness of the GaN substrate in the c-axis direction. For example, relative to the overall thickness of the GaN substrate of 400 μm, the thickness of the Fe-doped layer is sufficient as long as it is 100 μm of the surface layer of the GaN substrate. Of course, the thickness of the Fe-doped layer is not limited to the above thickness, and the case of being thicker or thinner than the above thickness is not excluded. In addition, the GaN substrate may be composed of an Fe-doped layer as a whole in the thickness direction of the GaN substrate.
[0199] When the GaN substrate includes an Fe-doped layer, the thickness of the Fe-doped layer may be 50 μm to 500 μm. When the GaN substrate includes an Fe-doped layer, the thickness of the Fe-doped layer may be 50 μm or more, 80 μm or more, or 100 μm or more. On the other hand, it may be 500 μm or less.
[0200] When the GaN substrate includes an Fe-doped layer, the C concentration in the Fe-doped layer is preferably 5×10 16 atoms / cm 3 In the case where the GaN substrate includes an Fe-doped layer, the C concentration in the Fe-doped layer may be 4×10 16 atoms / cm 3 Below, or 3×10 16 atoms / cm 3 Below, or 2×10 16 atoms / cm3 Below, or less than 1×10 16 atoms / cm 3 .
[0201] In terms of the relationship with the Fe-doped layer, from the viewpoint of making the Fe concentration gradient steep and more appropriately suppressing the diffusion of Fe, the Fe concentration in the GaN region present in the C-containing layer in the GaN buffer layer or in the GaN region present in the
[0001] axis direction relative to the C-containing layer is preferably less than 1×10 17 atoms / cm 3 , more preferably 1×10 16 atoms / cm 3 Below, more preferably 1×10 15 atoms / cm 3 Below, more preferably 5×10 14 atoms / cm 3 Below, particularly preferably 1×10 14 atoms / cm 3 the following.
[0202] In addition, the lower limit of the Fe concentration in the GaN region is not particularly limited, and the detection limit of Fe is usually consistent with the lower limit. It should be noted that, when the GaN buffer layer includes an i-GaN layer described later, the C-containing layer is present in the
[0001] axis direction and has a C concentration of less than 1×10 16 atoms / cm 3 The GaN region may have the same meaning as the i-GaN layer.
[0203] The GaN epitaxial substrate of the first embodiment in the second aspect preferably includes a point A and a point B that satisfy the following specific conditions. Point A is included in the GaN substrate or the GaN buffer layer, and point B is included in the GaN buffer layer. In addition, point B is located on a straight line that passes through point A and is parallel to the
[0001] axis, and exists in the
[0001] axis direction relative to point A. The Fe concentration [Fe] at point B is B and the Fe concentration at point A [Fe] A The ratio ([Fe] B / [Fe] A ) is 1 / 100, and the distance between point A and point B is less than 0.2μm.
[0204] As one embodiment of the above-mentioned point A and point B, it is preferred that point B exists in the C-containing layer or that a C-containing layer exists between point A and point B. That is, it is preferred that the C-containing layer includes point B or is located on the (000-1) plane side with respect to a plane parallel to the (0001) plane and including point B.
[0205] In addition, point A is preferably present in the Fe-doped layer. Point B is preferably present in the GaN buffer layer, and more preferably included in the C-containing layer or the GaN region. However, point A and point B are not limited to the above-mentioned forms.
[0206] [Fe] B / [Fe] A The distance between point A and point B being 1 / 100 of 0.2 μm or less means that the Fe concentration gradient between point A and point B is steep, which can appropriately inhibit the diffusion of Fe. This ensures the semi-insulating property brought about by Fe and inhibits the diffusion of Fe to the region where 2DEG is generated in the GaN-HEMT structure.
[0207] The distance between point A and point B can be 0.2 μm or less, and is preferably 0.15 μm or less, more preferably 0.13 μm or less, and further preferably 0.12 μm or less from the viewpoint of making the concentration gradient of Fe steeper. In addition, the shorter the distance between point A and point B, the better, but from the viewpoint of feasibility, it is usually 0.01 μm or more.
[0208] Fe concentration at point A [Fe] A Preferably 1×10 17 ~1×10 20 atoms / cm 3 , more preferably 5×10 17 ~1×10 19 atoms / cm 3 , more preferably 1×10 18 ~5×10 18 atoms / cm 3 Here, from the perspective of ensuring sufficient semi-insulation, [Fe] A Preferably 1×10 17 atoms / cm 3 More preferably 5×10 17 atoms / cm 3 More preferably, 1×10 18 atoms / cm 3 In addition, from the perspective of maintaining good crystal quality, [Fe] A Preferably 1×10 20 atoms / cm 3 Less than, more preferably 1×10 19 atoms / cm 3 Below, more preferably 5×10 18 atoms / cm 3 the following.
[0209] Since the Fe concentration at point B [Fe] B is the Fe concentration at point A [Fe] A 1 / 100 of the point, therefore, [Fe] B The preferred range of [Fe] A Change accordingly.
[0210] The GaN epitaxial substrate of the first embodiment in the second embodiment preferably includes a point A' and a point B' that satisfy the following specific conditions. Point A' is included in the GaN substrate or the GaN buffer layer, and point B' is included in the GaN buffer layer. In addition, point B' is located on a straight line that passes through point A' and is parallel to the
[0001] axis, and exists in the
[0001] axis direction relative to point A'. The Fe concentration [Fe] at point B' B’ and the Fe concentration at point A' [Fe] A’ The ratio ([Fe] B’ / [Fe] A’ ) is 1 / 10, and the distance between point A' and point B' is less than 0.15 μm.
[0211] As one embodiment of the above-mentioned point A' and point B', it is preferred that point B' exists in the C-containing layer, or that a C-containing layer exists between point A' and point B'. That is, it is preferred that the C-containing layer includes point B', or is located on the (000-1) plane side with respect to a plane parallel to the (0001) plane and including point B'.
[0212] In addition, point A' is preferably included in the Fe-doped layer. Point B' is preferably included in the GaN buffer layer, and more preferably included in the C-containing layer or the GaN region. However, point A' and point B' are not limited to the above-mentioned forms.
[0213] [Fe] B’ / [Fe] A’ The fact that the distance between point A' and point B' is 0.15 μm or less means that the Fe concentration gradient between points A' and B' is steep, which can appropriately inhibit the diffusion of Fe. This ensures the semi-insulation brought about by Fe and inhibits the diffusion of Fe to the region where 2DEG is generated in the GaN-HEMT structure.
[0214] The distance between point A' and point B' only needs to be 0.15 μm or less. From the perspective of making the Fe concentration gradient steeper, it is preferably 0.13 μm or less, more preferably 0.10 μm or less, further preferably 0.08 μm or less, and particularly preferably 0.05 μm or less. In addition, the shorter the distance between point A' and point B', the better. However, from the perspective of feasibility, it is usually 0.01 μm or more.
[0215] Fe concentration at point A' [Fe] A’ Preferably 1×1017 ~1×10 20 atoms / cm 3 , more preferably 5×10 17 ~1×10 19 atoms / cm 3 , more preferably 1×10 18 ~5×10 18 atoms / cm 3 Here, from the perspective of ensuring sufficient semi-insulation, [Fe] A’ Preferably 1×10 17 atoms / cm 3 More preferably 5×10 17 atoms / cm 3 More preferably, 1×10 18 atoms / cm 3 In addition, from the perspective of maintaining good crystal quality, [Fe] A’ Preferably 1×10 20 atoms / cm 3 Less than, more preferably 1×10 19 atoms / cm 3 Below, more preferably 5×10 18 atoms / cm 3 the following.
[0216] Since the Fe concentration at point B' [Fe] B’ The Fe concentration at point A' becomes [Fe] A’ 1 / 10 of the point, therefore, [Fe] B’ The preferred range of [Fe] A’ Change accordingly.
[0217] The GaN epitaxial substrate of the second embodiment in the second mode includes a GaN substrate and a GaN buffer layer epitaxially grown on the GaN substrate. The GaN substrate or the GaN buffer layer includes an Fe-doped layer doped with Fe, and the GaN buffer layer includes an Fe diffusion suppression layer that exists in the
[0001] axis direction relative to the Fe-doped layer and suppresses the diffusion of Fe. The Fe diffusion suppression layer is a layer containing C.
[0218] The Fe-doped layer doped with Fe means that the Fe concentration is 1×10 17 atoms / cm 3 The above regions can be distinguished from the case where Fe is unintentionally introduced during the process of manufacturing the GaN epitaxial substrate.
[0219] In the Fe-doped layer doped with Fe, by providing the Fe diffusion suppression layer containing C in the
[0001] axis direction relative to the Fe-doped layer, the movement of Fe between different regions defined by the Fe diffusion suppression layer can be inhibited.
[0220] The movement of Fe in the GaN epitaxial substrate usually occurs due to thermal diffusion defined by the diffusion equation. Therefore, the concentration distribution of Fe in the GaN epitaxial substrate should be described by the diffusion equation. However, it was found that in the presence of an Fe diffusion suppression layer, the concentration distribution of Fe around the Fe diffusion suppression layer deviates from the behavior predicted by the diffusion equation and shows a steep Fe concentration gradient. Therefore, it can be considered that the movement of Fe in the GaN epitaxial substrate can be effectively hindered by the presence of the Fe diffusion suppression layer.
[0221] Through the manufacturing method of the GaN epitaxial substrate, C from impurities is sometimes unintentionally introduced into the Fe diffusion suppression layer at a concentration above a certain level. In this case as well, if the C concentration is above a certain level, the effect of the present invention can be exerted. On the other hand, through the manufacturing method of the GaN epitaxial substrate, the C concentration sometimes cannot exert the effect of the present invention only through the impurity source. In this case, the Fe diffusion suppression layer is preferably a layer doped with C. As such a manufacturing method, for example, there can be cited: MOCVD method, Molecular Beam Epitaxy (MBE) method, etc. It should be noted that it is not excluded that on the basis of adopting the above-mentioned manufacturing method in which C from impurities is unintentionally introduced, C is further doped to make a C-containing layer.
[0222] The C concentration of the Fe diffusion suppression layer is preferably 1×10 16 ~1×10 18 atoms / cm 3 , more preferably 5×10 16 atoms / cm 3 More than and less than 1×10 18 atoms / cm 3 , more preferably 1×10 17 atoms / cm 3 Above and 8×10 17 atoms / cm 3 Below, more preferably 1×10 17 atoms / cm 3 Above and 5×10 17 atoms / cm 3 Here, the C concentration of the Fe diffusion suppression layer is preferably 1×10 16 atoms / cm 3From the viewpoint of further inhibiting the movement of Fe, 5×10 16 atoms / cm 3 More preferably, 1×10 17 atoms / cm 3 In addition, from the viewpoint of preventing the occurrence of defects such as threading dislocations and preventing leakage current caused by C, the C concentration of the Fe diffusion suppression layer is preferably 1×10 18 atoms / cm 3 Less than 1×10 18 atoms / cm 3 , more preferably 8×10 17 atoms / cm 3 Below, more preferably 5×10 17 atoms / cm 3 the following.
[0223] The thickness of the Fe diffusion suppression layer in the c-axis direction is preferably 50 to 900 nm, more preferably 100 to 600 nm, and further preferably 200 to 500 nm. Here, from the perspective of normal device production, the thickness of the Fe diffusion suppression layer is preferably 50 nm or more, more preferably 100 nm or more, and further preferably 200 nm or more. In addition, from the perspective of reducing leakage current, the thickness of the Fe diffusion suppression layer is preferably 900 nm or less, more preferably 600 nm or less, and further preferably 500 nm or less.
[0224] The thickness of the Fe diffusion suppression layer in the c-axis direction is preferably 5 to 90% of the total film thickness of the GaN buffer layer, more preferably 10 to 80%, and further preferably 20 to 70%. Here, from the perspective of normal device production, the thickness of the Fe diffusion suppression layer is preferably more than 5% of the total film thickness of the GaN buffer layer, more preferably more than 10%, and further preferably more than 20%. In addition, from the same point of view, the above thickness is preferably less than 90% of the total film thickness of the GaN buffer layer, more preferably less than 80%, and further preferably less than 70%. It should be noted that, as described later, when the GaN buffer layer includes an Fe-doped layer, an Fe diffusion suppression layer, an i-GaN layer, etc., the total film thickness of the GaN buffer layer refers to the total thickness in the c-axis direction including them.
[0225] The Fe-doped layer doped with Fe may be included in either the GaN substrate or the GaN buffer layer, and is preferably included in the GaN substrate from the viewpoint of ease of production.
[0226] The above-mentioned ease of production is the same as that of the Fe-doped layer of the first embodiment in the second aspect.
[0227] The Fe concentration of the Fe-doped layer doped with Fe is preferably 1×10 17 ~1×10 20 atoms / cm 3 , more preferably 5×10 17 ~1×10 19 atoms / cm 3 , more preferably 1×10 18 ~5×10 18 atoms / cm 3 Here, the Fe concentration of the Fe-doped layer is 1×10 17 atoms / cm 3 From the viewpoint of ensuring sufficient semi-insulation, 5×10 17 atoms / cm 3 More preferably 1×10 18 atoms / cm 3 In addition, from the viewpoint of maintaining good crystal quality, the Fe concentration of the Fe-doped layer is preferably 1×10 20 atoms / cm 3 Less than, more preferably 1×10 19 atoms / cm 3 Below, more preferably 5×10 18 atoms / cm 3 the following.
[0228] The thickness of the Fe-doped layer in the c-axis direction is preferably 50 to 500 nm, more preferably 80 to 450 nm, and further preferably 100 to 400 nm. Here, from the perspective of reducing the drain leakage current during transistor operation, the thickness of the Fe-doped layer is preferably 50 μm or more, more preferably 80 μm or more, and further preferably 100 μm or more. In addition, from the perspective of shortening the substrate thinning time during chip processing, the thickness of the Fe-doped layer is preferably 500 μm or less, more preferably 450 μm or less, and further preferably 400 μm or less.
[0229] In the case where the GaN substrate includes an Fe-doped layer, the upper end face of the Fe-doped layer is preferably present at a position consistent with the (0001) surface of the GaN substrate. The thickness of the Fe-doped layer in the c-axis direction does not need to be consistent with the thickness of the GaN substrate in the c-axis direction. For example, relative to the overall thickness of the GaN substrate of 400 μm, the thickness of the Fe-doped layer is sufficient as long as it is 100 μm of the surface layer of the GaN substrate. Of course, the thickness of the Fe-doped layer is not limited to the above thickness, and the case of being thicker or thinner than the above thickness is not excluded. In addition, the GaN substrate may be composed of an Fe-doped layer as a whole in the thickness direction of the GaN substrate.
[0230] In terms of the relationship with the Fe-doped layer, from the viewpoint that the Fe concentration gradient is steep and the diffusion of Fe can be more appropriately suppressed, the Fe concentration in the GaN region present in the Fe diffusion suppression layer in the GaN buffer layer or in the GaN region present in the
[0001] axis direction relative to the Fe diffusion suppression layer is preferably less than 1×10 17 atoms / cm 3 , more preferably 1×10 16 atoms / cm 3 Below, more preferably 1×10 15 atoms / cm 3 Below, more preferably 5×10 14 atoms / cm 3 Below, particularly preferably 1×10 14 atoms / cm 3 In addition, the lower limit of the Fe concentration in the GaN region is not particularly limited, and the detection limit of Fe is usually consistent with the lower limit. It should be noted that, when the GaN buffer layer includes the i-GaN layer described later, the Fe diffusion suppression layer is present in the
[0001] axis direction and the C concentration is less than 1×10 16 atoms / cm 3 The GaN region may have the same meaning as the i-GaN layer.
[0231] The GaN epitaxial substrate of the second embodiment in the second mode preferably includes a point A and a point B satisfying the following specific conditions. Point A is included in the GaN substrate or the GaN buffer layer, and point B is included in the GaN buffer layer. In addition, point B is located on a straight line passing through point A and parallel to the
[0001] axis, and exists in the
[0001] axis direction relative to point A. The Fe concentration [Fe] at point B is B and the Fe concentration at point A [Fe] A The ratio ([Fe] B / [Fe] A ) is 1 / 100, and the distance between point A and point B is less than 0.2μm.
[0232] In addition, the GaN epitaxial substrate of the second embodiment of the second mode preferably includes a point A' and a point B' that satisfy the following specific conditions. Point A' is included in the GaN substrate or the GaN buffer layer, and point B' is included in the GaN buffer layer. In addition, point B' is located on a straight line passing through point A' and parallel to the
[0001] axis, and exists in the
[0001] axis direction relative to point A'. The Fe concentration [Fe] at point B' B’ Fe concentration at point A' [Fe] A’ The ratio ([Fe]B’ / [Fe] A’ ) is 1 / 10, and the distance between point A' and point B' is less than 0.15 μm.
[0233] Preferred aspects of the point A, point B, point A′ and point B′ are respectively the same as the preferred aspects of the point A, point B, point A′ and point B′ in the first embodiment in the second aspect.
[0234] In any of the first embodiment and the second embodiment in the second aspect (hereinafter sometimes referred to as “this embodiment”), the GaN epitaxial substrate also includes a GaN buffer layer epitaxially grown on the GaN substrate.
[0235] In the second embodiment, a GaN substrate is used instead of a SiC substrate or the like which has been widely used in the past. As a result, defects are less likely to be generated at the interface with the GaN buffer layer to be formed later, and a high-concentration carrier compensation layer for suppressing leakage current is not required, so that the drain leakage current during the transistor operation of the GaN-HEMT can be suppressed.
[0236] In order to suppress the doping concentration of the compensating impurities, the total donor impurity concentration of the GaN substrate of the present embodiment in the second embodiment is preferably less than 4.0×10 16 atoms / cm 3 , more preferably less than 2.0×10 16 atoms / cm 3 .
[0237] The total donor impurity concentration refers to the sum of the concentrations of donor impurities contained in the GaN substrate of the present embodiment in the second mode. As impurities that act as donors for GaN, O (oxygen), Si (silicon), S (sulfur), Ge (germanium), or Sn (tin) are known. The total donor impurity concentration can be obtained by SIMS.
[0238] Of the two large-area surfaces of the GaN substrate, i.e., a pair of main surfaces, the (0001) surface is used as the front surface for epitaxial growth of the nitride semiconductor layer including the GaN buffer layer. The (0001) surface of the GaN substrate has been mirror-finished, and its root mean square (RMS) roughness measured by atomic force microscopy (AFM) is usually less than 2nm, preferably less than 1nm, and more preferably less than 0.5nm in a measurement range of 2μm×2μm.
[0239] The (000-1) surface of the GaN substrate is the back surface, and therefore, it may be mirror-finished or matte (rough-finished).
[0240] ·i-GaN layer
[0241] In the present embodiment of the second mode, it is preferred that the GaN buffer layer has an i-GaN layer in the
[0001] axis direction relative to the C-containing layer or the Fe diffusion suppression layer. It is more preferred that the i-GaN layer is directly disposed on the C-containing layer or the Fe diffusion suppression layer. Having an i-GaN layer in the
[0001] axis direction relative to the C-containing layer or the Fe diffusion suppression layer means that, compared with the C-containing layer or the Fe diffusion suppression layer, the i-GaN layer exists in the +c axis direction, i.e., the Ga polarity plane direction of the crystal. The i-GaN layer is a crystalline layer formed of GaN that is grown epitaxially without intentional impurity doping, and can be distinguished from the C-containing layer or the Fe diffusion suppression layer by the C concentration. That is, the C concentration of the i-GaN layer is less than 1×10 16 atoms / cm 3 When the GaN epitaxial substrate of the present embodiment in the second aspect is used for a HEMT, the i-GaN layer functions as a so-called channel layer.
[0242] In order to reduce the drain leakage current during HEMT operation, the thinner the thickness of the GaN buffer layer in the c-axis direction, the better. The thickness of the i-GaN layer in the GaN buffer layer in the c-axis direction is preferably 50 to 900 nm, more preferably 100 to 600 nm, and further preferably 200 to 500 nm. Here, from the perspective of normal device production, the above-mentioned thickness of the i-GaN layer is preferably greater than 50 nm, more preferably greater than 100 nm, and further preferably greater than 200 nm. In addition, from the perspective of reducing leakage current, the above-mentioned thickness of the i-GaN layer is preferably less than 900 nm, more preferably less than 600 nm, and further preferably less than 500 nm.
[0243] It is preferable that the upper end face of the i-GaN layer in the GaN buffer layer coincide with the upper end face of the GaN buffer layer.
[0244] Nitride semiconductor barrier layer
[0245] The GaN epitaxial substrate of the present embodiment in the second embodiment preferably further comprises a nitride semiconductor barrier layer on the GaN buffer layer, and more preferably the GaN buffer layer comprises the above-mentioned i-GaN layer, and further comprises a nitride semiconductor barrier layer on the above-mentioned i-GaN layer. Preferred examples of the nitride semiconductor barrier layer include Al x Ga 1-x The N (0<x<1) layer may be an AlInGaN layer. 2DEG is generated in a region sandwiched between the i-GaN layer and the nitride semiconductor barrier layer.
[0246] As a typical example, Al2O3 is formed on a GaN substrate with the (0001) plane as the primary surface. x Ga 1-xIn the heterostructure of N(0<x<1) / GaN, 2DEG is generated at the heterointerface by spontaneous polarization and piezoelectric polarization, and even without any doping, 1×10 13 cm -2 Therefore, when the GaN epitaxial substrate of the present embodiment in the second aspect is used for HEMT, it is necessary to include a nitride semiconductor barrier layer.
[0247] The thickness of the nitride semiconductor barrier layer in the c-axis direction is preferably 1 to 50 nm, more preferably 5 to 40 nm, and further preferably 10 to 30 nm. Here, from the perspective of normal device production, the thickness of the nitride semiconductor barrier layer is preferably 1 nm or more, more preferably 5 nm or more, and further preferably 10 nm or more. In addition, from the perspective of reducing leakage current, the thickness of the nitride semiconductor barrier layer is preferably 50 nm or less, more preferably 40 nm or less, and further preferably 30 nm or less.
[0248] GaN cap layer
[0249] In the case where the GaN epitaxial substrate of the present embodiment in the second mode has a nitride semiconductor barrier layer, a GaN cap layer may be provided on the nitride semiconductor barrier layer as needed. The thickness of the GaN cap layer in the c-axis direction is preferably 0.1 to 10 nm, more preferably 0.5 to 8 nm, and further preferably 0.5 to 5 nm. Here, from the perspective of normal device fabrication, the thickness of the GaN cap layer is preferably greater than 0.1 nm, more preferably greater than 0.5 nm, and further preferably greater than 1 nm. In addition, from the perspective of reducing leakage current, the thickness of the GaN cap layer is preferably less than 10 nm, more preferably less than 8 nm, and further preferably less than 5 nm.
[0250] The GaN epitaxial substrate of the present embodiment in the second aspect can be preferably used for the production of a nitride semiconductor device, particularly a nitride semiconductor device having a horizontal device structure.
[0251] In the case of nitride semiconductor devices, one or more nitride semiconductor layers can be epitaxially grown on the above-mentioned GaN epitaxial substrate as needed. Nitride semiconductors are also called nitride III-V compound semiconductors, III-nitride compound semiconductors, GaN semiconductors, etc., and in addition to GaN, they also include compounds formed by replacing part or all of the gallium of GaN with other elements of Group 13 of the periodic table (B, Al, In, etc.).
[0252] Then, electrodes may be provided on the GaN epitaxial substrate according to the type of nitride semiconductor device to be manufactured.
[0253] A typical example of a nitride semiconductor device with a horizontal device structure is GaN-HEMT (High Electron Mobility Transistor).
[0254] [Method for manufacturing GaN epitaxial substrate]
[0255] The manufacturing method of the GaN epitaxial substrate of the present embodiment in the second embodiment is not particularly limited, and an embodiment thereof will be described below as an example. In addition, the preferred embodiment of the GaN epitaxial substrate obtained by the above manufacturing method is the same as the preferred embodiment described in the above [GaN epitaxial substrate].
[0256] The method for manufacturing a GaN epitaxial substrate according to the above-mentioned one embodiment as a second aspect includes at least a step of preparing a GaN substrate and then a step of epitaxially growing a GaN buffer layer on the GaN substrate.
[0257] The GaN substrate used in the GaN epitaxial substrate of the present embodiment in the second embodiment may be a GaN substrate having an Fe-doped layer doped with Fe, or a GaN substrate without an Fe-doped layer, as described in the [GaN epitaxial substrate] in the second embodiment. When a GaN substrate without an Fe-doped layer is used, it is necessary to dope Fe in the GaN buffer layer in order to achieve semi-insulation using Fe, as described later.
[0258] The GaN substrate can be manufactured by a known method or a commercial product can be used. When manufacturing a GaN substrate, the step of preparing the GaN substrate becomes a step of manufacturing the GaN substrate, preferably a step of manufacturing a GaN substrate doped with Fe.
[0259] The Fe-doped GaN substrate can be obtained, for example, by growing an Fe-doped GaN crystal on a seed crystal by the HVPE method and performing processing such as slicing, grinding, and polishing.
[0260] ·GaN buffer layer formation method
[0261] The method for epitaxially growing the GaN buffer layer on the GaN substrate is not particularly limited, and various known methods can be used. Preferred examples include MOCVD and Molecular Beam Epitaxy (MBE).
[0262] When the MOCVD method is used, the raw material gas is not particularly limited as long as it contains a Ga source and an N source for forming GaN, and a known gas can be used.
[0263] In the case where the GaN substrate is a GaN substrate doped with Fe as described above, it is not necessary to dope the epitaxially grown GaN buffer layer with Fe. However, in the case of a GaN substrate that does not include an Fe-doped layer doped with Fe, a region doped with Fe is formed in the GaN epitaxial substrate by doping the epitaxially grown GaN buffer layer with Fe. In this case, it is considered that it is preferable for the manufacturing method of the GaN epitaxial substrate to include a step of doping with Fe in a part of the step of epitaxially growing the GaN buffer layer. In addition, it is preferable that the step of doping with Fe is performed before the step of forming the C-containing region described later.
[0264] In order to make the Fe concentration in the GaN epitaxial substrate of the present embodiment in the second embodiment satisfy the preferred characteristics of the first embodiment and the second embodiment in the second embodiment, it is preferred to perform the step of doping C in the epitaxially grown GaN buffer layer in a manner that includes a C-containing layer and a Fe diffusion suppression layer containing C. It should be noted that the preferred characteristics of the first embodiment and the second embodiment in the second embodiment refer to that the Fe concentration of the Fe doped layer is 1×10 17 atoms / cm 3 As described above, the Fe concentration of the GaN region present in the C-containing layer or the GaN region present in the
[0001] axis direction relative to the C-containing layer is 1×10 16 atoms / cm 3 the following.
[0265] C is preferably doped in a region existing in the
[0001] axis direction relative to the Fe-doped region. Therefore, when the GaN substrate includes a region doped with Fe, the C-containing layer or the Fe diffusion suppression layer must exist in the
[0001] axis direction relative to the Fe-doped region. On the other hand, when the GaN buffer layer formed by epitaxial growth includes a region doped with Fe, C is preferably doped after Fe doping.
[0266] In the first embodiment and the second embodiment of the second aspect, C is preferably doped so that the C-containing layer or the Fe diffusion suppression layer includes point B or point B'. In addition, C is also preferably doped on the (000-1) plane side with respect to the plane parallel to the (0001) plane and including point B or the plane parallel to the (0001) plane and including point B'. In the latter, C is doped between the plane parallel to the (0001) plane and including point A or point A' and the plane parallel to the (0001) plane and including point B or point B'.
[0267] When C is doped in the epitaxially grown GaN buffer layer, the thickness of the C-containing layer or the Fe diffusion suppression layer in the c-axis direction (height in the thickness direction) is preferably 50 to 900 nm as described in the [GaN epitaxial substrate] in the second embodiment. Here, from the perspective of normal device production, the above thickness is preferably 50 nm or more, and from the perspective of reducing leakage current, it is preferably 900 nm or less.
[0268] The concentration of C in the C-containing layer or the Fe diffusion suppression layer is 1×10 16 atoms / cm 3 The above concentration can be 5×10 16 atoms / cm 3 Above, 1×10 17 atoms / cm 3 Above and more.
[0269] In order to avoid a significant decrease in crystal quality due to excessive doping, the C concentration in the GaN buffer layer including the C-containing layer or the Fe diffusion suppression layer is preferably 1×10 18 atoms / cm 3 Below, or less than 1×10 18 atoms / cm 3 , is 8×10 17 atoms / cm 3 Below, 5×10 17 atoms / cm 3 The following etc.
[0270] C can be doped by a conventionally known method, for example, preferably by MOCVD or MBE.
[0271] In the case of using the MOCVD method, as the raw material gas, for example, a hydrocarbon gas such as CH4 (methane) can be used. From the perspective of simplification, it is preferred to use a raw material gas that also contains a Ga source and an N source for forming GaN. From the above perspective, as the raw material gas of C, trimethylgallium (TMG) and triethylgallium (TEG) are preferably used, and TMG is more preferred. In addition, it is further preferred to use a mixed gas of TMG and ammonia (NH3) or a mixed gas of TEG and NH3.
[0272] When a mixed gas of trimethylgallium (TMG) and ammonia (NH3) is used, the supply rate of TMG is preferably 100 to 500 μmol / min, more preferably 200 to 300 μmol / min. Here, from the viewpoint of reducing the concentration of impurities such as Si, the supply rate of TMG is preferably 100 μmol / min or more, more preferably 200 μmol / min or more. In addition, from the viewpoint of film thickness controllability, the supply rate of TMG is preferably 500 μmol / min or less, more preferably 300 μmol / min or less.
[0273] From the viewpoint of controllability of C concentration, the supply rate ratio represented by TMG:NH3 is preferably 1:100 to 1:4000, more preferably 1:500 to 1:4000 or 1:100 to 1:2000, and further preferably 1:500 to 1:2000.
[0274] In the case where C is doped to form a C-containing region and Fe is also doped in the epitaxially grown GaN buffer layer, it is preferred that Fe doping and C doping are performed discontinuously from the viewpoint of reducing the memory effect during epitaxial growth. In other words, it is preferred to avoid performing C doping continuously after Fe doping. "Performed continuously" means, for example, that the Fe doping operation and the C doping operation are not purged between the two operations, or that an interval of more than several hours is not separated, and that the C doping operation is performed after the Fe doping operation using the same growth apparatus.
[0275] It should be noted that, when C is doped to form a C-containing region and a substrate having a region doped with Fe is used as a GaN substrate, it is natural that Fe doping and C doping are performed discontinuously in the entire manufacturing process.
[0276] As described above, as an epitaxial GaN buffer layer, an i-GaN layer can be formed after forming an Fe-doped region and a C-containing region doped with Fe as needed. When the GaN epitaxial substrate of this embodiment in the second mode is used for HEMT, the i-GaN layer functions as a so-called channel layer, so it is necessary to form an i-GaN layer. The method of forming the i-GaN layer is no different from the method of epitaxially growing the GaN buffer layer, except that it is not accompanied by intentional impurity doping. As preferred examples, MOCVD method and MBE method can be cited.
[0277] When the i-GaN layer is formed by MOCVD, a hydrocarbon gas such as CH4 (methane) can be used as a raw material gas. From the perspective of simplification, it is preferable to use a raw material gas that also contains a Ga source and an N source for forming GaN.
[0278] When a mixed gas of trimethylgallium (TMG) and ammonia (NH3) is used, the supply rate of TMG is preferably 50 to 250 μmol / min, more preferably 100 to 150 μmol / min. Here, from the viewpoint of reducing the concentration of impurities such as Si, the supply rate of TMG is preferably 50 μmol / min or more, more preferably 100 μmol / min or more. In addition, from the viewpoint of film thickness controllability, the supply rate of TMG is preferably 250 μmol / min or less, more preferably 150 μmol / min or less.
[0279] From the viewpoint of reducing the C concentration, the supply rate ratio represented by TMG:NH3 is preferably 1:400 to 1:16000, more preferably 1:400 to 1:1800 or 1:2000 to 1:16000, and further preferably 1:2000 to 1:8000.
[0280] The thickness of the i-GaN layer in the GaN buffer layer in the c-axis direction is the same as that described in the present embodiment of the [GaN epitaxial substrate] in the second embodiment, and is preferably 50 to 900 nm. Here, from the perspective of normal device production, the thickness is preferably 50 nm or more, and from the perspective of reducing leakage current, it is preferably 900 nm or less.
[0281] ·Method for forming nitride semiconductor barrier layer
[0282] After forming the above-mentioned epitaxial GaN buffer layer, a nitride semiconductor barrier layer may be formed. When the GaN epitaxial substrate of the present embodiment in the second mode is used for HEMT, a nitride semiconductor barrier layer needs to be formed in order to generate 2DEG. Preferred examples of the barrier layer include Al x Ga 1-x The N (0<x<1) layer may be an AlInGaN layer. 2DEG is generated in a region sandwiched by the GaN buffer layer and the nitride semiconductor barrier layer.
[0283] The method for forming the nitride semiconductor barrier layer is not particularly limited, and a conventionally known method can be used. Preferred examples include MOCVD and MBE.
[0284] The preferred thickness of the nitride semiconductor barrier layer on the GaN buffer layer in the c-axis direction is the same as that described in this embodiment of the [GaN epitaxial substrate] in the above-mentioned second aspect.
[0285] When the above-mentioned nitride semiconductor barrier layer is formed, a conventionally known layer such as a GaN cap layer may be formed by a conventionally known method as needed.
[0286] Example
[0287] Hereinafter, the present invention will be specifically described with reference to Examples, but the present invention is not limited thereto.
[0288] [Example 1]
[0289] The GaN buffer layer was deposited on the C-face GaN substrate with Fe doping layer obtained by HVPE by MOCVD to obtain a GaN epitaxial substrate with HEMT structure. The thickness of the C-face GaN substrate in the c-axis direction is 400 μm, of which the Fe doping layer is about 100 μm thick on the Ga polar surface side. The Fe concentration of the Fe doping layer is 2.2×10 18 atoms / cm 3 .
[0290] To form the GaN buffer layer, specifically, a C-face GaN substrate was placed in an MOCVD device, heated to 1090°C in a hydrogen / nitrogen mixed gas atmosphere and at atmospheric pressure, and trimethylgallium (TMG) and NH3 gas were supplied. The gas supply rate was set to 410 μmol / min for TMG and 5 slm for NH3 gas. Under the above conditions, the crystal was grown for 2.7 minutes, thereby forming a GaN buffer layer with a C concentration of 1×10 17 atoms / cm 3 The thickness of the C-containing region was 300 nm. The total time for heating to 1090° C. was 17 minutes.
[0291] Next, on the obtained C-containing region, the supply rate and growth time of TMG and NH3 gas, i.e., the gas supply amount, was changed to grow an i-GaN layer with a thickness of 200 nm. Furthermore, an Al layer with a thickness of 18 nm was grown thereon. x Ga 1-x The N (0<x<1) layer and the GaN cap layer with a thickness of 2 nm serve as nitride semiconductor barrier layers.
[0292] Through the above operation, a GaN epitaxial substrate of a HEMT structure is obtained. With respect to the first embodiment, the obtained GaN epitaxial substrate has a C-containing layer in the GaN buffer layer. In addition, with respect to the second embodiment, a Fe diffusion suppression layer containing C is present in the GaN buffer layer. In addition, the C-containing layer or the Fe diffusion suppression layer is present in the GaN buffer layer in the
[0001] axis direction relative to the Fe-doped layer.
[0293] [Evaluation of GaN epitaxial substrate]
[0294] The GaN epitaxial substrate obtained in Example 1 was subjected to SIMS measurement. Figure 1The solid line shows the Fe concentration curve at the interface between the Fe-doped layer with high Fe concentration and the C-containing region in the GaN epitaxial substrate. Figure 3 It is expressed in logarithm Figure 1 The vertical axis is the Fe concentration curve, and Figure 1 Likewise, the results of Example 1 are shown by a solid line.
[0295] As a result, for the first and second embodiments, the Fe concentration in the GaN epitaxial substrate is 2.2×10 18 atoms / cm 3 The Fe-doped layer has an Fe concentration of 1 / 100, that is, 2.2×10 16 atoms / cm 3 The distance between the Fe doped layer and the Fe doped layer is 0.122 μm. In addition, the Fe concentration is 1 / 10, that is, 2.2×10 17 atoms / cm 3 The distance between the Fe and Fe is 0.045 μm. In addition, both the measurement point where the Fe concentration becomes 1 / 100 and the measurement point where the Fe concentration becomes 1 / 10 are located in the C-containing region.
[0296] In addition, in the second embodiment, the GaN substrate includes an Fe-doped layer, the GaN buffer layer includes a C-containing layer, and the concentration of the Fe-doped layer is 2.2×10 18 atoms / cm 3 , the C concentration of the C-containing layer is 1×10 17 atoms / cm 3 In addition, the Fe concentration in the C-containing layer and in the region in the
[0001] axis direction relative to the C-containing layer, i.e., the GaN region, is less than 1×10 17 atoms / cm 3 .
[0297] [Comparative Example 1]
[0298] The Fe concentration of the Fe-doped layer was 1.2×10 18 atoms / cm 3 A GaN epitaxial substrate was obtained by growing a GaN buffer layer without a C-containing region on a C-plane GaN substrate having an Fe-doped layer which was the same as the C-plane GaN substrate of Example 1 except for this point by the HVPE method.
[0299] Specifically, while maintaining the reactor temperature at 1090°C, ammonia and gallium chloride are supplied, thereby growing an undoped GaN buffer layer on a C-face GaN substrate to a thickness of 5.5 μm. The growth rate is set to 50 μm / hr. The growth conditions are set to a reactor pressure of 101 kPa, an ammonia partial pressure of 3.172 kPa, a GaCl partial pressure of 0.847 kPa, a hydrogen partial pressure of 43.4 kPa, and a nitrogen partial pressure of 55.581 kPa. Then, the supply of gallium chloride is stopped while maintaining the same temperature. At the moment when the total growth and holding time reaches 60 minutes, the heating of the reactor is stopped and the reactor temperature is lowered to room temperature.
[0300] Through the above operations, a GaN epitaxial substrate was obtained.
[0301] The obtained GaN epitaxial substrate was subjected to SIMS measurement. Figure 2 The solid line of represents the result. Based on the result, the diffusion constant of Fe in the GaN crystal without the C-containing region at 1090°C was obtained.
[0302] It should be noted that the reason why the growth method used to determine the diffusion constant uses the HVPE method instead of the MOCVD method is as follows. As shown in Example 1, the MOCVD method preferably uses TMG in the III group raw material. Due to the alkyl group in the TMG, unexpected carbon is introduced into the GaN crystal. As will be described later Figure 1 and Figure 3 As described above, this carbon inhibits the diffusion of Fe, so the diffusion constant of Fe in GaN crystal cannot be accurately estimated. On the other hand, the HVPE method contains a Group III raw material and does not use a raw material containing a carbon source, so the diffusion constant of Fe in a pure GaN crystal can be estimated.
[0303] When determining the diffusion constant of Fe, the SIMS measurement results of Comparative Example 1 were fitted using the diffusion equation. The diffusion time was 60 minutes. Thus, the diffusion constant of Fe in the GaN crystal at 1090°C was determined to be 0.00005 μm 2 / min. It should be noted that the fitting results of the above diffusion equation are as follows Figure 2 As shown by the dotted line.
[0304] Using this value of the diffusion constant, the C concentration is 1×10 17 atoms / cm 3 A GaN epitaxial substrate with a HEMT structure was obtained by MOCVD in the same manner as the GaN epitaxial substrate of Example 1 except for the C-containing region. This case was taken as Comparative Example 2, and the Fe concentration curve of Comparative Example 2 was calculated by the diffusion equation. The diffusion time used was 17 minutes, which was the same as the time required for MOCVD growth in Example 1. Figure 1 and Figure 3 The dashed line shows the result.
[0305] The results show that Fe diffused significantly in Comparative Example 2 compared to Example 1. That is, it can be seen that the C-containing region in the GaN buffer layer inhibits the diffusion of Fe. Figure 1 and Figure 3 In the GaN epitaxial substrate of Comparative Example 2, it is assumed that there is an Fe concentration of 2.2×10 18 atoms / cm 3 In the case of an Fe-doped layer, the Fe concentration becomes 1 / 100, that is, 2.2×10 16 atoms / cm 3 The distance between the two is 0.24 μm. In addition, the Fe concentration is reduced to 1 / 10, that is, to 2.2×10 17 atoms / cm 3 The distance is 0.18μm.
[0306] The present invention is described in detail with reference to specific embodiments, but it is clear to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on Japanese patent applications (Japanese patent application 2022-039628) filed on March 14, 2022 and Japanese patent applications (Japanese patent application 2022-039629) filed on March 14, 2022, and their contents are incorporated herein by reference.
Claims
1. A GaN epitaxial substrate comprising a GaN substrate and a GaN buffer layer epitaxially grown on the GaN substrate, The GaN epitaxial substrate includes a point A and a point B, wherein the point B is located on a straight line passing through the point A and parallel to the [0001] axis, and exists in the [0001] axis direction relative to the point A. The point A exists in the GaN substrate or in the GaN buffer layer, The point B exists in the GaN buffer layer, The Fe concentration at point B [Fe] B and the Fe concentration at point A [Fe] A The ratio ([Fe] B / [Fe] A ) is 1 / 100, and the distance between the point A and the point B is less than 0.2 μm.
2. A GaN epitaxial substrate comprising a GaN substrate and a GaN buffer layer epitaxially grown on the GaN substrate, The GaN epitaxial substrate includes a point A' and a point B', wherein the point B' is located on a straight line passing through the point A' and parallel to the [0001] axis, and exists in the [0001] axis direction relative to the point A'. The point A' exists in the GaN substrate or in the GaN buffer layer, The point B' exists in the GaN buffer layer, The Fe concentration at point B' [Fe] B’ and the Fe concentration at point A' [Fe] A’ The ratio ([Fe] B’ / [Fe] A’ ) is 1 / 10, and the distance between the point A' and the point B' is less than 0.1 μm.
3. A GaN epitaxial substrate comprising a GaN substrate and a GaN buffer layer epitaxially grown on the GaN substrate, The GaN epitaxial substrate includes a point A″ and a point B″, wherein the point B″ is located on a straight line passing through the point A″ and parallel to the [0001] axis, and exists in the [0001] axis direction relative to the point A″. The point A" exists in the GaN substrate or in the GaN buffer layer, The point B" exists in the GaN buffer layer, The Fe concentration at point A" is 1×10 17 atoms / cm 3 The Fe concentration at point B" is 1×10 15atoms / cm 3 Hereinafter, the distance between the point A" and the point B" is less than 0.2 μm.
4. A GaN epitaxial substrate comprising a GaN substrate and a GaN buffer layer epitaxially grown on the GaN substrate, The GaN epitaxial substrate includes a point A'' and a point B''', wherein the point B''' is located on a straight line passing through the point A''' and parallel to the [0001] axis, and exists in the [0001] axis direction relative to the point A'''. The point A'' exists in the GaN substrate or in the GaN buffer layer, The point B'' exists in the GaN buffer layer, The Fe concentration at point A'' is 1×10 17 atoms / cm 3 The Fe concentration at point B'' is 1×10 16 atoms / cm 3 Hereinafter, the distance between the point A''' and the point B'''' is less than 0.1 μm.
5. The GaN epitaxial substrate according to claim 1 or 2, wherein: The [Fe] A or the [Fe] A’ 1×10 17 atoms / cm 3 above.
6. The GaN epitaxial substrate according to any one of claims 1 to 5, wherein The point A, the point A′, the point A″ or the point A′″ exists in the GaN substrate.
7. The GaN epitaxial substrate according to any one of claims 1 to 6, wherein The GaN buffer layer contains a C concentration of 1×10 16 ~1×10 18 atoms / cm 3 The C-containing region, The C-containing region includes point B, point B', point B", or point B'", or is located on the (000-1) plane side with respect to a plane parallel to the (0001) plane and including point B, point B', point B", or point B''".
8. The GaN epitaxial substrate according to any one of claims 1 to 7, wherein At least one of the GaN substrate and the GaN buffer layer includes an Fe-doped layer doped with Fe.
9. The GaN epitaxial substrate according to any one of claims 1 to 8, wherein The GaN substrate comprises an Fe-doped layer doped with Fe, The point A, the point A′, the point A″ or the point A′″ exists in the Fe-doped layer.
10. The GaN epitaxial substrate according to any one of claims 7 to 9, wherein The GaN buffer layer includes an i-GaN layer in the [0001] axis direction relative to the C-containing region.
11. The GaN epitaxial substrate according to any one of claims 1 to 10, wherein A nitride semiconductor barrier layer is further provided on the GaN buffer layer.
12. A GaN epitaxial substrate comprising a GaN substrate and a GaN buffer layer epitaxially grown on the GaN substrate, At least one of the GaN substrate and the GaN buffer layer includes an Fe-doped layer doped with Fe, The GaN buffer layer comprises a C-containing layer, The C-containing layer is present in the [0001] axis direction relative to the Fe-doped layer, and the C concentration is 1×10 16 ~1×10 18 atoms / cm 3 .
13. A GaN epitaxial substrate, comprising a GaN substrate and a GaN buffer layer epitaxially grown on the GaN substrate, The GaN substrate or the GaN buffer layer includes an Fe-doped layer doped with Fe, The GaN buffer layer includes an Fe diffusion suppression layer that exists in the [0001] axis direction relative to the Fe doped layer and contains C to suppress diffusion of Fe.
14. The GaN epitaxial substrate according to claim 13, wherein: The C concentration of the Fe diffusion suppression layer is 1×10 18 atoms / cm 3 the following.
15. The GaN epitaxial substrate according to any one of claims 12 to 14, wherein The GaN substrate includes the Fe-doped layer.
16. The GaN epitaxial substrate according to any one of claims 12 to 15, wherein The Fe concentration of the Fe doped layer is 1×10 17 atoms / cm 3 above.
17. The GaN epitaxial substrate according to any one of claims 12 to 16, wherein: The C-containing layer or the Fe diffusion suppression layer is a layer doped with C.
18. The GaN epitaxial substrate according to any one of claims 12 to 17, wherein In the GaN buffer layer, the Fe concentration in the C-containing layer or the Fe diffusion suppression layer, or in the GaN region located in the [0001] axis direction relative to the C-containing layer or the Fe diffusion suppression layer is less than 1×10 17 atoms / cm 3 .
19. The GaN epitaxial substrate according to any one of claims 12 to 18, wherein The GaN substrate or the GaN buffer layer includes a point A, The GaN buffer layer includes a point B, which is located on a straight line passing through the point A and parallel to the [0001] axis, and exists in the [0001] axis direction relative to the point A. The Fe concentration at point B [Fe] B and the Fe concentration at point A [Fe] A The ratio ([Fe] B / [Fe] A ) is 1 / 100, and the distance between the point A and the point B is less than 0.2 μm.
20. The GaN epitaxial substrate according to any one of claims 12, 15 to 19, wherein: The GaN buffer layer includes an i-GaN layer in the [0001] axis direction relative to the C-containing layer.
21. The GaN epitaxial substrate according to any one of claims 12 to 20, wherein: A nitride semiconductor barrier layer is further provided on the GaN buffer layer.